An electrolyte, its preparation method, and a lithium-ion battery
By introducing phosphate and phenyl groups into the electrolyte as solvents and F-atom-containing additives, a stable interfacial film is formed, which solves the stability and safety problems of high-voltage lithium-ion batteries and improves the cycle and rate performance of the batteries.
Patent Information
- Application Number
- CN202310747816.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-06-25
AI Technical Summary
High-voltage lithium-ion batteries suffer from poor cathode oxidation stability, poor cycle stability, and flammable electrolyte, which affect battery safety and performance.
Solvent a, which has excellent flame-retardant properties, is introduced, along with an additive b containing F atoms, to form a P- and S-rich interfacial film and a F-rich inorganic layer. This improves the high-voltage stability and safety performance of the electrolyte, while reducing the electrolyte viscosity and inhibiting the dissolution of the positive electrode metal.
It significantly improves the high-voltage stability, cycle performance and safety performance of the battery, and forms a uniform and dense SEI film, thereby enhancing the battery's cycle and rate performance.
Smart Images

Figure CN117096451B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery technology, and particularly relates to an electrolyte, its preparation method, and a lithium-ion battery. Background Technology
[0002] Lithium-ion batteries have advantages such as high energy density, long cycle life, and environmental friendliness, and have been widely used in digital consumer electronics, electric vehicles, and energy storage. However, the development of high-voltage lithium-ion batteries is hampered by problems such as poor oxidation stability of the high-voltage cathode and poor cycle stability. At the same time, in traditional carbonate electrolytes, the presence of flammable solvents poses serious safety hazards, making electrolyte safety one of the key aspects of electrolyte design.
[0003] Therefore, it is imperative to develop a new electrolyte that balances electrode stability and safety. Summary of the Invention
[0004] The purpose of this invention is to address the shortcomings of existing technologies by providing an electrolyte in which solvent a is introduced with phosphate groups and phenyl groups that have excellent flame-retardant effects, further improving the high-voltage stability and safety performance of the electrolyte. Additive b introduces F atoms, which improves the stability of the electrolyte while inhibiting the dissolution of the positive electrode metal, thus significantly improving the battery cycle and rate performance and effectively enhancing the battery safety performance.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] An electrolyte of the present invention includes a lithium salt, an organic solvent, solvent a, additive b, and additive c, wherein solvent a is a compound represented by formula I, and additive b is a compound represented by formula II;
[0007]
[0008] R1, R2, R3, R4, R5, R6, R7, R8, R9, R10, R11, and R12 are each independently selected from one of H, a halogen atom, an alkane group having 1 to 10 carbon atoms, an unsaturated hydrocarbon group having 2 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkanoyl group having 2 to 10 carbon atoms, and a phenyl group, and the H in the alkane group, the unsaturated hydrocarbon group, the alkoxy group, and the alkanoyl group is partially or completely substituted by one or more of a halogen atom, a cyano group, a carboxyl group, and a sulfonic acid group.
[0009] Preferably, in the compound represented by Formula I, R1, R4, and R5 are alkane groups with 1 to 10 carbon atoms, and R2, R3, R6, and R7 are hydrogen atoms; in the compound represented by Formula II, R10 is an alkane group with 1 to 10 carbon atoms, R8, R9, and R12 are hydrogen atoms, and R11 is a halogen atom.
[0010] Preferably, in the compound represented by Formula I, R1 is methyl, R4 and R5 are ethyl, and R2, R3, R6 and R7 are hydrogen atoms; in the compound represented by Formula II, R10 is methyl, R8, R9 and R12 are hydrogen atoms, and R11 is a fluorine atom.
[0011] Preferably, additive c is one or more of the following: ethylene carbonate, fluoroethylene carbonate, ethylene ethylene carbonate, 1,3-propanesulfonate lactone, propylene sulfite, ethylene sulfate, 4-methylethylene sulfate, succinic anhydride, succinic anhydride, adiponitrile, and 1,3,6-hexanetrionitrile.
[0012] Preferably, the additive c is a mixture of fluoroethylene carbonate, 1,3-propanesulfonate lactone, and 1,3,6-hexanetrionitrile, wherein the mass ratio of the fluoroethylene carbonate, 1,3-propanesulfonate lactone, and 1,3,6-hexanetrionitrile is (5-8):(3-6):(1-5).
