An electrochemical device and an electronic device

By combining bilayer graphene-coated micron-sized silicon with a low-temperature electrolyte, the volume expansion and low-temperature performance issues of micron-sized silicon-based anode materials in lithium-ion batteries are solved, thereby improving the battery's cycle performance and energy density.

CN117154024BActive Publication Date: 2026-11-10LIYANG TIANMU PILOT BATTERY MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210565287.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-23
Publication Date
2026-11-10
Estimated Expiration
2042-05-23

AI Technical Summary

Technical Problem

Micron-sized silicon-based anode materials in lithium-ion batteries suffer from SEI film breakage and decreased cycle performance due to volume expansion. Solvent co-intercalation at low temperatures leads to increased electrolyte viscosity and reduced lithium-ion migration rate, all of which affect battery performance.

Method used

The anode material uses a double-layer graphene-coated micron-sized silicon and a low-temperature electrolyte, including propylene carbonate and other low-temperature solvents, to avoid solvent co-intercalation and improve the low-temperature performance of the anode material.

Benefits of technology

It effectively alleviates the volume expansion of micron-sized silicon, improves the low-temperature cycle performance of the anode material and the energy density of the battery, and increases the battery's range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117154024B_ABST
    Figure CN117154024B_ABST
Patent Text Reader

Abstract

The present application relates to an electrochemical device and an electronic device, the electrochemical device comprising a negative electrode sheet and a low-temperature electrolyte; the negative electrode sheet comprising a negative electrode material layer, the negative electrode material layer comprising a negative electrode material composite, the negative electrode material composite being a composite material of a negative electrode active material and hard carbon, the negative electrode active material being composed of micron silicon and double-layer graphene material coated on the micron silicon, and not containing any of artificial graphite, natural graphite, massive graphite, flaky graphite or microcrystalline graphite; wherein the first graphene material forms a first mixed phase with the micron silicon, the first mixed phase forms a second mixed phase after heat treatment, and then forms a third mixed phase with the second graphene material, and the third mixed phase forms the negative electrode active material after heat treatment; the mass percentage of the first graphene material in the first mixed phase is 10%-30%; the mass percentage of the second graphene material in the third mixed phase is 5%-20%; and the low-temperature electrolyte comprises a low-temperature solvent, and the low-temperature solvent comprises propylene carbonate (PC) and other low-temperature solvents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials technology, and more particularly to an electrochemical device and an electronic device. Background Technology

[0002] Silicon-based anodes possess extremely high theoretical specific capacity, making them a popular anode material. Micron-sized silicon is one of the most closely watched materials. However, micron-sized silicon exhibits significant volume expansion, resulting in approximately 400% volume change during lithium-ion insertion / extraction. This stress is sufficient to cause the solid electrolyte interphase (SEI) film to break down, leading to material pulverization and impacting battery cycle performance.

[0003] To address this issue, most commercially available silicon-based lithium-ion batteries utilize silicon-based materials in conjunction with graphite, leveraging the low expansion of graphite's single-phase structure to mitigate the expansion of silicon-based materials. However, other problems also exist.

[0004] Commercially viable electrolytes for silicon-based composite materials use ethylene carbonate (EC) or fluoroethylene carbonate (FEC) as solvents. However, solvent co-intercalation is prone to occur at low temperatures. Furthermore, because the graphite interlayers are governed by intermolecular forces, solvent co-intercalation causes reduction reactions between solvent molecules and electrons, generating stress that damages the graphite layer structure. Simultaneously, the bonding between the solvent and lithium ions increases the radius of the lithium ions, further disrupting the graphite interlayer structure during the intercalation / deintercalation process and leading to decreased cycle performance.

[0005] In summary, there are three main reasons for the poor low-temperature performance of anode materials: 1. The viscosity of the electrolyte increases and the conductivity decreases under low-temperature conditions; 2. The electrode impedance at the electrolyte / electrode interface increases; 3. The migration rate of lithium ions in the active material decreases. Summary of the Invention

[0006] This invention provides an electrochemical device and an electronic device. The invention uses a double-layer graphene coating, which effectively alleviates the volume expansion of micron-sized silicon. The low-temperature electrolyte combined with a graphite-free composite system effectively avoids the problem of solvent co-intercalation. In addition, it also effectively improves the low-temperature performance of the negative electrode material.

[0007] In a first aspect, embodiments of the present invention provide an electrochemical device, including a negative electrode and a low-temperature electrolyte;

[0008] The negative electrode sheet includes a negative electrode material layer.

