Separator, battery and battery preparation method
By employing a composite structure of a first coating of oily binder and ceramic particles and a second coating of water-based binder and ceramic particles on the lithium-ion battery separator, the problems of insufficient separator adhesion and thermal shrinkage are solved, thereby improving battery safety and electrolyte flowability.
Patent Information
- Application Number
- CN202310505698.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-05-06
AI Technical Summary
The existing lithium-ion battery separator has insufficient adhesion, which makes it prone to shrinkage when heated, causing safety hazards.
The composite structure employs a first coating comprising an oil-based binder and ceramic particles and a second coating comprising a water-based binder layer and a ceramic layer. The first coating is in contact with the electrode, and the thickness of the second coating is greater than or equal to twice the thickness of the first coating, thereby enhancing adhesion and reducing thermal shrinkage.
It improves the adhesion of the separator, reduces the probability of safety accidents caused by insufficient adhesion between the separator and the electrode or separator shrinkage when heated, and enhances the storage and flow capacity of the electrolyte.
Smart Images

Figure CN116780109B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a separator, a battery, and a method for preparing the battery. Background Technology
[0002] Lithium-ion batteries are widely used in digital products and power supplies due to their high energy density and fast charging technology. With the continuous upgrading of technology, there are higher challenges to the performance and safety of lithium-ion batteries. Improving the charging window of lithium-ion batteries and improving lithium plating during the cycle process are necessary to enhance safety performance.
[0003] As a key component of lithium-ion batteries, the separator's main function is to separate the positive and negative electrodes, preventing contact between them and thus avoiding internal short circuits. It also allows electrolyte ions to pass through. In some related technologies, the separator has weak adhesion, resulting in insufficient bonding between the separator and the electrodes, which can lead to safety hazards. Some separators are also prone to shrinkage when heated, and this shrinkage can easily cause safety accidents. Summary of the Invention
[0004] This application aims to at least solve one of the technical problems existing in the prior art. To this end, this application proposes a separator, a battery, and a method for preparing the battery, which enables the separator to have strong adhesion and is not easily shrunk when heated.
[0005] The diaphragm according to a first aspect embodiment of this application includes:
[0006] Base film;
[0007] A first coating comprising an oily binder and first ceramic particles, wherein the oily binder is mixed with the first ceramic particles, and the first coating is applied to a first surface of the base film;
[0008] The second coating comprises an aqueous adhesive layer and a ceramic layer, wherein the aqueous adhesive layer is coated on the ceramic layer, the second coating is coated on the second surface of the base film, and the ceramic layer is located between the aqueous adhesive layer and the second surface, the second surface being opposite to the first surface;
[0009] The thickness of the second coating is greater than or equal to twice the thickness of the first coating.
[0010] The separator according to the embodiments of this application has at least the following beneficial effects: When the separator of the embodiments of this application is applied to a battery, the first coating contacts the battery electrode. Since the first coating includes an oily binder and first ceramic particles, and the oily binder and the first ceramic particles are mixed, the first coating has good adhesion characteristics and can form a good adhesion force with the electrode, so that the battery has good hardness and flatness. The second coating includes an aqueous binder layer and a ceramic layer. The second coating is coated on the second surface of the base film, and the aqueous binder layer is coated on the ceramic layer, with the ceramic layer located between the aqueous binder layer and the second surface. Therefore, the second coating has a small shrinkage rate when heated, which can reduce the shrinkage of the separator when heated. Therefore, the separator in this embodiment has strong adhesion and is not easily shrinkable when heated, thereby improving battery safety and reducing the probability of safety accidents caused by insufficient adhesion between the separator and the electrode or by separator shrinkage when heated; and since the thickness of the second coating is greater than or equal to twice the thickness of the first coating, when the separator is applied to the cell, a larger gap can be formed at the corner of the cell, so as to store more electrolyte and facilitate the flow of electrolyte.
[0011] According to some embodiments of this application, the diameter of the first ceramic particle is 0.5 micrometers to 1.5 micrometers.
[0012] According to some embodiments of this application, the ceramic layer includes second ceramic particles with a diameter of 1 micrometer to 3 micrometers.