[0013] Preferably, the lithium salt is one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, and lithium difluorooxalate borate.
[0014] Preferably, the organic solvent includes cyclic organic solvents and chain organic solvents, wherein the cyclic organic solvent is one or more of ethylene carbonate, propylene carbonate, and butene carbonate, and the chain organic solvent is one or more of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethyl propionate, and propyl propionate.
[0015] According to another aspect of this application, this application provides a method for preparing an electrolyte, comprising the following steps:
[0016] 1) In a nitrogen-filled glove box, ethylene carbonate, propylene carbonate, diethyl carbonate, and propyl propionate are mixed in a weight ratio of (13-17):(6-12):(6-12):(60-70) to prepare an organic solvent.
[0017] 2) Slowly add lithium salt to the organic solvent to prepare a lithium salt solution with a concentration of 1.2 mol / L;
[0018] 3) The electrolyte is prepared by mixing lithium salt, organic solvent, solvent a, additive b and additive c in a weight ratio of (14-16):(35-70):(5-20):(1-10):(14-16).
[0019] According to another aspect of this application, this application provides a lithium-ion battery, including a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the electrolyte is the electrolyte described above.
[0020] The beneficial effects of this invention are as follows: Solvent a introduces phosphate and phenyl groups with excellent flame-retardant properties, further improving the high-voltage stability and safety performance of the electrolyte. The introduction of diethoxy groups provides multiple coordination sites with Li+, thereby reducing the electrolyte viscosity. Simultaneously, solvent a participates in the formation of positive and negative electrode films, generating dense and stable interface films rich in P and S, improving the battery's cycle and rate performance. Additive b introduces F atoms, improving electrolyte stability while participating in the formation of F-rich inorganic layer interface films on the positive and negative electrodes, inhibiting the dissolution of the positive electrode metal, and improving the battery's high-voltage cycle stability. The presence of methoxy groups provides coordination, further reducing electrolyte viscosity. In summary, the functional electrolyte additive of this invention can significantly improve battery cycle and rate performance. Its synergistic use with additive c forms a more uniform, dense, and low-impedance SEI film, thus further improving the battery's cycle, rate, and safety performance. Attached Figure Description
[0021] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 The electrolyte combustion tests are for Examples 1, 4 and Comparative Example 1 of this application. Detailed Implementation
[0023] To make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] According to one aspect of this application, an electrolyte is provided, comprising a lithium salt, an organic solvent, solvent a, additive b, and additive c, wherein solvent a is a compound represented by formula I, and additive b is a compound represented by formula II;
[0025]
[0026] R1, R2, R3, R4, R5, R6, R7, R8, R9, R10, R11, and R12 are each independently selected from one of H, a halogen atom, an alkane group having 1 to 10 carbon atoms, an unsaturated hydrocarbon group having 2 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkanoyl group having 2 to 10 carbon atoms, and a phenyl group, and the H in the alkane group, the unsaturated hydrocarbon group, the alkoxy group, and the alkanoyl group is partially or completely substituted by one or more of a halogen atom, a cyano group, a carboxyl group, and a sulfonic acid group.
[0027] In one embodiment of the present application, in the compound represented by Formula I, R1, R4 and R5 are alkane groups having 1 to 10 carbon atoms, and R2, R3, R6 and R7 are hydrogen atoms; in the compound represented by Formula II, R10 is an alkane group having 1 to 10 carbon atoms, R8, R9 and R12 are hydrogen atoms, and R11 is a halogen atom.
[0028] In one embodiment of the present application, in the compound represented by Formula I, R1 is methyl, R4 and R5 are ethyl, and R2, R3, R6 and R7 are hydrogen atoms; in the compound represented by Formula II, R10 is methyl, R8, R9 and R12 are hydrogen atoms, and R11 is a fluorine atom.