[0009] The negative electrode material layer includes a negative electrode material composite, which is a composite material of a negative electrode active material and hard carbon. The negative electrode active material is composed of micron-sized silicon and a bilayer graphene material coated with micron-sized silicon. Specifically, a first graphene material forms a first mixed phase with micron-sized silicon; the first mixed phase is heat-treated to form a second mixed phase, which is then heat-treated to form a third mixed phase with a second graphene material. The third mixed phase is then heat-treated to form the negative electrode active material. The first graphene material accounts for 10%-30% of the mass percentage of the first mixed phase; the second graphene material accounts for 5%-20% of the mass percentage of the third mixed phase.

[0010] The cryogenic electrolyte includes a cryogenic solvent, which includes propylene carbonate (PC) and other cryogenic solvents; the other cryogenic solvents include ethers and / or carbonate solvents; the ethers include one or more of diethylene glycol butyl ether, ethylene glycol dimethyl ether, dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dimethoxymethane, and 1,2-dimethoxyethane; the carbonate solvents include one or more of diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, and ethyl propyl carbonate.

[0011] Preferably, the first graphene material has 2-10 layers, and the size of the first graphene material layer is ≤45μm;

[0012] The second graphene material has 1-9 layers, and the size of each layer is ≤65μm.

[0013] The Dv50 of the micron-sized silicon is 1μm≤Dv50≤5μm.

[0014] More preferably, the number of layers in the second graphene material is less than the number of layers in the first graphene material; and the sheet size of the second graphene material is greater than the sheet size of the first graphene material.

[0015] Preferably, the negative electrode material layer does not contain any of the following: artificial graphite, natural graphite, block graphite, flake graphite, or microcrystalline graphite.

[0016] Preferably, the negative electrode material layer further includes a dispersant and a binder.

[0017] Preferably, the mass ratio of propylene carbonate to the other low-temperature solvent is 2:8.

[0018] Preferably, the negative electrode material composite is obtained by combining the negative electrode active material and hard carbon with a specific capacity of 600 mAh / g.

[0019] In a second aspect, embodiments of the present invention provide an electronic device including the electrochemical device described in the first aspect above.

[0020] The electrochemical device proposed in this invention effectively mitigates the volume expansion of micron-sized silicon by employing a double-layer graphene coating; the use of a low-temperature electrolyte in conjunction with a graphite-free composite system effectively avoids the problem of solvent co-intercalation, ensuring cycle performance and effectively improving the low-temperature performance of the anode material. Simultaneously, using micron-sized silicon as the substrate significantly increases the battery's energy density and extends its battery life. Attached Figure Description

[0021] The technical solutions of the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings and examples.

[0022] Figure 1 This is a flowchart illustrating the preparation method of the electrochemical device according to an embodiment of the present invention. Detailed Implementation

[0023] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. However, it should be understood that these embodiments are only for more detailed description and should not be construed as limiting the present invention in any way, that is, not intended to limit the scope of protection of the present invention.

[0024] The electrochemical device of the present invention includes a negative electrode and a low-temperature electrolyte;

[0025] The negative electrode sheet includes a material layer;

[0026] The negative electrode material layer includes a negative electrode material composite, which is a composite material of negative electrode active material and hard carbon. The negative electrode active material is composed of micron-sized silicon and bilayer graphene material coated with micron-sized silicon. The first graphene material forms a first mixed phase with micron-sized silicon. The first mixed phase is heat-treated to form a second mixed phase, which is then heat-treated with the second graphene material to form a third mixed phase. The third mixed phase is then heat-treated to form the negative electrode active material.

[0027] The first graphene material accounts for 10%-30% of the mass percentage of the first mixed phase; the second graphene material accounts for 5%-20% of the mass percentage of the third mixed phase; the number of layers of the second graphene material is less than the number of layers of the first graphene material; and the sheet size of the second graphene material is greater than the sheet size of the first graphene material.

[0028] The Dv50 of micron-sized silicon is 1μm≤Dv50≤5μm;

[0029] The Dv50 of the micron-sized silicon described above is 1μm ≤ Dv50 ≤ 5μm; this value was obtained through rigorous theoretical analysis and practical testing during the invention process. When the Dv50 of the micron-sized silicon is too small (less than 1μm), its specific surface area increases, the material activity increases, and the contact between the negative electrode active material and the electrolyte increases, leading to increased side reactions and electrolyte consumption, thus affecting the cycle performance and safety performance of the electrochemical device. When the Dv50 of the micron-sized silicon is too large (greater than 5μm), the Dv50 after secondary granulation is too large, the contact between the negative electrode active materials deteriorates, affecting the cycle stability of the electrochemical device.

