An electrospun lithium-ion battery separator and its preparation method
Electrospun lithium-ion battery separators were prepared by mixing modified boron nitride and triphenyl phosphate with polyacrylonitrile using electrospinning technology. This solved the problems of insufficient heat resistance and electrolyte wettability of lithium-ion battery separators, and improved the safety and performance of the batteries.
Patent Information
- Application Number
- CN202311201450.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-18
AI Technical Summary
Existing lithium-ion battery separators have insufficient heat resistance and electrolyte wettability, which limits battery safety and performance, and the problem of lithium dendrite growth has not been effectively solved.
Modified boron nitride and triphenyl phosphate were mixed with polyacrylonitrile using electrospinning technology. After a three-step modification process, the mixture was mixed with PAN solution to prepare an electrospinned lithium-ion battery separator. This process enhanced the thermal stability and mechanical strength of the separator and inhibited the growth of lithium dendrites.
It improves the porosity and liquid absorption rate of the separator, enhances the thermal stability and safety performance of the battery, inhibits lithium dendrite growth, and improves the electrochemical performance and safety performance of the battery.
Smart Images

Figure CN117154337B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of new energy materials, specifically, it relates to an electrospun lithium-ion battery separator and its preparation method. Background Technology
[0002] Lithium-ion batteries (LIBs) consist of a positive electrode, a negative electrode, an electrolyte, and a separator. The separator is a key component affecting battery performance, serving not only as a storage medium for the electrolyte but also facilitating its migration to the electrodes. Generally, the porosity and pore size of the separator determine its electrolyte storage capacity; porosity and pore size must exceed 40% and 0.5 μm, respectively, to meet the basic standards for commercially available separators. Porosity is a crucial factor affecting separator performance; sufficient electrolyte permeation into the pores helps accelerate lithium-ion conduction, improves ionic conductivity, and mitigates electrode / electrolyte interface issues, thereby enhancing battery performance. Furthermore, the separator's porous structure, wettability, surface chemical properties, electrochemical stability window, thermal stability, and mechanical properties play a vital role in regulating ionic conductivity and lithium-ion migration.
[0003] The overall properties of the separator are closely related to the intrinsic properties of the polymer matrix. Currently, polyolefin separators (polypropylene and polyethylene) are widely used. However, these separators have low melting temperatures and poor thermal stability, making them prone to thermal shrinkage at high temperatures, which can lead to internal short circuits in the battery. Although the separator can be modified by coating it with heat-resistant materials, the inherent low thermal stability of the polypropylene and polyethylene matrices limits the improvement in the heat resistance of the modified separator. Therefore, it is necessary to develop high-temperature resistant polymer separators to improve battery safety.
[0004] In the existing technology, ordinary commercial separators have low melting points and poor wettability, resulting in excessive battery capacity loss. They also have low mechanical strength and are easily punctured by lithium dendrites, which can lead to battery short circuits or even explosions and fires.
[0005] Although the porous single-ion polymer electrolyte PI-FPAS membrane based on polyimide disclosed in patent document CN111081946A has good tensile strength and heat resistance, its membrane porosity is only 65-67% and its liquid absorption rate is only 265%-275%, which has limited effect on improving ionic conductivity.
[0006] Electrospun polyacrylonitrile (PAN) separators feature stacked nanofibers that create a porous three-dimensional structure, resulting in a high specific surface area and porosity. This not only enhances the separator's electrolyte storage capacity but also provides more channels for lithium ions to pass through. Furthermore, the cyano groups in the PAN molecules can interact with lithium ions, further improving the separator's liquid absorption rate. However, the heat resistance of existing PAN separators still has significant room for improvement. Summary of the Invention
[0007] Based on the above problems, the purpose of this invention is to provide an electrospun lithium-ion battery separator and its preparation method, so that the electrospun lithium-ion battery separator has electrolyte wettability and heat resistance far superior to commercial Celgard separators, and can maintain the high porosity of the original electrospun polyacrylonitrile (PAN) separator, thereby greatly improving the electrochemical performance and safety performance of lithium-ion batteries.
[0008] The technical solution to the technical problem in this invention is as follows:
[0009] In a first aspect, the present invention provides a method for preparing an electrospun lithium-ion battery separator. The method specifically comprises: mixing a modified material with a polyacrylonitrile (PAN) solution as a spinning solution, and preparing the lithium-ion battery separator by electrospinning. The PAN solution is wherein the solvent is N,N-dimethylformamide and the solute is PAN. The modified material refers to a material that has undergone three steps of modification treatment: ultrasonic dispersion treatment with tris(hydroxymethyl)aminomethane hydrochloride (Tris-HCl) buffer solution, dopamine surface coating, and silane coupling agent surface modification. In this invention, the modified material is boron nitride (BN) after the above-mentioned modification treatment (hereinafter referred to as modified boron nitride FBN). The weight ratio of the modified material to the polyacrylonitrile (PAN) raw material is (0.01–0.05):1.11, preferably (0.01–0.03):1.11.