[0029] In solvent a, sulfone solvents introduce phosphate groups and phenyl groups with excellent flame-retardant effects, further improving the high-voltage stability and safety performance of the electrolyte. The introduction of bisethoxy groups provides multiple coordination sites with Li+, thereby reducing the electrolyte viscosity. At the same time, solvent a participates in the formation of positive and negative electrode films, generating dense and stable interface films rich in P and S, improving the cycle and rate performance of the battery. In additive b, benzonitrile with excellent high-voltage resistance introduces F atoms, improving the stability of the electrolyte while participating in the formation of F-rich inorganic layer interface films of positive and negative electrodes, inhibiting the dissolution of positive electrode metal, and improving the high-voltage cycle stability of the battery. At the same time, the presence of methoxy groups provides coordination, thereby reducing the electrolyte viscosity.
[0030] In one embodiment of this application, the additive c is one or more selected from ethylene carbonate, fluoroethylene carbonate, ethylene ethylene carbonate, 1,3-propanesulfonate lactone, propylene sulfite, ethylene sulfate, 4-methylethylene sulfate, succinic anhydride, succinic anhydride, adiponitrile, and 1,3,6-hexanetrionitrile.
[0031] In one embodiment of this application, the additive c is a mixture of fluoroethylene carbonate, 1,3-propanesulfonate lactone, and 1,3,6-hexanetrionitrile, wherein the mass ratio of the fluoroethylene carbonate, 1,3-propanesulfonate lactone, and 1,3,6-hexanetrionitrile is (5-8):(3-6):(1-5), for example, 5:6:5, 6:5:4, 7:4:3, or 8:3:1.
[0032] In one embodiment of this application, the lithium salt is one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, and lithium difluorooxalate borate.
[0033] In one embodiment of this application, the organic solvent includes cyclic organic solvents and chain organic solvents, wherein the cyclic organic solvent is one or more of ethylene carbonate, propylene carbonate, and butene carbonate, and the chain organic solvent is one or more of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethyl propionate, and propyl propionate.
[0034] According to another aspect of this application, this application provides a method for preparing an electrolyte, comprising the following steps:
[0035] 1) In a nitrogen-filled glove box, ethylene carbonate, propylene carbonate, diethyl carbonate, and propyl propionate are mixed in a weight ratio of (13-17):(6-12):(6-12):(60-70) to prepare an organic solvent.
[0036] 2) Slowly add lithium salt to the organic solvent to prepare a lithium salt solution with a concentration of 1.2 mol / L;
[0037] 3) The electrolyte is prepared by mixing lithium salt, organic solvent, solvent a, additive b and additive c in a weight ratio of (14-16):(35-70):(5-20):(1-10):(14-16).
[0038] According to another aspect of this application, this application provides a lithium-ion battery, including a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the electrolyte is the electrolyte described above.
[0039] The present application will be further described below with reference to specific embodiments.
[0040] Example 1
[0041] Positive electrode preparation: Positive electrode material 4.53V high voltage LiCoO2, binder PVDF (polyvinylidene fluoride), and conductive agent CNT were dispersed in NMP (N-methylpyrrolidone) organic solvent at a mass ratio of 98:1:1. The mixture was stirred under vacuum until stable and homogeneous, and then uniformly coated onto an aluminum foil with a thickness of 10μm. After drying the aluminum foil at room temperature, it was transferred to a 120℃ forced-air oven for 1 hour of drying. Then, it was cold-pressed and die-cut to form the positive electrode sheet.
[0042] Negative electrode preparation: Commercial graphite, PVDF binder, and CNT conductive agent were mixed together at a mass ratio of 97:2:1, dispersed in NMP organic solvent, and uniformly coated onto a copper foil with a thickness of 8 μm. After the aluminum foil was dried at room temperature, it was transferred to a 120°C forced-air oven for 1 hour of drying, and then cold-pressed and die-cut to form a negative electrode sheet.
[0043] Electrolyte preparation:
[0044] 1) Prepare an organic solvent in a glove box filled with nitrogen (O2 < 2 ppm, H2O < 3 ppm). The organic solvent consists of EC (ethylene carbonate), PC (propylene carbonate), DEC (diethyl carbonate), and PP (propyl propionate) in a weight ratio of 15:10:10:65.
[0045] 2) Slowly add LiPF6 to the organic solvent to prepare a lithium salt solution with a concentration of 1.2 mol / L;
[0046] 3) An electrolyte is prepared by mixing lithium salt solution, organic solvent, solvent a, additive b and additive c in weight parts of 15 parts, 59 parts, 10 parts, 1 part and 15 parts respectively.