[0013] According to some embodiments of this application, the water-based adhesive layer includes any one or a mixture of several of the following: styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl methacrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate, and polyurethane.
[0014] According to some embodiments of this application, the oily adhesive includes any one or a mixture of several of vinylidene fluoride homopolymer powder, vinylidene fluoride and hexafluoropropylene copolymer.
[0015] A second aspect of this application provides a battery including a separator as described in any one of the first aspects of the embodiment. The battery further includes a positive electrode and a negative electrode, and the separator is disposed between the positive electrode and the negative electrode.
[0016] A third aspect of this application provides a method for preparing a battery, comprising:
[0017] The positive electrode slurry is coated onto the positive electrode current collector, and the positive electrode current collector is cold-pressed and then slit to obtain the positive electrode sheet;
[0018] The negative electrode slurry is coated onto the negative electrode current collector, and the negative electrode current collector is cold-pressed and then slit to obtain the negative electrode sheet;
[0019] An oily binder is mixed with first ceramic particles to form a first coating. The first coating is applied to a first surface of a base film, a ceramic layer is applied to a second surface of the base film, and an aqueous binder layer is applied to the ceramic layer to obtain a separator. The second surface is opposite to the first surface, and the aqueous binder layer and the ceramic layer form a second coating. The thickness of the second coating is greater than or equal to twice the thickness of the first coating.
[0020] The positive electrode, the negative electrode, and the separator are used to form a bare battery cell;
[0021] Ethylene carbonate, propylene carbonate, diethyl carbonate, and propyl propionate are mixed to obtain a first solvent. Lithium salt is dissolved in the first solvent to obtain an electrolyte.
[0022] The battery is obtained by encapsulating the bare cell with the electrolyte.
[0023] According to some embodiments of the third aspect of this application, the positive electrode slurry is prepared in the following manner:
[0024] The positive electrode active material, conductive agent, conductive carbon nanotubes, and first binder are mixed in a second solvent to obtain the positive electrode slurry; wherein the weight percentage of the positive electrode active material is 96% to 98%, the weight percentage of the conductive agent is 0% to 1%, the weight percentage of the conductive carbon nanotubes is 0% to 1%, and the weight percentage of the first binder is 0.6% to 1.5%.
[0025] According to some embodiments of the third aspect of this application, the negative electrode slurry is prepared in the following manner:
[0026] The negative electrode active material, dispersant, and second binder are mixed to obtain the negative electrode slurry; wherein the weight percentage of the negative electrode active material is 96.5% to 98.5%, the weight percentage of the dispersant is 0% to 1%, and the weight percentage of the second binder is 0.7% to 1.5%.
[0027] According to some embodiments of the third aspect of this application, the volume percentage of ethylene carbonate is 5% to 20%, the volume percentage of propylene carbonate is 5% to 20%, the volume percentage of diethyl carbonate is 30% to 60%, and the volume percentage of propyl propionate is 30% to 60%.
[0028] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0029] The present application will be further described below with reference to the accompanying drawings and embodiments, wherein:
[0030] Figure 1 This is a schematic diagram of the diaphragm structure according to an embodiment of this application;
[0031] Figure 2 This is a flowchart illustrating the steps of a battery preparation method according to an embodiment of this application.
[0032] Figure label:
[0033] Base film 100; first ceramic particles 110; oil-based binder 120; water-based binder layer 130; ceramic layer 140. Detailed Implementation
[0034] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.
[0035] In the description of this application, it should be understood that the orientation descriptions, such as up, down, front, back, left, right, etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0036] In the description of this application, "several" means one or more, "multiple" means two or more, "greater than," "less than," and "exceeding" are understood to exclude the stated number, while "above," "below," and "within" are understood to include the stated number. The use of "first" and "second" in the description is merely for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.
[0037] In the description of this application, unless otherwise expressly defined, terms such as "setup," "installation," and "connection" should be interpreted broadly, and those skilled in the art can reasonably determine the specific meaning of the above terms in this application in conjunction with the specific content of the technical solution.