[0010] Preferably, the electrospinning operation steps are as follows: after the spinning solution is magnetically stirred for 12 hours, it is drawn up with a disposable syringe using an 18-gauge needle, the voltage is set to 18KV, and electrospinning is performed under the conditions of a push speed of 0.15mm / min, a receiver distance of 20cm, and a stroke of 20mm to prepare the electrospinned lithium-ion battery separator.
[0011] Preferably, the silane coupling agent is aminopropyltriethoxysilane;
[0012] Preferably, the ultrasonic dispersion treatment of the Tris-HCl buffer solution of tris(hydroxymethyl)aminomethane hydrochloride specifically involves stirring the material to be modified in the buffer solution under ultrasonic conditions of 80-100 kHz for 1-3 hours to complete the ultrasonic exfoliation and dispersion of the material to be modified.
[0013] Preferably, the dopamine surface coating step specifically involves adding dopamine hydrochloride and performing a polymerization reaction for 5 to 10 hours; more preferably, the polymerization reaction temperature is room temperature (25°C) and the reaction time is 6 hours.
[0014] Preferably, the surface modification step of the silane coupling agent specifically involves adding aminopropyltriethoxysilane and carrying out a surface modification reaction at a temperature of 50–80°C for 5–10 hours to obtain the modified material; more preferably, the surface modification reaction is carried out at a temperature of 60°C for 6 hours.
[0015] Preferably, the mass-to-volume ratio of BN, dopamine hydrochloride, and aminopropyltriethoxysilane is 1–5 g: 1 g: 10 mL. Further, the mass-to-volume ratio of BN, dopamine hydrochloride, and aminopropyltriethoxysilane is 5 g: 1 g: 10 mL.
[0016] In a preferred embodiment of the method for preparing the electrospun lithium-ion battery separator of the present invention, the spinning solution is further mixed with modified triphenyl phosphate. The modified triphenyl phosphate (FTPP) is also a modified material obtained by the above three-step modification treatment, that is, the modified material is a mixture of modified boron nitride (FBN) and modified triphenyl phosphate (FTPP); and the weight ratio of modified boron nitride, modified triphenyl phosphate and polyacrylonitrile is (0.01~0.05) : 0.05 : 1.11, preferably (0.01~0.03) : 0.05 : 1.11.
[0017] As a preferred preparation method, the triphenyl phosphate and boron nitride can be simultaneously modified in the same reaction vessel to obtain a mixture of modified triphenyl phosphate and modified boron nitride, which is then mixed with the PAN solution as a spinning solution. The mass-volume ratio of the BN and TPP mixture, dopamine hydrochloride, and aminopropyltriethoxysilane is 1-5 g: 1 g: 10 mL. Preferably, the mass-volume ratio of the BN and TPP mixture, dopamine hydrochloride, and aminopropyltriethoxysilane is 5 g: 1 g: 10 mL.
[0018] Preferably, the Tris-HCl buffer solution has a pH of 8.5 and a concentration of 5 mM, and is used for ultrasonic stirring to disperse the material to be modified;
[0019] Preferably, after the modification reaction is completed, the product is centrifuged, washed successively with deionized water and ethanol, and dried at 80°C for 24 hours to obtain the modified product, wherein the modified product is FBN or FTPP or a mixture of both.
[0020] Secondly, the present invention provides an electrospun lithium-ion battery separator prepared by the above-described preparation method.
[0021] Thirdly, the present invention provides a lithium-ion battery, wherein the separator of the lithium-ion battery is the electrospun lithium-ion battery separator described above.
[0022] Invention Principle: This invention utilizes the disordered stacking of nanofibers in an electrospun PAN separator to form a separator with a thickness of approximately 30 nm. This separator possesses a porous three-dimensional structure and a high specific surface area, ensuring its high porosity. This not only enhances the separator's ability to store electrolyte but also provides more channels for lithium ions to shuttle through the separator. The cyano groups in the PAN molecule can interact with lithium ions in the electrolyte, increasing the separator's liquid absorption rate. Based on the inherently good porosity and liquid absorption rate of the electrospun PAN separator, this invention enhances the thermal stability and mechanical strength of the PAN separator by incorporating modified boron nitride into the spinning solution, without reducing or even increasing the PAN separator's porosity and liquid absorption rate.
[0023] In ceramic materials, boron nitride (BN) possesses excellent lubricity, mechanical properties, and thermal conductivity similar to graphite, but also exhibits superior insulation, chemical stability, and thermal stability. For example, its decomposition temperature in nitrogen reaches 2800℃, and its oxidation temperature exceeds 800℃. It also boasts advantages such as radiation resistance and good biocompatibility. Studies have found that adding 1 wt% BN can reduce the heat release of epoxy resin composites by nearly half, and adding 50 wt% BN can increase the thermal conductivity of epoxy resin composites by 40 times. Although BN is chemically stable, it lacks surface-active groups, resulting in poor interaction with polymer molecular chains and consequently poor dispersibility. This significantly reduces the modification effect of BN on materials. This patent uses dopamine to surface-encapsulate BN that has been pre-dispersed by ultrasonic exfoliation, obtaining BN rich in surface functional groups. Subsequently, surface modification is performed using a silane coupling agent such as aminopropyltriethoxysilane to obtain modified boron nitride (FBN). After modification with dopamine, a polydopamine coating layer is formed on the surface of the BN. Boron nitride (FBN) modified with aminopropyltriethoxysilane has abundant surface functional groups and good electrolyte affinity; the modified boron nitride has higher matrix compatibility and can form a continuous physical reinforcement network, thereby effectively improving the mechanical strength of the membrane.