[0047] Solvent a is a compound of formula 1, and additive b is a compound of formula 2, the structures of which are shown below:
[0048]
[0049] Lithium-ion battery fabrication: The positive electrode, separator, and negative electrode are stacked in sequence and wound to obtain a bare cell. The cell is then packaged in an aluminum-plastic film, baked, injected with electrolyte, left to stand, formed, shaped in a fixture, resealed, and its capacity is tested to complete the fabrication of the lithium-ion battery.
[0050] Example 2
[0051] The difference from Example 1 is that the lithium salt solution, organic solvent, solvent a, additive b, and additive c are in parts by weight of 15 parts, 58 parts, 10 parts, 2 parts, and 15 parts, respectively.
[0052] The rest is the same as in Example 1, and will not be repeated here.
[0053] Example 3
[0054] The difference from Example 1 is that the lithium salt solution, organic solvent, solvent a, additive b, and additive c are in parts by weight of 15 parts, 57 parts, 10 parts, 3 parts, and 15 parts, respectively.
[0055] The rest is the same as in Example 1, and will not be repeated here.
[0056] Example 4
[0057] The difference from Example 1 is that solvent a is a compound of formula 3, with the structure shown below:
[0058]
[0059] The rest is the same as in Example 1, and will not be repeated here.
[0060] Example 5
[0061] The difference from Example 1 is that additive b consists only of compounds of Formula 4, the structural formula of which is shown below:
[0062]
[0063] The rest is the same as in Example 1, and will not be repeated here.
[0064] Example 6
[0065] The difference from Example 1 is that the lithium salt solution, organic solvent, solvent a, additive b, and additive c are in parts by weight of 15 parts, 64 parts, 5 parts, 1 part, and 15 parts, respectively.
[0066] The rest is the same as in Example 1, and will not be repeated here.
[0067] Example 7
[0068] The difference from Example 1 is that the lithium salt solution, organic solvent, solvent a, additive b, and additive c are in parts by weight of 15 parts, 49 parts, 20 parts, 1 part, and 15 parts, respectively.
[0069] The rest is the same as in Example 1, and will not be repeated here.
[0070] Example 8
[0071] The difference from Example 1 is that the lithium salt solution, organic solvent, solvent a, additive b, and additive c are in parts by weight of 15 parts, 39 parts, 10 parts, 1 part, and 15 parts, respectively.
[0072] The rest is the same as in Example 1, and will not be repeated here.
[0073] Comparative Example 1
[0074] The difference from Example 1 is that the lithium salt solution, organic solvent, additive b, and additive c are in parts by weight of 15 parts, 69 parts, 1 part, and 15 parts, respectively.
[0075] The rest is the same as in Example 1, and will not be repeated here.
[0076] Comparative Example 2
[0077] The difference from Example 1 is that the lithium salt solution, organic solvent, solvent a, and additive c are in parts by weight of 15, 60, 10, and 15, respectively.
[0078] The rest is the same as in Example 1, and will not be repeated here.
[0079] The lithium-ion batteries obtained in the examples and comparative examples were subjected to electrochemical performance tests, and the experimental results are shown in Tables 1 and 2.
[0080] Room temperature / high temperature cycle test: Place the battery in an oven at a constant temperature of 25℃ / 45℃ for 4 hours, then charge it at a constant current of 0.5C to 4.53V, then charge it at a constant voltage until the current drops to 0.05C, then discharge it at a constant current of 1C to 3.0V. Repeat this cycle and record the initial capacity of the battery and the discharge capacity of the last cycle (300 / 200th cycle).
[0081] Capacity retention rate = discharge capacity in the last cycle (cycle 300 / 200) / initial capacity × 100%.
[0082] Rate performance: The battery is charged at a constant current of 0.5C to 4.53V in an environment of 25℃, charged at a constant voltage until the current drops to 0.02C, and then discharged at a constant current of 0.2C / 1C / 2C / 3C / 5C to 3.0V. This is recorded as the discharge capacity of the cell.
[0083] Capacity retention rate at different discharge rates = discharge capacity at different discharge rates / initial capacity at 0.2C × 100%.