[0038] In the description of this application, the terms "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0039] Reference Figure 1 The first aspect of this application provides a diaphragm, comprising:
[0040] Base film 100;
[0041] A first coating comprising an oily binder 120 and first ceramic particles 110, wherein the oily binder 120 is mixed with the first ceramic particles 110, and the first coating is applied to the first surface of the base film 100.
[0042] The second coating comprises an aqueous adhesive layer 130 and a ceramic layer 140, wherein the aqueous adhesive layer 130 is coated on the ceramic layer 140, and the second coating is coated on the second surface of the base film 100, wherein the ceramic layer 140 is located between the aqueous adhesive layer 130 and the second surface, and the second surface is opposite to the first surface.
[0043] The thickness of the second coating is greater than or equal to twice the thickness of the first coating.
[0044] The separator according to the embodiments of this application has at least the following beneficial effects: When the separator of the embodiments of this application is applied to a battery, the first coating contacts the battery electrode. Since the first coating includes an oily binder 120 and first ceramic particles 110, and the oily binder 120 and the first ceramic particles 110 are mixed, the first coating has good adhesion characteristics and can form a good adhesion force with the electrode, so that the battery has good hardness and flatness. The second coating includes an aqueous binder layer 130 and a ceramic layer 140. The second coating is coated on the second surface of the base film 100, and the aqueous binder layer 130 is coated on the ceramic layer 140, and the ceramic layer 140 is located between the aqueous binder layer 130 and the second surface. Therefore, the second coating has a small shrinkage rate when heated, which can reduce the shrinkage of the separator when heated. Therefore, the separator in this embodiment has strong adhesion and is not easily shrinkable when heated, thereby improving battery safety and reducing the probability of safety accidents caused by insufficient adhesion between the separator and the electrode or by separator shrinkage when heated; and since the thickness of the second coating is greater than or equal to twice the thickness of the first coating, when the separator is applied to the cell, a larger gap can be formed at the corner of the cell, so as to store more electrolyte and facilitate the flow of electrolyte.
[0045] Understandably, in one embodiment, the separator is disposed between the positive and negative electrodes of the battery. The first coating can contact the positive electrode, while the second coating contacts the negative electrode. Due to the strong adhesion of the first coating, a good bond is formed between the first coating and the positive electrode, giving the battery better hardness and flatness. This avoids safety hazards caused by low hardness or insufficient flatness. Furthermore, the second coating has a smaller shrinkage rate when heated, reducing the shrinkage of the separator during heating and lowering the probability of safety accidents caused by separator shrinkage during heating.
[0046] In another embodiment, the separator is disposed between the positive and negative electrodes of the battery. The first coating can contact the negative electrode, while the second coating contacts the positive electrode. Because the first coating has strong adhesion, it forms a good bond with the negative electrode, giving the battery better hardness and flatness. This avoids safety hazards caused by low hardness or insufficient flatness. Furthermore, the second coating has a smaller shrinkage rate when heated, reducing the shrinkage of the separator and lowering the probability of safety accidents caused by separator shrinkage during heating.
[0047] It should be noted that the base film 100 is one of polyethylene base film 100, polypropylene base film 100, polypropylene composite base film 100, polyethylene composite base film 100, polypropylene composite base film 100, polyimide base film 100, polyvinylidene fluoride film 100, polyethylene nonwoven base film 100, polypropylene nonwoven base film 100, and polyimide nonwoven base film 100. Those skilled in the art can select the base film 100 according to actual needs, and this application does not limit it in this regard.
[0048] Understandably, the thickness of the base film 100 is 3 to 10 micrometers, for example, the thickness of the base film 100 is 3 micrometers, 5 micrometers, or 10 micrometers. The porosity of the base film 100 is 20% to 50%, for example, the porosity of the base film 100 is 20%, 35%, or 50%.
[0049] It is understandable that the first ceramic particle 110 can be one or more of alumina, zirconium oxide, and zinc oxide. The second ceramic particle can be one or more of alumina, zirconium oxide, and zinc oxide.
[0050] It is understood that the diameter of the first ceramic particle 110 is between 0.5 micrometers and 1.5 micrometers. For example, the diameter of the first ceramic particle 110 can be 0.5 micrometers, 1 micrometer, or 1.5 micrometers.