[0030] Furthermore, in a preferred embodiment of this application, the first graphene material comprises 2-10 layers, and the size of each layer is ≤45μm. For example, the number of layers can be 2, 3, 4, 5, 6, 7, 8, 9, or 10. The layer size described here refers to the particle size of the layer, which is a dimensional characteristic of the layer on the xy-plane in a three-dimensional coordinate system, and can be understood as particle size; while the number of layers is a parameter of the graphene thickness, located in the z-direction. The applicant has found that when the number of graphene layers exceeds 10, its overall performance decreases; if the size of the graphene material layer is greater than 45μm, the particle size of the secondary granulation is too large, resulting in poor contact between the negative electrode active materials and affecting the cycle stability of the electrochemical device. The first graphene material accounts for 10%-30% of the mass percentage of the first mixed phase, and can be 10%, 15%, 20%, 25%, 30%, or any value within this range. The applicant discovered that when the content is below 10%, the integrity of the micron-sized silicon coating is poor, and when it is above 30%, it affects the coating of secondary graphene.

[0031] In a preferred embodiment of this application, the second graphene material has 1-9 layers, and the size of the second graphene material layer is ≤65μm. For example, the number of layers can be 1, 2, 3, 4, 5, 6, 7, 8, or 9. The applicant has found that if the size of the second graphene material layer is greater than 65μm, the particle size of the secondary granulation is too large, resulting in poor contact between the negative electrode active materials and affecting the cycle stability of the electrochemical device. The second graphene material accounts for 5%-20% of the mass percentage of the third mixed phase. For example, it can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, or any value within this range. The applicant has found that when it is below 5%, the integrity of the micron-sized silicon coating is poor; when it is above 20%, it affects the yield and pulping performance of the final product. Simultaneously, a high graphite content in the negative electrode material affects the energy density of the lithium-ion battery.

[0032] The second graphene material has fewer layers than the first graphene material. For example, if the first graphene material has 5 layers, the second graphene material can have any number of layers: 1, 2, 3, or 4. The applicant has found that when using two graphene layers of different thicknesses, a combination of a small, thick inner graphene layer and a thin, large outer graphene layer is more effective. This is because using small-particle graphene as the inner coating layer allows for effective adhesion to micron-sized silicon, increasing interfacial bonding. If large-particle graphene is used as the inner coating layer, there are numerous gaps between the inner layer and the micron-sized silicon, resulting in weak bonding and a lower tap density, which affects the material's energy density. Using thin, large graphene as the outer coating layer ensures complete coating of the primary particles, guaranteeing coating integrity, and the fewer the bonding points between the thin graphene sheets, the lower the contact resistance. Moreover, the outer layer uses thin-layer graphene, which has better conductivity and mechanical properties, and is beneficial for lithium ion insertion / extraction and rate performance improvement.

[0033] The negative electrode material layer of the present invention also includes a dispersant and a binder, both of which can be commonly used dispersants and binders for negative electrodes.

[0034] It should be noted that the negative electrode active material or negative electrode material layer of the present invention does not contain any of the following: artificial graphite, natural graphite, block graphite, flake graphite or microcrystalline graphite.

[0035] The negative electrode sheet of the present invention also includes a negative electrode current collector. The present invention does not have any particular limitation on the negative electrode current collector, as long as it can achieve the purpose of the present invention. For example, it may include, but is not limited to, copper foil, copper alloy foil, nickel foil, stainless steel foil, foamed nickel, foamed copper or composite current collector, etc.

[0036] The cryogenic electrolyte of this invention includes a cryogenic solvent, which includes propylene carbonate (PC) and other cryogenic solvents; other cryogenic solvents include ethers and / or carbonate solvents; ethers include one or more of diethylene glycol butyl ether, ethylene glycol dimethyl ether, dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dimethoxymethane, and 1,2-dimethoxyethane; carbonate solvents include one or more of diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, and ethyl propyl carbonate. Preferably, the mass ratio of propylene carbonate to other cryogenic solvents is 2:8.

[0037] In this invention, the electrochemical device may also include a positive electrode, without any particular limitation herein.