[0024] Triphenyl phosphate (TPP) is a phosphorus-rich flame retardant. Therefore, as a preferred embodiment of the electrospun lithium-ion battery separator of the present invention, in addition to incorporating the aforementioned FBN, FTPP, which is also sequentially modified with Tris-HCl buffer solution, dopamine hydrochloride, and aminopropyltriethoxysilane, can be incorporated into the PAN. That is, the PAN separator is modified simultaneously using modified boron nitride FBN and modified triphenyl phosphate FTPP, thereby further improving the flame retardant performance of the electrospun lithium-ion battery separator.
[0025] The thermal runaway behavior of lithium-ion batteries assembled using this separator is significantly delayed, resulting in higher safety performance.
[0026] The present invention has the following technical effects:
[0027] The electrospun lithium-ion battery separator provided by this invention is prepared by sequentially modifying boron nuclei (BN) with Tris-HCl buffer solution, dopamine hydrochloride, and aminopropyltriethoxysilane to obtain fumed silica (FBN), and then incorporating FBN into poly(PAN) via electrospinning. This separator exhibits high porosity, high liquid absorption rate, good thermal stability, fire resistance, and electrolyte wettability.
[0028] Compared to the electrospun separator provided in patent document CN107834006A, the modified PAN separator provided in this invention exhibits better heat resistance and thermal stability. Although the PI-FPAS separator provided in patent document CN111081946A can also improve the thermal stability of lithium-ion batteries to some extent, it does not address the lithium dendrite growth problem that occurs during battery cycling. This invention, however, modifies the separator using FBN or an FBN / FTPP mixture, giving the separator a certain mechanical strength that can suppress lithium dendrite growth. Furthermore, the electrospun separator provided in this invention has higher porosity and liquid absorption rate compared to the PI-FPAS separator provided in patent document CN111081946A. After testing, the porosities of the separators prepared in Examples 1 to 6 of this invention were 239.7%, 317.3%, 375.8%, 226.4%, 266.6%, and 346.3%, respectively, which are much higher than the porosity of commercial separators (74.6%), and also much higher than the 79% to 84% porosity of the invention with publication number CN107834006A and the 65% to 67% porosity of the invention with publication number CN111081946A. Under the same battery system and current density, the modified PAN-based separator of this invention gives the battery a higher capacity. Attached Figure Description
[0029] Figure 1a The image shows a scanning electron microscope (SEM) image of the PAN diaphragm prepared in Comparative Example 1.
[0030] Figure 1b This is a scanning electron microscope image of the PAN@FBN-1 membrane prepared in Example 1;
[0031] Figure 1c This is a scanning electron microscope image of the PAN@FBN / FTPP-1 membrane prepared in Example 4;
[0032] Figure 2a A comparison chart of the porosity of the Celgard membrane, Comparative Example 1, and the membranes prepared in Examples 1 to 6;
[0033] Figure 2b Comparison graph of electrolyte uptake for Celgard diaphragm, Comparative Example 1, and diaphragm electrolytes prepared in Examples 1 to 6;
[0034] Figure 3 Physical images of the Celgard diaphragm, Comparative Example 1, and the diaphragms prepared in Examples 1 to 6 after heat treatment at different temperature conditions;
[0035] Figure 4a This is a comparison chart of the TGA curves of the membrane prepared in Example 1, the Celgard membrane, and the PAN membrane under nitrogen.
[0036] Figure 4b This is a comparison chart of the TGA curves of the membrane prepared in Example 2, the Celgard membrane, and the PAN membrane under nitrogen.
[0037] Figure 4c This is a comparison chart of the TGA curves of the membrane prepared in Example 3, the Celgard membrane, and the PAN membrane under nitrogen.
[0038] Figure 4d This is a comparison chart of the TGA curves of the membrane prepared in Example 4, the Celgard membrane, and the PAN membrane under nitrogen.
[0039] Figure 4e This is a comparison chart of the TGA curves of the membrane prepared in Example 5, the Celgard membrane, and the PAN membrane under nitrogen.
[0040] Figure 4f This is a comparison chart of the TGA curves of the membrane prepared in Example 6, the Celgard membrane, and the PAN membrane under nitrogen.
[0041] Figure 5a This is a comparison chart of the DTG curves of the membrane prepared in Example 1, the Celgard membrane, and the PAN membrane under nitrogen.
[0042] Figure 5bThis is a comparison chart of the DTG curves of the membrane prepared in Example 2, the Celgard membrane, and the PAN membrane under nitrogen.