[0051] It is worth noting that the diameter of the first ceramic particles 110 in the first coating is 0.5 micrometers to 1.5 micrometers. The small diameter of the first ceramic particles 110 can reduce the thickness of the separator and enhance the adhesion between the first coating and the active material of the electrode, so that the battery has better hardness and flatness, thereby avoiding safety hazards caused by low hardness or insufficient flatness of the battery.
[0052] It is understood that the ceramic layer 140 includes second ceramic particles with a diameter of 1 micrometer to 3 micrometers, for example, the diameter of the second ceramic particles is 1 micrometer, 2 micrometers or 3 micrometers.
[0053] It is worth noting that the diameter of the second ceramic particles in the second coating is 1 to 3 micrometers. The larger size of the second ceramic particles results in a greater binding force on the side of the separator coated with the second coating, which can suppress separator shrinkage, reduce the shrinkage of the separator when heated, and reduce the probability of safety accidents caused by separator shrinkage when heated. In addition, the larger size of the second ceramic particles results in larger pores between the second coating of the separator and the active material of the electrode, so that the second coating can retain more electrolyte.
[0054] The thickness of the first coating is determined by the first ceramic particles, and the thickness of the second coating is determined by the second ceramic particles. Setting the diameter of the first ceramic particles to 0.5 to 1.5 micrometers and the diameter of the second ceramic particles to 1 to 3 micrometers ensures that the thickness of the second coating is greater than or equal to twice the thickness of the first coating. Specifically, compared to the first coating, the second ceramic particles in the second coating are larger, and the second coating uses a water-based binder. Therefore, the second coating can retain more electrolyte. The thickness of the second coating is d2, and the thickness of the first coating is d1, where d2 ≥ 2 * d1. When the separator is applied to the battery cell, it can form a larger gap at the cell corners, facilitating the storage of more electrolyte and its flow. The larger gap at the cell corners allows for the retention of more electrolyte, reducing the probability of lithium plating at the cell corners due to insufficient electrolyte, thus improving the situation and extending the battery cell's lifespan.
[0055] It is worth noting that there are multiple data for both the first ceramic particle 110 and the second ceramic particle, and this application does not make a specific limitation on the number of the first ceramic particle 110 and the second ceramic particle.
[0056] It is understood that the waterborne adhesive layer 130 includes any one or a mixture of several of the following: styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl methacrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate, and polyurethane.
[0057] It is understood that the oily adhesive 120 includes any one or a mixture of several of the following: vinylidene fluoride homopolymer powder, vinylidene fluoride and hexafluoropropylene copolymer.
[0058] It is understood that the second aspect of this application provides a battery, which is a secondary battery. The battery includes a separator as described in any one of the first aspect embodiments, and the battery also includes a positive electrode and a negative electrode, with the separator disposed between the positive electrode and the negative electrode.
[0059] Since the battery in the second aspect embodiment includes a separator as described in any of the embodiments in the first aspect of this application, the corresponding content of the separator in the embodiments mentioned in the first aspect is also applicable to the battery in the embodiments mentioned in the second aspect, and has the same implementation principle and technical effect. To avoid redundancy, it will not be described in detail here.
[0060] Reference Figure 2 The third aspect of this application provides a method for preparing a battery, including but not limited to the following steps:
[0061] Step S210: Coat the positive electrode slurry onto the positive electrode current collector, and then slit the positive electrode current collector after cold pressing to obtain the positive electrode sheet;
[0062] Step S220: The negative electrode slurry is coated onto the negative electrode current collector, and the negative electrode current collector is cold-pressed and then slit to obtain the negative electrode sheet;
[0063] In step S230, the oily binder 120 is mixed with the first ceramic particles 110 to form a first coating. The first coating is applied to the first surface of the base film 100, the ceramic layer 140 is applied to the second surface of the base film 100, and the watery binder layer 130 is applied to the ceramic layer 140 to obtain a separator. The second surface is opposite to the first surface, and the watery binder layer and the ceramic layer form a second coating. The thickness of the second coating is greater than or equal to twice the thickness of the first coating.