[0038] The electrochemical device of the present invention is not particularly limited and may include any device in which an electrochemical reaction occurs. In some embodiments, the electrochemical device may include, but is not limited to, lithium metal secondary batteries, lithium-ion secondary batteries, lithium polymer secondary batteries, or lithium-ion polymer secondary batteries or capacitors. This electrochemical device can be used in electronic devices.

[0039] This invention utilizes highly conductive propylene carbonate as the main solvent and low-viscosity, low-melting-point ethers and carbonates as secondary solvents, effectively reducing electrolyte viscosity and increasing electrolyte conductivity. Simultaneously, employing 1-5 micrometer-sized micron-sized silicon helps shorten the lithium-ion diffusion path, reducing diffusion resistance and electrochemical polarization, while providing more lithium intercalation sites and improving low-temperature cycling performance. Furthermore, the double-layer infiltration coating with graphene of different sizes effectively isolates side reactions caused by electrolyte infiltration and reduces interfacial resistance, further enhancing the battery's low-temperature cycling performance.

[0040] The electrochemical device proposed in this invention has good cycle performance and safety performance, thereby enabling the electronic device to have a long service life.

[0041] In the aforementioned electrochemical device, it has been stated that the active layer of the negative electrode material is composed of micron-sized silicon and a bilayer graphene material coating micron-sized silicon. The electrochemical device of this invention can be prepared by the following method, specifically as follows: Figure 1 As shown, the main steps include:

[0042] Step 110: Prepare the negative electrode sheet;

[0043] The method includes: weighing the negative electrode material composite, conductive additives, and binders according to the required proportions, and preparing a slurry in a pulping machine at room temperature. The prepared slurry is then uniformly coated onto the negative electrode and the fluid, dried in a forced-air drying oven, cut into electrode sheets, and vacuum-dried in a vacuum drying oven. The dried electrode sheets are then immediately transferred to a glove box for later use in battery assembly.

[0044] The preparation of the anode material composite specifically includes:

[0045] Step 111: Micron-sized silicon and the first graphene material are mixed in a certain proportion and spray-dried to obtain the first mixed phase;

[0046] Step 112: Heat-treat the first mixed phase at 600℃-1000℃ for 2-12 hours under a nitrogen atmosphere to obtain the second mixed phase;

[0047] Step 113: The second mixed phase and the second graphene material are mixed in a certain proportion and spray-dried to obtain the third mixed phase;

[0048] Step 114: The third mixed phase is heat-treated at 600℃-1000℃ for 2-12 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0049] Step 115: The negative electrode active material and hard carbon are compounded at a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0050] Step 120: Prepare the positive electrode sheet;

[0051] The positive electrode active material, conductive agent, and binder are mixed in the required proportions, a solvent is added, and the mixture is stirred evenly under vacuum to obtain a positive electrode slurry. The positive electrode slurry is then uniformly coated onto a positive electrode current collector and dried to obtain a positive electrode sheet with a positive electrode material layer.

[0052] Step 130: Prepare a low-temperature electrolyte;

[0053] In an argon atmosphere glove box with a water content of <10ppm, propylene carbonate and other low-temperature solvents are mixed evenly at a mass ratio of 2:8 to obtain an organic solvent. Then, lithium salt LiPF6 is added to the organic solvent and mixed evenly to obtain a low-temperature electrolyte.

[0054] In one specific embodiment of the present invention, the lithium salt content in the low-temperature electrolyte is 12.5%.

[0055] Step 140: Assemble the electrochemical device;

[0056] Assemble the electrochemical device according to the following steps: positive electrode shell + positive electrode + separator + negative electrode + gasket + spring sheet + negative electrode shell; before assembling the battery, drop 100 μL of low-temperature electrolyte onto both the negative electrode and the positive electrode.

[0057] The choice of diaphragm is not specifically limited here.

[0058] To better understand the technical solutions provided by the present invention, the following uses several specific examples to illustrate the specific process of preparing electrochemical devices using the methods provided in the above embodiments of the present invention, and the electrochemical characteristics obtained by testing them.

[0059] In this embodiment, the preparation method is as follows:

[0060] Preparation of negative electrode sheet:

[0061] The negative electrode material composite, conductive additive carbon black, and binder (sodium cellulate and styrene-butadiene rubber in a 1:1 ratio) obtained by the above method are weighed in a ratio of 95:2:3. A slurry is prepared in a pulping machine at room temperature. The prepared slurry is evenly coated onto copper foil. After drying in a forced-air drying oven at 50°C for 2 hours, it is cut into 8×8mm electrode sheets and vacuum-dried in a vacuum drying oven at 100°C for 10 hours. The dried electrode sheets are then immediately transferred to a glove box for use in battery assembly.