[0084] Electrolyte combustion test: such as Figure 1 As shown, cotton balls soaked in different electrolytes (Example 1, Example 4 and Comparative Example 1) were brought close to the outer flame of an alcohol lamp, and then the cotton balls were removed from the outer flame to observe the burning of the cotton balls.
[0085] Table 1
[0086]
[0087] Table 2
[0088]
[0089] The above test results show that the electrolyte combustion test results indicate that ( Figure 1 Example 1 did not burn, Example 4 burned, and Comparative Example 1 burned, proving that solvent a has a significant flame retardant effect.
[0090] The battery prepared in Example 1 with a novel solvent a, novel additive b, and additive c in a fixed ratio showed improved cycle capacity retention, rate performance, and capacity retention. Moreover, the battery prepared in Example 1 achieved the best performance compared to other examples and comparative examples.
[0091] Based on the disclosure and teachings of the foregoing specification, those skilled in the art can make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments described above, and any obvious improvements, substitutions, or modifications made by those skilled in the art based on the present invention are within the scope of protection of the present invention. Furthermore, although some specific terms are used in this specification, these terms are only for convenience of explanation and do not constitute any limitation on the present invention.
Claims
1. An electrolyte, characterized in that, It includes lithium salt, organic solvent, solvent a and additive b, wherein solvent a is a compound represented by formula I and additive b is a compound represented by formula II; Formula I Formula II In the compound represented by Formula I, R1, R4, and R5 are alkane groups with 1 to 10 carbon atoms, and R2, R3, R6, and R7 are hydrogen atoms; in the compound represented by Formula II, R10 is an alkane group with 1 to 10 carbon atoms, R8, R9, and R12 are hydrogen atoms, and R11 is a fluorine atom. The organic solvent includes cyclic organic solvents and chain organic solvents. The cyclic organic solvent is one or more of ethylene carbonate, propylene carbonate, and butene carbonate. The chain organic solvent is one or more of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethyl propionate, and propyl propionate.
2. The electrolyte according to claim 1, characterized in that, In the compound represented by Formula I, R1 is methyl, R4 and R5 are ethyl, and R2, R3, R6 and R7 are hydrogen atoms; in the compound represented by Formula II, R10 is methyl, and R8, R9 and R12 are hydrogen atoms.
3. The electrolyte according to claim 1, characterized in that, It also includes additive c, which is one or more of ethylene carbonate, fluoroethylene carbonate, ethylene ethylene carbonate, 1,3-propanesulfonate lactone, propylene sulfite, ethylene sulfate, 4-methylethylene sulfate, succinic anhydride, succinic anhydride, adiponitrile, and 1,3,6-hexanetrionitrile.
4. The electrolyte according to claim 3, characterized in that, The additive c is a mixture of fluoroethylene carbonate, 1,3-propanesulfonate lactone, and 1,3,6-hexanetrionitrile, wherein the mass ratio of the fluoroethylene carbonate, 1,3-propanesulfonate lactone, and 1,3,6-hexanetrionitrile is (5-8):(3-6):(1-5).
5. The electrolyte according to claim 1, characterized in that, The lithium salt is one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, and lithium difluorooxalate borate.
6. A method for preparing an electrolyte according to any one of claims 3-4, characterized in that, Includes the following steps: 1) In a nitrogen-filled glove box, ethylene carbonate, propylene carbonate, diethyl carbonate, and propyl propionate are mixed in a weight ratio of (13-17):(6-12):(6-12):(60-70) to prepare an organic solvent. 2) Slowly add lithium salt to the organic solvent to prepare a lithium salt solution with a concentration of 1.2 mol / L; 3) An electrolyte is prepared by mixing lithium salt, organic solvent, solvent a, additive b and additive c in a weight ratio of (14-16):(35-70):(5-20):(1-10):(14-16).
7. A lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that, The electrolyte is the electrolyte according to any one of claims 1-5.
Citation Information
Patent Citations
A lithium ion battery resistant to high voltage and an electrolyte thereof
CN108963340A
Method for detecting 11 organophosphorus pesticide residues in radix paeoniae alba by ultra-high performance liquid chromatography-mass spectrometry