[0043] Figure 5c This is a comparison chart of the DTG curves of the membrane prepared in Example 3, the Celgard membrane, and the PAN membrane under nitrogen.
[0044] Figure 5d This is a comparison chart of the DTG curves of the membrane prepared in Example 4, the Celgard membrane, and the PAN membrane under nitrogen.
[0045] Figure 5e This is a comparison chart of the DTG curves of the membrane prepared in Example 5, the Celgard membrane, and the PAN membrane under nitrogen.
[0046] Figure 5f This is a comparison chart of the DTG curves of the membrane prepared in Example 6, the Celgard membrane, and the PAN membrane under nitrogen.
[0047] Figure 6a The cycle performance curves of batteries assembled with the separators prepared in Examples 1 to 3 and Celgard separators and PAN separators are shown.
[0048] Figure 6b The cycle performance curves of batteries assembled with the separators prepared in Examples 4 to 6 and Celgard separators and PAN separators are shown.
[0049] Figure 7 The figures show the ARC test results of batteries assembled with Celgard separator, PAN separator, PAN@FBN-3 separator and PAN@FBN / FTPP-3 separator, where (a) is the temperature change curve and (b) is the heating rate curve.
[0050] Figure 8a These are comparison curves of Li-to-Li cycle tests on batteries equipped with Celgard separators and PAN@FBN-1 separators; Figure 8b This is a comparison curve of Li-to-Li cycle tests for batteries equipped with Celgard separators and PAN@FBN / FTPP-1 separators. Detailed Implementation
[0051] To further illustrate the technical solution of the present invention, preferred embodiments are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, and not for limiting the scope of the claims. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of the present invention. Furthermore, unless otherwise specified, the raw materials or reagents mentioned below are commercially available products, and the process steps or methods not mentioned in detail are process steps or methods known to those skilled in the art.
[0052] The sources of some of the raw materials and reagents used in the following examples, comparative examples, and test cases are shown below:
[0053] Polyacrylonitrile (PAN) AR, 99wt% Bid Medical Technology Boron nitride (BN) AR, 98.5 wt% McLean Biotech Triphenyl phosphate (TPP) AR, 98wt% Aladdin Biochemical Technology Tris-HCl (Tris-HCl) AR, 99wt% McLean Biotech Dopamine hydrochloride AR, 98wt% McLean Biotech Aminopropyltriethoxysilane (APTES) AR, 98wt% McLean Biotech
[0054] Example 1: FBN-modified PAN separator PAN@FBN-1
[0055] The fabrication of a novel lithium-ion battery separator includes the following steps:
[0056] (1) Preparation of modified boron nitride (FBN): 1 g of BN was dispersed in 200 mL of Tris-HCl buffer solution (pH = 8.5, 5 mM) and ultrasonically stirred for 2 hours. Then, 0.2 g of dopamine hydrochloride was added, and ultrasonic stirring was continued for 6 hours. After polymerization was completed, 2 mL of aminopropyltriethoxysilane was first dissolved in 20 mL of water, and then slowly added dropwise to the above mixture. The reaction was carried out at 60 °C for 6 hours. After the reaction was completed, the mixture was centrifuged and washed with deionized water and ethanol, respectively, to obtain FBN. The product was dried at 80 °C for 24 hours.
[0057] (2) Preparation of modified PAN membrane: 1.11g of PAN and 0.01g of FBN were added to 10g of N,N-dimethylformamide solvent and magnetically stirred for 12 hours to prepare spinning solution. An appropriate amount of spinning solution was drawn with a disposable syringe and spun using an 18-gauge needle at a voltage of 18KV, a pushing speed of 0.15mm / min, a needle distance of 20cm from the receiver, and a stroke of 20mm.
[0058] Example 2: FBN-modified PAN separator PAN@FBN-2
[0059] The only difference between Example 2 and Example 1 is that in the preparation of the modified PAN membrane, 1.11g of PAN and 0.02g of FBN are added to 10g of N,N-dimethylformamide solvent; the other steps are the same.
[0060] Example 3: FBN-modified PAN separator PAN@FBN-3
[0061] The only difference between Example 3 and Example 1 is that in the preparation step of the modified PAN membrane, 1.11g of PAN and 0.03g of FBN are added to 10g of N,N-dimethylformamide solvent; the other steps are the same.
[0062] Example 4: FBN / FTPP modified PAN separator PAN@FBN / FTPP-1
[0063] (1) Preparation of a mixture of modified boron nitride and modified triphenyl phosphate (FBN / FTPP)
[0064] A mixture of BN and TPP with a mass ratio of 1:5 and a total mass of 1 g was dispersed in 200 mL of Tris-HCl buffer solution (pH = 8.5, 5 mM) and ultrasonically stirred for 2 hours. Then, 0.2 g of dopamine hydrochloride was added, and ultrasonic stirring continued for 6 hours. After polymerization was complete, 2 mL of aminopropyltriethoxysilane was dissolved in 20 mL of water and then slowly added dropwise to the above mixture. The reaction was carried out at 60 °C for 6 hours. After the reaction was completed, the mixture was centrifuged and washed with deionized water and ethanol, respectively, to obtain an FBN / FTPP mixture. The product was dried at 80 °C for 24 hours.