[0062] Preparation of the positive electrode sheet:

[0063] Lithium cobalt oxide (LiCoO2), acetylene black (conductive agent), and polyvinylidene fluoride (PVDF) (binder) were mixed in a mass ratio of 96:2:2. N-methylpyrrolidone (NMP) was added, and the mixture was stirred evenly under vacuum to obtain a positive electrode slurry. The positive electrode slurry was uniformly coated onto one surface of an aluminum foil current collector and dried to obtain a positive electrode sheet with a single-sided coating of the positive electrode material. The above steps were repeated on the other surface of the aluminum foil to obtain a positive electrode sheet with a double-sided coating of the positive electrode material.

[0064] Preparation of low-temperature electrolyte:

[0065] In an argon atmosphere glove box with a water content of <10ppm, propylene carbonate and other selected low-temperature solvents are mixed evenly at a mass ratio of 2:8 to obtain an organic solvent. Then, lithium salt LiPF6 is added to the organic solvent and mixed evenly to obtain a low-temperature electrolyte, wherein the lithium salt content is 12.5%.

[0066] The following is a further detailed description of each embodiment.

[0067] Example 1

[0068] Micron-sized silicon with a Dv50 of 3.8 μm and a first graphene material with a sheet size of 28 μm and a number of layers of 7 were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 18% of the mass percentage of the first mixed phase.

[0069] The first mixed phase was treated at 900°C under a nitrogen atmosphere for 4 hours to obtain the second mixed phase;

[0070] The second mixed phase and a second graphene material with a sheet size of 50 μm and a number of layers of 4 were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 20% of the mass percentage of the third mixed phase.

[0071] The third mixed phase was heat-treated at 850°C for 6 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0072] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0073] The preparation methods for the negative electrode, low-temperature electrolyte, and positive electrode are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: methyl propyl carbonate: diethyl carbonate = 2:2:6, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0074] Constant current charge-discharge mode tests were conducted using a charge-discharge meter. At 25°C, the discharge cutoff voltage was 0.005V and the charge cutoff voltage was 1.5V. The first week of charge-discharge tests were conducted at a current density of C / 10, and the second week of discharge tests were conducted at a current density of C / 10.

[0075] The specific capacity of the negative electrode is 599mAh / g, and the efficiency in the first week is 87%.

[0076] Under the above conditions, a cyclic test was conducted, and the capacity retention rate was 95% after 500 cycles at room temperature.

[0077] Constant current charge-discharge mode tests were conducted using a charge-discharge meter. At -40℃, the discharge cutoff voltage was 0.005V and the charge cutoff voltage was 1.5V. The first week of charge-discharge tests were conducted at a current density of C / 10, and the second week of discharge tests were conducted at a current density of C / 10.

[0078] Under the above conditions, a cyclic test was conducted, and the capacity retention rate was 90% after 500 cycles of low temperature cycling.

[0079] Example 2

[0080] Micron-sized silicon with a Dv50 of 2.4 μm and a first graphene material with a sheet size of 40 μm and a number of layers of 5 were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 26% of the mass percentage of the first mixed phase.

[0081] The first mixed phase was treated at 700°C under a nitrogen atmosphere for 5 hours to obtain the second mixed phase;

[0082] The second mixed phase and a second graphene material with a sheet size of 58 μm and a number of layers of 3 were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 14% of the mass percentage of the third mixed phase;

[0083] The third mixed phase was heat-treated at 850°C for 8 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0084] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0085] The preparation methods for the negative electrode, low-temperature electrolyte, and positive electrode are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: methyl propyl carbonate: ethylene glycol dimethyl ether = 2:2:6, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0086] The specific capacity of the negative electrode is 601mAh / g, and the efficiency in the first week is 86.8%.

[0087] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 95% at room temperature and 90% at low temperature after 500 cycles.

[0088] Example 3

[0089] Micron-sized silicon with a Dv50 of 3.7 μm and a first graphene material with a sheet size of 36 μm and 6 layers were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 27% of the mass percentage of the first mixed phase.