[0064] Step S240: The positive electrode, negative electrode and separator are made into a bare cell;
[0065] In step S250, ethylene carbonate, propylene carbonate, diethyl carbonate, and propyl propionate are mixed to obtain a first solvent, and lithium salt is dissolved in the first solvent to obtain an electrolyte.
[0066] Step S260: The bare cell and electrolyte are packaged to obtain the battery.
[0067] The battery is prepared through steps S210 to S260. The battery separator includes a base film 100, a first coating, and a second coating. Since the first coating includes an oily binder 120 and first ceramic particles 110, and the oily binder 120 and the first ceramic particles 110 are mixed, the first coating has good adhesion properties and can form a good adhesion to the electrode, giving the battery good hardness and flatness. The second coating includes an aqueous binder layer 130 and a ceramic layer 140. The second coating is applied to the second surface of the base film 100, and the aqueous binder layer 130 is applied on the ceramic layer 140, with the ceramic layer 140 located between the aqueous binder layer 130 and the second surface. Therefore, the second coating has a smaller shrinkage rate when heated, which can reduce the shrinkage of the separator when heated. Therefore, the separator in this embodiment has strong adhesion and is not easily shrinkable when heated, thereby improving battery safety and reducing the probability of safety accidents caused by insufficient adhesion between the separator and the electrode or by separator shrinkage when heated; and since the thickness of the second coating is greater than or equal to twice the thickness of the first coating, the separator can form gaps at the corners of the cell during cell encapsulation, so as to store more electrolyte and facilitate the flow of electrolyte.
[0068] It is understandable that the positive electrode slurry in step S210 is prepared in the following manner:
[0069] A positive electrode active material, a conductive agent, conductive carbon nanotubes, and a first binder are mixed in a second solvent to obtain a positive electrode slurry. The positive electrode active material comprises 96% to 98% by weight, the conductive agent comprises 0% to 1% by weight, the conductive carbon nanotubes comprises 0% to 1% by weight, and the first binder comprises 0.6% to 1.5% by weight. For example, the positive electrode active material may comprise 96%, 97%, or 98% by weight, the conductive agent may comprise 0%, 0.5%, or 1% by weight, the conductive carbon nanotubes may comprise 0%, 0.5%, or 1% by weight, and the first binder may comprise 0.6%, 1%, or 1.5% by weight. In one embodiment, the weight ratio of the positive electrode active material, the conductive agent, the conductive carbon nanotubes, and the first binder is 97.9:0.6:0.5:1.0.
[0070] It is worth noting that the positive electrode active material can be LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiMnPO4, LiFePO4, or LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.1 Mn 0.3 O2, LiNi 0.85 Co 0.15 Al 0.05 One or more of O2.
[0071] It is worth noting that the conductive agent is acetylene black, the first binder is polyvinylidene fluoride, and the second solvent is N-methylpyrrolidone; the positive electrode current collector is an aluminum current collector. After the positive electrode slurry is coated onto the aluminum current collector, the aluminum current collector is cold-pressed and then slit to form the positive electrode sheet.
[0072] It is understood that the negative electrode slurry in step S220 is prepared in the following manner:
[0073] A negative electrode active material, a dispersant, and a second binder are mixed to obtain a negative electrode slurry; wherein the weight percentage of the negative electrode active material is 96.5% to 98.5%, the weight percentage of the dispersant is 0% to 1%, and the weight percentage of the second binder is 0.7% to 1.5%. For example, the weight percentage of the negative electrode active material is 96.5%, 97.5%, or 98.5%, the weight percentage of the dispersant can be 0%, 0.5%, or 1%, and the weight percentage of the second binder can be 0.7%, 1%, or 1.5%. In one embodiment, the weight ratio of the negative electrode active material, the dispersant, and the second binder is 97.7:1:1.3.
[0074] It is worth noting that the second binder can be polyvinylidene fluoride. The negative electrode active material can be one or more of graphite, silicon, and hard carbon. The negative electrode current collector is a copper current collector. After the negative electrode slurry is coated onto the copper current collector, the copper current collector is cold-pressed and then slit to form the negative electrode sheet.