[0065] (2) Preparation of FBN / FTPP modified PAN membrane
[0066] A spinning solution was prepared by adding 1.11 g of PAN and 0.06 g of FBN / FTPP mixture to 10 g of N,N-dimethylformamide solvent and stirring magnetically for 12 hours. An appropriate amount of the spinning solution was drawn up using a disposable syringe with an 18-gauge needle. Spinning was performed under the following conditions: voltage of 18 kV, push speed of 0.15 mm / min, needle distance from receiver of 20 cm, and stroke of 20 mm.
[0067] Example 5: FBN / FTPP modified PAN separator PAN@FBN / FTPP-2
[0068] The only difference between Example 5 and Example 4 is that the raw material ratio of BN and TPP in step (1) is 2:5, and the raw material amount of the FBN / FTPP mixture in step (2) is 0.07g.
[0069] Example 6: FBN / FTPP modified PAN separator PAN@FBN / FTPP-3
[0070] The only difference between Example 6 and Example 4 is that the raw material ratio of BN and TPP in step (1) is 3:5, and the raw material amount of the FBN / FTPP mixture in step (2) is 0.08g.
[0071] Comparative Example 1: Unmodified PAN separator
[0072] Add 1.11g of PAN to 10g of N,N-dimethylformamide solvent and stir magnetically for 12 hours to prepare a spinning solution. Use a disposable syringe to draw an appropriate amount of spinning solution and spin the yarn using an 18-gauge needle at a voltage of 18KV, a pushing speed of 0.15mm / min, a needle distance of 20cm from the receiver, and a stroke of 20mm.
[0073] Table 1 shows the raw material ratios of the spinning solutions in the comparative examples and embodiments above.
[0074] Group Diaphragm components PAN(g) FBN(g) FTPP(g) Comparative Example 1 PAN 1.11 0 0 Example 1 PAN@FBN-1 1.11 0.01 0 Example 2 PAN@FBN-2 1.11 0.02 0 Example 3 PAN@FBN-3 1.11 0.03 0 Example 4 PAN@FBN / FTPP-1 1.11 0.01 0.05 Example 5 PAN@FBN / FTPP-2 1.11 0.02 0.05 Example 6 PAN@FBN / FTPP-3 1.11 0.03 0.05
[0075] Test Example 1: Microscopic Morphology Observation of the Diaphragm
[0076] To observe the microstructure of different modified PAN membranes, SEM scanning was performed on the composite membranes. Figure 1a The image shows the morphology of the PAN membrane before modification, exhibiting a distinct fibrous structure with uniform thickness and distribution. The fibers are slightly curved, randomly arranged, and crisscrossed. Figure 1b The morphology of the PAN@FBN-1 diaphragm is shown. Figure 1c The morphology of the PAN@FBN / FTPP-1 separator is shown. It can be seen that the addition of FBN and FTPP does not significantly change the morphology of the PAN separator.
[0077] The morphological photographs of the diaphragm disclosed in publications CN107834006A and CN111081946A, and the present invention... Figure 1b The electrospun separator PAN@FBN-1 prepared in Example 1 is shown. Figure 1c Comparing the electrospun diaphragm PAN@FBN / FTPP-1 prepared in Example 4, it is easy to see that the spun diaphragm of the present invention has a higher porosity.
[0078] Test Example 2: Diaphragm Porosity Test
[0079] The membrane porosity P is obtained by gravimetric method by measuring the weight difference between the dry membrane and the sealed n-butanol in the membrane pores, and then the membrane porosity is calculated according to the following formula.
[0080]
[0081] w d It is the dry weight of the membrane, w w It is the wet weight of the membrane, ρ b The density and V of n-butanol m Let be the volume of the membrane.
[0082] The porosity of PAN, PAN@FBN-1, PAN@FBN-2, PAN@FBN-3, PAN@FBN / FTPP-1, PAN@FBN / FTPP-2, and PAN@FBN / FTPP-3 membranes was tested. Figure 2a The calculated porosities of the membranes are 224.7%, 239.7%, 317.3%, 375.8%, 226.4%, 266.6%, and 346.3%, respectively. Compared with the Celgard membrane, which has a porosity of only 74.6%, the porosity of the modified PAN membranes has been significantly improved.
[0083] Test Example 3: Diaphragm Electrolyte Absorption Rate Test
[0084] The liquid absorption rate of the diaphragm is mainly used to characterize the diaphragm's ability to store electrolyte. The liquid absorption rate of the diaphragm is tested as follows: Celgard diaphragm, PAN diaphragm, and diaphragms prepared in Examples 1 to 6 are respectively made into 17 mm diameter discs. The weight of the diaphragm before the test is recorded. Then, the diaphragm is immersed in a beaker containing electrolyte solution. After 1 hour, it is taken out, and excess electrolyte on the surface is wiped off with filter paper. The weight after immersion is recorded. The electrolyte used is an organic electrolyte solution of ethylene carbonate (EC) and diethyl carbonate (DEC) in a 1:1 ratio plus 1.0 M LiPF6.