[0090] The first mixed phase was treated under a nitrogen atmosphere at 600°C for 10 hours to obtain the second mixed phase;

[0091] The second mixed phase and a second graphene material with a sheet size of 57 μm and a number of layers were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 16% of the mass percentage of the third mixed phase;

[0092] The third mixed phase was heat-treated at 900°C for 7 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0093] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0094] The preparation methods for the negative electrode, low-temperature electrolyte, and positive electrode are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: methyl propyl carbonate: ethyl propyl carbonate = 2:4:4, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0095] The specific capacity of the negative electrode is 599mAh / g, and the efficiency in the first week is 86.5%.

[0096] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 94% after 500 cycles at room temperature and 91% after low temperature cycling.

[0097] Example 4

[0098] Micron-sized silicon with a Dv50 of 4.8 μm and a first graphene material with a sheet size of 32 μm and 8 layers were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 24% of the mass percentage of the first mixed phase.

[0099] The first mixed phase was treated at 850°C under a nitrogen atmosphere for 5 hours to obtain the second mixed phase;

[0100] The second mixed phase and a second graphene material with a sheet size of 60 μm and a number of layers of 3 were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 14% of the mass percentage of the third mixed phase;

[0101] The third mixed phase was heat-treated at 1000℃ for 8 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0102] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0103] The preparation methods for the negative electrode, low-temperature electrolyte, and positive electrode are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: diethylene glycol dimethyl ether: tetraethylene glycol dimethyl ether = 2:4:4, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0104] The specific capacity of the negative electrode is 598mAh / g, and the efficiency in the first week is 86.6%.

[0105] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 93% at room temperature after 500 cycles and 88% at low temperature.

[0106] Example 5

[0107] Micron-sized silicon with a Dv50 of 3.5 μm and a first graphene material with a sheet size of 36 μm and 8 layers were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 18% of the mass percentage of the first mixed phase.

[0108] The first mixed phase was treated at 900°C under a nitrogen atmosphere for 4 hours to obtain the second mixed phase;

[0109] The second mixed phase and a second graphene material with a sheet size of 48 μm and a number of layers of 6 were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 20% of the mass percentage of the third mixed phase.

[0110] The third mixed phase was heat-treated at 850°C for 10 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0111] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0112] The preparation methods for the negative electrode, low-temperature electrolyte, and positive electrode are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: dipropyl carbonate: diethyl carbonate = 2:3:5, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0113] The specific capacity of the negative electrode is 605mAh / g, and the efficiency in the first week is 86.2%.

[0114] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 94% at room temperature after 800 cycles and 90% at low temperature.

[0115] Example 6

[0116] Micron-sized silicon with a Dv50 of 2.9 μm and a first graphene material with a sheet size of 36 μm and 5 layers were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 26% of the mass percentage of the first mixed phase.

[0117] The first mixed phase was treated under a nitrogen atmosphere at 800°C for 10 hours to obtain the second mixed phase;

[0118] The second mixed phase and a second graphene material with a sheet size of 56 μm and a number of layers of 2 were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 18% of the mass percentage of the third mixed phase;

[0119] The third mixed phase was heat-treated at 1000℃ for 4 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0120] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0121] The preparation methods for the negative electrode, low-temperature electrolyte, and positive electrode are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: dipropyl carbonate: tetraethylene glycol dimethyl ether = 2:3:5, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0122] The specific capacity of the negative electrode is 599mAh / g, and the efficiency in the first week is 86.7%.

[0123] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 93% at room temperature and 90% at low temperature after 500 cycles.

[0124] Example 7

[0125] Micron-sized silicon with a Dv50 of 1.2 μm and a first graphene material with a sheet size of 40 μm and a number of layers were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 24% of the mass percentage of the first mixed phase.

[0126] The first mixed phase was treated at 950°C under a nitrogen atmosphere for 6 hours to obtain the second mixed phase;

[0127] The second mixed phase and a second graphene material with a sheet size of 60 μm and a number of layers of 2 were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 15% of the mass percentage of the third mixed phase;

[0128] The third mixed phase was heat-treated at 950°C for 6 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0129] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0130] The preparation methods for the negative electrode, low-temperature electrolyte, and positive electrode are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: dipropyl carbonate: diethyl carbonate = 2:3:5, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0131] The specific capacity of the negative electrode is 603mAh / g, and the efficiency in the first week is 86.5%.

[0132] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 95% at room temperature and 89% at low temperature after 500 cycles.

[0133] Example 8

[0134] Micron-sized silicon with a Dv50 of 3.5 μm and a first graphene material with a sheet size of 42 μm and 9 layers were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 20% of the mass percentage of the first mixed phase.