[0075] Understandably, in step S240, the positive electrode, negative electrode, and separator are wound or stacked to form a bare battery cell, with the separator located between the positive and negative electrode. In one embodiment, the first coating may contact the negative electrode of the battery, while the second coating may contact the positive electrode of the battery; in another embodiment, the first coating may contact the positive electrode of the battery, while the second coating may contact the negative electrode of the battery.
[0076] It is understood that in the first solvent, the volume percentage of ethylene carbonate is 5% to 20%, the volume percentage of propylene carbonate is 5% to 20%, the volume percentage of diethyl carbonate is 30% to 60%, and the volume percentage of propyl propionate is 30% to 60%. For example, the volume percentage of ethylene carbonate may be 5%, 15%, or 20%, the volume percentage of propylene carbonate may be 5%, 15%, or 20%, the volume percentage of diethyl carbonate may be 30%, 45%, or 60%, and the volume percentage of propyl propionate may be 30%, 40%, or 60%. In one embodiment, the volume ratio of ethylene carbonate, propylene carbonate, diethyl carbonate, and propyl propionate is 1:1:4:4.
[0077] It should be noted that some separators in related technologies use oil-based adhesives on both opposite surfaces, which has a weakness in terms of heat shrinkage, potentially leading to safety accidents due to separator shrinkage. Other separators in related technologies use water-based adhesives on both opposite surfaces, which can easily result in insufficient interfacial adhesion, posing a safety hazard. In contrast, the separator in this embodiment has strong adhesion and is less prone to shrinkage when heated, thereby improving battery safety and reducing the probability of safety accidents caused by insufficient adhesion between the separator and the electrodes or separator shrinkage when heated.
[0078] Table 1
[0079]
[0080] Referring to Table 1, which shows the diaphragm designs of seven specific embodiments of this application and two comparative examples in related technologies, D1 represents the diameter of the first ceramic particle, d1 represents the thickness of the first coating, D2 represents the diameter of the second ceramic particle, and d2 represents the thickness of the second coating. Table 1 shows the diaphragm designs of seven embodiments and two comparative examples, and specifically shows the thickness of the first and second coatings, the binder used, and the diameter of the ceramic particles in each embodiment or comparative example.
[0081] Table 2
[0082]
[0083] Referring to Table 2, the heat shrinkage performance of the diaphragm for each case corresponding to Table 1 was tested. Table 2 shows the heat shrinkage rate of the diaphragm for each case. When conducting the heat shrinkage performance test, the diaphragm was first cut into 10cm×10cm sizes, and the TD direction was marked. The cut diaphragm was placed in a 90℃ oven and baked for 0.5h. The dimensions before and after baking were measured. Heat shrinkage rate = (dimensional before baking - dimensional after baking) / dimensional before baking.
[0084] Referring to Table 2, the separators for each case in Table 1 were fabricated into battery cells. The cells underwent a hot box test, where the failure temperature was measured at 1°C intervals, with a heating rate of 2°C / minute, and held at the target temperature for 1 hour. Table 2 shows the target temperatures for the hot box test of each cell, and each cell passed the test.
[0085] Referring to Table 2, cycle performance tests were performed on each cell. Under normal temperature conditions, the cells were charged to 4.25V at a constant current rate of 2.7C, then to 4.5V at a constant current rate of 1.8C, followed by constant voltage charging to 200mA, and finally discharged to 3.0V at a DC rate of 0.7C. This charge-discharge cycle process was repeated 1000 times to obtain the cycle capacity retention rate of each cell.
[0086] As shown in Table 2, compared with Comparative Example 1, the separator thermal shrinkage rate of Examples 1 to 7 is lower, which can reduce the probability of safety accidents caused by separator shrinkage when the battery is heated. Furthermore, after 1000 cycle tests, the cell cycle capacity retention rate of Examples 1 to 7 is higher than that of Comparative Example 1 and Comparative Example 2. Therefore, compared with Comparative Example 1 and Comparative Example 2, the cell of this application has better cycle performance.
[0087] The embodiments of this application have been described in detail above with reference to the accompanying drawings. However, this application is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of this application. Furthermore, unless otherwise specified, the embodiments and features described in the embodiments of this application can be combined with each other.