[0085] The liquid absorption rate is calculated using formula 2-2:
[0086]
[0087] Where M is the liquid absorption rate (%) of the tested diaphragm, M1 is the mass of the tested diaphragm before wetting, in g; and M2 is the mass of the tested diaphragm after wetting, in g.
[0088] like Figure 2b As shown, the electrolyte absorption rate of the Celgard membrane was 98.0%. In contrast, the absorption rates of the modified PAN membranes prepared in Examples 1 to 6 were significantly improved. The absorption rates of PAN and PAN-modified membranes reached 664.7%, 688.5%, 700.0%, 715.8%, 852.0%, 895.0%, and 916.8%, respectively, which were much higher than those of the Celgard membrane. This is attributed to the fibrous porous structure of the PAN membrane. The addition of FBN further improved the absorption rate of the membrane.
[0089] Test Example 4: Thermal Stability Test of the Diaphragm
[0090] The safety performance of the separator at high temperatures directly affects the safety of the battery. Next, we will characterize the separator's safety by examining its thermal stability and flame retardant properties. First, we will test the separator's thermal stability through heat shrinkage and thermogravimetric analysis (TGA) experiments. The heat shrinkage experiment characterizes the separator's dimensional stability; the separator is heat-treated at 100, 120, 140, 160, 180, and 200°C for 30 minutes, and the dimensional changes are recorded. From... Figure 3 It can be seen that the Celgard separator began to deform severely at only 140℃ and could no longer be used normally, indicating that batteries using the Celgard separator would experience internal short circuits before reaching 140℃. The PAN-modified separator, however, maintained a better morphology and remained unchanged. At 160℃, the Celgard separator underwent pyrolysis and became transparent. At temperatures of 100, 120, 140, 160, and 180℃, the PAN-modified separator did not exhibit thermal shrinkage. Only at 200℃ did it begin to change from white to yellow, showing only slight thermal shrinkage, mainly due to the oxidation of the nitrile groups in PAN at high temperatures. In summary, the PAN-modified separator did not experience thermal shrinkage before 180℃, demonstrating significantly higher heat resistance than the Celgard separator.
[0091] Next, the diaphragm was subjected to TGA testing, such as... Figure 4a , Figure 4b , Figure 4c , Figure 4d , Figure 4e and Figure 4f The figures shown are TGA curves of the membranes prepared in Examples 1 to 6, the Celgard membrane, and the PAN membrane under nitrogen atmosphere. When the test temperature reaches 800℃, the solid residue of the Celgard membrane is only 0.26wt%, while the solid residue of the PAN, PAN@FBN-1, PAN@FBN-2, PAN@FBN-3, PAN@FBN / FTPP-1, PAN@FBN / FTPP-2, and PAN@FBN / FTPP-3 membranes are significantly increased to 39.25wt%, 40.85wt%, 40.28wt%, 43.71wt%, 40.59wt%, 40.29wt%, and 39.56wt%, respectively, which are much higher than the residue of the Celgard membrane.
[0092] like Figure 5a , Figure 5b , Figure 5c , Figure 5d , Figure 5e and Figure 5fThe figures show a comparison of the micro-quotient thermogravimetric analysis (DTG) curves of the membranes prepared in Examples 1-6, the Celgard membrane, and the PAN membrane under nitrogen atmosphere. The maximum mass loss rate of the Celgard membrane was 3.078% / ℃. The maximum mass loss rates of the PAN membrane and its modified membranes (i.e., the membranes prepared in Examples 1-6) all decreased significantly, to 1.088% / ℃, 1.070% / ℃, 1.123% / ℃, 0.697% / ℃, 0.804% / ℃, 0.931% / ℃, and 1.056% / ℃, respectively. These results indicate that the PAN-modified membrane has higher thermal stability.
[0093] Test Example 6: Battery Capacity Retention Rate
[0094] The separators prepared in Examples 1 to 6 were cut to sizes suitable for assembling button batteries. The button batteries were then assembled in a glove box for performance testing. Specifically, the cut separators were moved to the glove box for assembly. The positive electrode was LiFePO4, the negative electrode was a lithium sheet, and the electrolyte was 1M LiPF6 and EMC / EC (v / v = 1 / 1). The assembly sequence was: negative electrode casing - lithium sheet - separator - 80μL electrolyte - positive electrode plate - stainless steel gasket - spring sheet - positive electrode casing. Finally, the battery was placed in a packaging machine and subjected to a pressure of 5MPa for 5 seconds to complete the battery assembly.
[0095] In the prior art patent CN111081946A, the cycle test results of a lithium-ion battery equipped with a PI-FPAS separator were shown, and its capacity was far lower than that of a lithium-ion battery equipped with the separator of the present invention.
[0096] After equipping with lithium batteries, such as Figure 6a The figure shows a comparison of the cycle performance curves of batteries assembled with Celgard separator, PAN separator, and modified PAN@FBN-1, PAN@FBN-2, and PAN@FBN-3.