[0135] The first mixed phase was treated under a nitrogen atmosphere at 1000°C for 4 hours to obtain the second mixed phase;

[0136] The second mixed phase and a second graphene material with a sheet size of 49 μm and a number of layers of 6 were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 16% of the mass percentage of the third mixed phase;

[0137] The third mixed phase was heat-treated at 850°C for 9 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0138] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0139] The preparation methods for the negative electrode, low-temperature electrolyte, and positive electrode are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: dipropyl carbonate: methyl propyl carbonate = 2:3:5, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0140] The specific capacity of the negative electrode is 604mAh / g, and the efficiency in the first week is 87.2%.

[0141] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 93% at room temperature after 500 cycles and 88% at low temperature.

[0142] The present invention also provides some comparative examples for comparison with the above embodiments.

[0143] Comparative Example 1

[0144] Micron-sized silicon with a Dv50 of 3.8 μm and a first graphene material with a sheet size of 28 μm and a number of layers of 7 were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 18% of the mass percentage of the first mixed phase.

[0145] The first mixed phase was treated at 900°C under a nitrogen atmosphere for 4 hours to obtain the second mixed phase;

[0146] The second mixed phase and a second graphene material with a sheet size of 50 μm and a number of layers of 4 were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 20% of the mass percentage of the third mixed phase.

[0147] The third mixed phase was heat-treated at 850°C for 6 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0148] The negative electrode active material and graphite were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0149] The preparation methods for the negative electrode, electrolyte, and positive electrode are as described above. The electrolyte ratio is propylene carbonate: ethylene carbonate: fluoroethylene carbonate = 2:2:6, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0150] The specific capacity of the negative electrode is 603mAh / g, and the efficiency in the first week is 87.3%.

[0151] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 94% at room temperature after 500 cycles and 65% at low temperature.

[0152] Comparative Example 2

[0153] Micron-sized silicon with a Dv50 of 3.2 μm and a first graphene material with a sheet size of 29 μm and a number of layers of 3 were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 22% of the mass percentage of the first mixed phase.

[0154] The first mixed phase was treated at 650°C under a nitrogen atmosphere for 4 hours to obtain the second mixed phase;

[0155] The second mixed phase and a second graphene material with a sheet size of 57 μm and 8 layers were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 12% of the mass percentage of the third mixed phase;

[0156] The third mixed phase was heat-treated at 850°C for 6 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0157] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0158] The preparation methods for the negative electrode, electrolyte, and positive electrode are as described above. The electrolyte ratio is propylene carbonate: methyl propyl carbonate: diethyl carbonate = 2:2:6, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0159] The specific capacity of the negative electrode is 598mAh / g, and the efficiency in the first week is 86.4%.

[0160] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 75% at room temperature after 500 cycles and 64% at low temperature.

[0161] Comparative Example 3

[0162] Micron-sized silicon with a Dv50 of 3.2 μm and a first graphene material with a sheet size of 56 μm and 6 layers were mixed uniformly in a certain proportion to obtain a first mixed phase; wherein the first graphene material accounted for 22% of the mass percentage of the first mixed phase.

[0163] The first mixed phase was treated at 650°C under a nitrogen atmosphere for 4 hours to obtain the second mixed phase;

[0164] The second mixed phase and a second graphene material with a sheet size of 36 μm and a number of layers were mixed in a certain proportion and spray-dried to obtain a third mixed phase; wherein the second graphene material accounted for 12% of the mass percentage of the third mixed phase;

[0165] The third mixed phase was heat-treated at 850°C for 6 hours in a nitrogen atmosphere, and then demagnetized in stages to obtain the negative electrode active material.

[0166] The negative electrode active material and hard carbon were combined with a specific capacity of 600 mAh / g to obtain a negative electrode material composite.

[0167] The preparation methods for the negative electrode, electrolyte, and positive electrode are as described above. The electrolyte ratio is propylene carbonate: methyl propyl carbonate: diethyl carbonate = 2:2:6, with lithium salt accounting for 12.5%. The battery is then assembled according to the above method.

[0168] The specific capacity of the negative electrode is 599mAh / g, and the efficiency in the first week is 87.2%.

[0169] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 72% at room temperature after 500 cycles and 64% at low temperature.

[0170] Comparative Example 4

[0171] Pure hard carbon was used as the negative electrode active material. The preparation methods for the negative electrode sheet, low-temperature electrolyte, and positive electrode sheet are as described above. The ratio of the low-temperature electrolyte is propylene carbonate: methyl propyl carbonate: diethyl carbonate = 2:2:6, with lithium salt accounting for 12.5%. The battery was assembled according to the above method.