Claims
1. A diaphragm, characterized by include: Base film; A first coating comprising an oily binder and first ceramic particles, wherein the oily binder is mixed with the first ceramic particles, and the first coating is applied to a first surface of the base film; The second coating comprises an aqueous adhesive layer and a ceramic layer, wherein the aqueous adhesive layer is coated on the ceramic layer, the second coating is coated on the second surface of the base film, and the ceramic layer is located between the aqueous adhesive layer and the second surface, the second surface being opposite to the first surface; The thickness of the second coating is greater than or equal to twice the thickness of the first coating; The diameter of the first ceramic particle is 0.5 micrometers to 1.5 micrometers; the ceramic layer includes a second ceramic particle with a diameter of 1 micrometer to 3 micrometers.
2. The separator according to claim 1, characterized in that The water-based adhesive layer includes any one or a mixture of several of the following: styrene-butadiene latex, styrene-acrylic latex, polymethyl methacrylate, polybutyl methacrylate, polyethyl methacrylate, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate, and polyurethane.
3. The separator of claim 1, wherein The oily binder includes any one or a mixture of several of the following: vinylidene fluoride homopolymer powder, vinylidene fluoride and hexafluoropropylene copolymer.
4. A battery, characterized in that, The battery includes a separator as described in any one of claims 1 to 3, and further includes a positive electrode and a negative electrode, wherein the separator is disposed between the positive electrode and the negative electrode.
5. A method for preparing a battery, characterized in that, include: The positive electrode slurry is coated onto the positive electrode current collector, and the positive electrode current collector is cold-pressed and then slit to obtain the positive electrode sheet; The negative electrode slurry is coated onto the negative electrode current collector, and the negative electrode current collector is cold-pressed and then slit to obtain the negative electrode sheet; An oil-based binder is mixed with first ceramic particles to form a first coating. The first coating is applied to a first surface of a base film. A ceramic layer is applied to a second surface of the base film. An aqueous binder layer is applied to the ceramic layer to obtain a separator. The second surface is opposite to the first surface. The aqueous binder layer and the ceramic layer form a second coating. The thickness of the second coating is greater than or equal to twice the thickness of the first coating. The diameter of the first ceramic particles is 0.5 to 1.5 micrometers. The ceramic layer includes second ceramic particles with a diameter of 1 to 3 micrometers. The positive electrode, the negative electrode, and the separator are used to form a bare battery cell; Ethylene carbonate, propylene carbonate, diethyl carbonate, and propyl propionate are mixed to obtain a first solvent. Lithium salt is dissolved in the first solvent to obtain an electrolyte. The battery is obtained by encapsulating the bare cell with the electrolyte.
6. The method for preparing a battery according to claim 5, characterized in that, The positive electrode slurry is prepared in the following manner: The positive electrode active material, conductive agent, conductive carbon nanotubes, and first binder are mixed in a second solvent to obtain the positive electrode slurry; wherein the weight percentage of the positive electrode active material is 96% to 98%, the weight percentage of the conductive agent is 0% to 1%, the weight percentage of the conductive carbon nanotubes is 0% to 1%, and the weight percentage of the first binder is 0.6% to 1.5%.
7. The method for preparing a battery according to claim 5, characterized in that, The negative electrode slurry is prepared in the following manner: The negative electrode active material, dispersant, and second binder are mixed to obtain the negative electrode slurry; wherein the weight percentage of the negative electrode active material is 96.5% to 98.5%, the weight percentage of the dispersant is 0% to 1%, and the weight percentage of the second binder is 0.7% to 1.5%.
8. The method for preparing a battery according to claim 5, characterized in that, The volume percentage of ethylene carbonate is 5% to 20%, the volume percentage of propylene carbonate is 5% to 20%, the volume percentage of diethyl carbonate is 30% to 60%, and the volume percentage of propyl propionate is 30% to 60%.
Citation Information
Patent Citations
Ceramic composite diaphragm and lithium ion battery
CN114374052A
Isolating membrane coating slurry, preparation method thereof and lithium ion battery
CN114583391A