[0097] Figure 6b A comparison of cycle performance curves for batteries assembled with Celgard separators, PAN separators, and modified PAN@FBN / FTPP-1, PAN@FBN / FTPP-2, and PAN@FBN / FTPP-3; from Figure 6a and Figure 6bIt can be seen that the first-cycle discharge specific capacities of the Celgard separator, PAN separator, and the modified PAN@FBN-1, PAN@FBN-2, PAN@FBN-3, PAN@FBN / FTPP-1, PAN@FBN / FTPP-2, and PAN@FBN / FTPP-3 batteries are 158.9, 155.0, 158.4, 156.5, 154.2, 159.2, 155.7, and 157.1 mAh g, respectively. -1 After 0.1C cycle activation, increasing the current density to 1C resulted in a significant decrease in the discharge specific capacity of all batteries. The Celgard battery exhibited a clear downward trend in discharge specific capacity, stabilizing only after 30 cycles and then beginning a significant capacity decline again after 80 cycles. In contrast, the battery equipped with the modified separator maintained a stable cycling trend throughout. For the Celgard battery, its discharge specific capacity at cycles 6, 10, 30, 50, and 100 were 134.2, 123, 105.3, 102.7, and 82.4 mAh g, respectively. -1 The PAN@FBN-1 battery's discharge specific capacities at 6, 10, 30, 50, and 100 cycles were 138.2, 133.8, 122.2, 124, and 114.5 mAh g, respectively. -1 The PAN@FBN / FTPP-1 battery exhibited specific capacities of 134.7, 129.4, 116.1, 117.7, and 112.8 mAh g at 6, 10, 30, 50, and 100 discharge cycles, respectively. -1 Comparing the discharge specific capacity at 6th and 100th cycles, it can be found that the discharge specific capacity of the Celgard battery decreased by 38.6%, while the discharge specific capacity of the PAN@FBN-1 and PAN@FBN / FTPP-1 batteries decreased by only 17.1% and 16.8%, respectively. The above analysis shows that the battery equipped with the PAN modified separator has a higher capacity retention rate.
[0098] Test Example 7: ARC Test with Battery
[0099] Adiabatic Accelerated Calorimetry (ES-ARC) was used to perform ARC tests on batteries with different separators. During the test, ES-ARC operated in a "heat-wait-search" mode, gradually increasing the battery temperature. Heating was stopped when the battery exhibited self-heating and the temperature rise rate exceeded 0.02℃ / min. The temperature characteristic points of the button cell include: T S —Self-exothermic onset temperature; T r —The temperature at which the heating rate exceeds 1℃ / min is the thermal runaway initiation temperature; T M —The highest temperature at which thermal runaway occurs, i.e. the highest temperature that can be reached during the thermal runaway reaction.
[0100] Figure 7 These are the results of the battery ARC test. It is clearly visible that when a PAN battery experiences thermal runaway, the temperature curve tends to rise vertically, and the highest temperature T... M The maximum thermal runaway temperature reached 387.8℃. In contrast, the batteries assembled with modified separators PAN@FBN-3 and PAN@FBN / FTPP-3 exhibited significantly higher safety, with maximum thermal runaway temperatures of 262.6℃ and 299.9℃, respectively, representing a decrease of 32.3% and 22.7% compared to the maximum temperature of the PAN battery. The temperature rise rate curves also show that the maximum temperature rise rate of the unmodified PAN battery reached 9.7℃ / min, while the maximum temperature rise rates of the PAN@FBN-3 and PAN@FBN / FTPP-3 batteries decreased to 3.6 and 1.8℃ / min, respectively. During the entire test, the adiabatic temperature rise of the batteries was 267.7℃, 151.4℃, and 184.1℃, respectively. Using PAN@FBN-3 and PAN@FBN / FTPP-3 separators reduced the adiabatic temperature rise of the batteries by 43.2% and 31.2%, respectively. From the perspective of the overall temperature rise rate of battery thermal runaway, the PAN battery with added FBN and FTPP has the lowest temperature rise rate, indicating that the PAN@FBN / FTPP-3 separator significantly reduces the harm of battery thermal runaway. This is because TPP has flame retardancy and can release phosphorus-containing free radicals when a chain reaction occurs inside the battery, inhibiting the internal thermal runaway chain reaction and reducing the temperature rise rate of the battery.
[0101] Test Example 8: Test for Suppressing Lithium Dendrites
[0102] The growth of lithium dendrites in lithium-ion batteries is one of the main causes of internal short circuits. The growth of lithium dendrites inside the battery punctures the separator, causing the positive and negative electrodes to connect and resulting in a short circuit. Lithium dendrites form because during charging and discharging, lithium ions shuttle back and forth, continuously depositing lithium on the surface of the negative electrode. With increasing cycle count, lithium dendrites continue to grow, leading to a decrease in battery capacity. Eventually, the continuous growth of lithium dendrites will puncture the separator, triggering an internal short circuit and even thermal runaway. Therefore, suppressing lithium dendrite growth is a necessary measure to improve battery safety performance.