[0172] The specific capacity of the negative electrode is 449mAh / g, and the efficiency in the first week is 86.5%.

[0173] According to the test conditions of Example 1 above, a cyclic test was conducted, and the capacity retention rate was 92% at room temperature after 500 cycles and 88% at low temperature.

[0174] As can be seen from Examples 1-8, by designing a low-temperature electrolyte and combining it with a negative electrode material infiltrated with small-sized micron-sized silicon and bilayer graphene, the cycle performance of lithium-ion batteries is significantly improved. Comparative Example 1 shows that when using a conventional electrolyte, the room-temperature cycle performance is not weakened. This is because a graphite composite system is used, and graphite helps reduce expansion, thus improving cycle performance. However, the low-temperature cycle performance of Comparative Example 1 is very poor. This is because the solvent co-intercalation reaction rate is greater than the lithium-ion deintercalation rate at low temperatures, making it easy for solvent co-intercalation with graphite to occur, resulting in rapid cycle decay. Comparative Example 2 shows that the inner thin-layer and outer thick-layer graphene coating does not significantly improve the material's cycle performance. Comparative Example 3 shows that the outer layer uses small-sheet graphene coating, but the coating effect is not ideal; some exposed silicon is not completely coated, resulting in a relatively lower lifespan. Comparative Example 4 shows that although pure hard carbon has relatively ideal low-temperature and cycle performance, its specific capacity and energy density are low.

[0175] The electrochemical device proposed in this invention effectively mitigates the volume expansion of micron-sized silicon by employing a double-layer graphene coating; the use of a low-temperature electrolyte in conjunction with a graphite-free composite system effectively avoids the problem of solvent co-intercalation, ensuring cycle performance and effectively improving the low-temperature performance of the anode material. Simultaneously, using micron-sized silicon as the substrate significantly increases the battery's energy density and extends its battery life.

[0176] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An electrochemical device, characterized in that, The electrochemical device includes a negative electrode and a low-temperature electrolyte; The negative electrode sheet includes a negative electrode material layer; The negative electrode material layer includes a negative electrode material composite, which is a composite material of a negative electrode active material and hard carbon. The negative electrode active material is composed of micron-sized silicon and bilayer graphene material coated with micron-sized silicon. Specifically, a first graphene material forms a first mixed phase with micron-sized silicon; the first mixed phase is heat-treated to form a second mixed phase, which is then heat-treated to form a third mixed phase with a second graphene material. The third mixed phase is then heat-treated to form the negative electrode active material. The first graphene material accounts for 10%-30% of the mass percentage of the first mixed phase; the second graphene material accounts for 5%-20% of the mass percentage of the third mixed phase. The first graphene material has 2-10 layers, and the size of each layer is ≤45μm. The second graphene material has 1-9 layers, and the size of each layer is ≤65μm. The second graphene material has fewer layers than the first graphene material; the sheet size of the second graphene material is larger than the sheet size of the first graphene material. The Dv50 of the micron-sized silicon is 1μm≤Dv50≤5μm; The negative electrode material layer does not contain any of the following: artificial graphite, natural graphite, block graphite, flake graphite, or microcrystalline graphite. The cryogenic electrolyte includes a cryogenic solvent, which includes propylene carbonate (PC) and other cryogenic solvents; the mass ratio of propylene carbonate to the other cryogenic solvents is 2:8; the other cryogenic solvents include ethers and / or carbonate solvents; the ethers include one or more of diethylene glycol butyl ether, ethylene glycol dimethyl ether, dimethyl ether, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dimethoxymethane, and 1,2-dimethoxyethane; the carbonate solvents include one or more of diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, and ethyl propyl carbonate.

2. The electrochemical device according to claim 1, characterized in that, The negative electrode material layer also includes a dispersant and a binder.

3. The electrochemical device according to claim 1, characterized in that, The negative electrode material composite is obtained by combining the negative electrode active material and hard carbon with a specific capacity of 600 mAh / g.

4. An electronic device, characterized in that, The electronic device includes the electrochemical device according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Organic electrolyte with propylene carbonate as base solvent

    CN103022560A

  • Silicon-containing composite, preparing method thereof, and carbon composite, electrode, lithium battery and equipment each including the same

    CN109994717A

  • Method for manufacturing electrolyte for manufacturing ultralow-temperature lithium ion battery

    CN114156542A