[0103] Commercial Celgard separators, the PAN@FBN-3 separator prepared in Example 3, and the PAN@FBN / FTPP-3 separator prepared in Example 6 were cut to sizes suitable for assembling button cells. The separators were then assembled into Li-to-Li button cells in a glove box, and the cells were initially heated to 0.05 mA / cm². -2 Under the condition of 0.05mAh, it undergoes 5 charge-discharge cycles, and then at a current density of 1mAcm. -2 The lithium-ion symmetric battery was cycled at a charge-discharge capacity of 1 mAh to test the separator's ability to suppress lithium dendrite growth. Cycling data for the lithium-ion symmetric battery are as follows: Figure 8a and Figure 8b As shown, batteries equipped with PAN@FBN-3 and PAN@FBN / FTPP-3 separators have a capacity of 1mAh cm⁻¹. -2 Under ideal cycling conditions, the PAN@FBN-3 separator maintained a stable voltage plateau after 1000 hours of operation, while the ordinary Celgard separator showed voltage instability starting from the 300th hour, and completely lost stability by the 500th hour. This indicates that batteries equipped with Celgard separators exhibit more severe lithium dendrite growth, significantly reducing battery safety. The stable voltage plateau of batteries using PAN@FBN-3 and PAN@FBN / FTPP-3 separators during long-term cycling demonstrates that these two separators possess excellent capabilities in suppressing lithium dendrite growth.
[0104] The above are merely embodiments of the present invention and do not limit the scope of the patent. Any equivalent modifications made based on the content of this specification, or direct or indirect applications in other related technical fields, are similarly included within the scope of patent protection of the present invention.
Claims
1. A method for preparing an electrospun lithium-ion battery separator, characterized in that, The specific preparation method is as follows: the modified material is mixed with a polyacrylonitrile solution as a spinning solution, and the lithium-ion battery separator is prepared by electrospinning. The weight ratio of the modified material to the polyacrylonitrile raw material is (0.01~0.05):1.
11. The solvent of the polyacrylonitrile solution is N,N-dimethylformamide. The modified material is boron nitride that has undergone three steps of modification treatment: ultrasonic dispersion treatment with tris-HCl buffer solution, dopamine surface coating, and silane coupling agent surface modification. The ultrasonic dispersion treatment of the tris-HCl buffer solution of tris(hydroxymethyl)aminomethane hydrochloride specifically involves stirring the material to be modified in the buffer solution under ultrasonic conditions of 80-100 kHz for 1-3 hours to complete the ultrasonic exfoliation and dispersion of the material to be modified; the dopamine surface coating step specifically involves adding dopamine hydrochloride and carrying out a polymerization reaction for 5-10 hours; the silane coupling agent surface modification step specifically involves adding aminopropyltriethoxysilane and carrying out a surface modification reaction at a temperature of 50-80℃ for 5-10 hours to obtain the modified material; The spinning solution also contains modified triphenyl phosphate, which is also a modified material obtained by a three-step modification process, and the weight ratio of modified boron nitride, modified triphenyl phosphate and polyacrylonitrile is (0.01~0.05):0.05:1.
11. The triphenyl phosphate and boron nitride are simultaneously modified in the same reaction vessel to prepare a mixture of modified triphenyl phosphate and modified boron nitride, which is then mixed with the polyacrylonitrile solution as a spinning solution. The mass-volume ratio of the mixture of boron nitride and triphenyl phosphate, dopamine hydrochloride and aminopropyltriethoxysilane is (1~5g):1g:10mL.
2. The method for preparing an electrospun lithium-ion battery separator according to claim 1, characterized in that, The specific steps of the electrospinning include: magnetically stirring the spinning solution for 12 hours, then drawing it up with a disposable syringe using an 18-gauge needle, setting the voltage to 18 kV, and performing electrospinning under the conditions of a push speed of 0.15 mm / min, a receiver distance of 20 cm, and a stroke of 20 mm to prepare the electrospinned lithium-ion battery separator.
3. The method for preparing an electrospun lithium-ion battery separator according to claim 1, characterized in that, The mass-to-volume ratio of boron nitride, dopamine hydrochloride, and aminopropyltriethoxysilane is (1~5) g: 1 g: 10 mL.
4. The method for preparing an electrospun lithium-ion battery separator according to claim 1, characterized in that, The Tris-HCl buffer solution has a pH of 8.5 and a concentration of 5 mM.
5. An electrospun lithium-ion battery separator prepared by the preparation method according to any one of claims 1 to 4.
6. A lithium-ion battery, wherein the separator of the lithium-ion battery is the electrospun lithium-ion battery separator as described in claim 5.
Citation Information
Patent Citations
PI / PVDF-HFP / PI nano-fiber composite lithium ion battery diaphragm and preparation method thereof
CN107834006A
Polyimide-based porous single-ion polymer electrolyte PI-FPAS diaphragm as well as preparation method and application thereof
CN111081946A
Method for preparing heat-conducting film with three-dimensional structure by electrostatic spinning-hot pressing method and application of heat-conducting film
CN116427102A