A three-dimensional egg yolk shell structure V2O3 electrode material, its preparation method and application
A three-dimensional eggshell-shell structured V2O3 electrode material was prepared by a high-temperature mixed solvothermal method, which solved the problem of volume change of V2O3 anode material during charge and discharge, and achieved high capacity and long cycle stability, making it suitable for lithium-ion battery anode materials.
Patent Information
- Application Number
- CN202311356621.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-19
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-10-19
AI Technical Summary
Existing V2O3 anode materials exhibit large volume changes during charge and discharge, leading to structural instability and poor retention of active material density and capacity, making it difficult to meet the energy density requirements of lithium-ion batteries.
A three-dimensional egg yolk shell structure V2O3 electrode material was prepared by a high-temperature mixed solvothermal method. V2O5 and glucose were reacted in a specially designed double-chamber reactor to form a three-dimensional egg yolk shell structure with a core layer, cavity, and shell layer. Combined with annealing under a nitrogen atmosphere, a micron-sized material composed of V2O3 nanoparticles was formed.
This improved the structural stability and tap density of the material, enhanced electrolyte penetration and lithium-ion diffusion, improved electrochemical performance, and achieved high capacity and long-cycle stability.
Smart Images

Figure CN117374246B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a three-dimensional eggshell-structured V2O3 electrode material, its preparation method, and its application, belonging to the field of energy storage materials technology. Background Technology
[0002] Rechargeable lithium-ion batteries, with their high energy density, high power density, long cycle life, and good safety performance, have become key components in portable electronic devices, electric vehicles, and large-scale energy storage. Electrode materials are crucial in determining the energy density and cost of lithium-ion batteries. Currently, commercially available lithium-ion battery cathode materials mainly include LiCoO2 and LiFePO4, but their theoretical specific capacities are relatively low (100–160 mAh / g). Anode materials are primarily graphite, with a theoretical specific capacity of 372 mAh / g, which cannot meet the future energy density requirements of lithium-ion batteries in energy storage technology. Vanadium oxides (VO2, V2O5, V3O7·H2O, V6O) are also important considerations. 13 V₂O₃ (V₂O₃) is a promising electrode material for lithium-ion batteries due to its diverse valence states, layered structure facilitating ion insertion / extraction, abundant natural reserves, and environmental friendliness. V₂O₃, in particular, possesses a rich channel structure formed by the stacking of VO layers, and V₃⁻ electrons can exchange along the V₃V chain. Therefore, V₂O₃ exhibits a high theoretical specific capacity (356 mAh / g) and good conductivity, making it an ideal anode material for lithium-ion batteries. Xie et al. synthesized V₂O₃ nanorods using a solvothermal method at 220℃ for 48 hours. Huang et al. first synthesized V₃O₇·H₂O@C and VO₂(B)@C wear-resistant tapes using a hydrothermal method, and then obtained V₂O₃@C nanoribbons through annealing. Similar to V₂O₅, one-dimensional V₂O₃ materials exhibit poor capacity retention. Fu et al. synthesized a 3D core-shell structured hollow V₂O₃ microsphere using a template-free polyol solvothermal method, alleviating the capacity retention problem. However, the hollow structure reduces the density of the active material, resulting in a decrease in volumetric capacity, which is also detrimental to industrial applications. Therefore, achieving a balance between improving capacity stability and maintaining a high density of active material (energy density) has become an important direction in the research of V₂O₃ anode materials. Summary of the Invention
[0003] Objectives of the Invention: The first objective of this invention is to provide a three-dimensional egg yolk shell structure V2O3 electrode material that buffers the volume expansion during charge and discharge; the second objective of this invention is to provide a method for preparing the three-dimensional egg yolk shell structure V2O3 electrode material; and the third objective of this invention is to provide the application of the three-dimensional egg yolk shell structure V2O3 electrode material as a negative electrode material in lithium-ion batteries.
[0004] Technical solution: The present invention provides a three-dimensional egg yolk shell structure V2O3 electrode material, wherein the V2O3 electrode material is a spherical particle with a three-dimensional egg yolk shell structure composed of a core layer, a cavity, and a shell layer, wherein both the shell layer and the core layer are V2O3 nanoparticles, and there is a certain space (i.e., cavity) between the shell layer and the core layer.
[0005] Furthermore, the diameter of the spherical particles is 1–2 μm.
[0006] The present invention describes a method for preparing a three-dimensional egg yolk shell structure V2O3 electrode material, comprising the following steps:
[0007] (1) Add V2O5 to anhydrous ethanol and stir until homogeneous to obtain solution A. Add glucose to anhydrous ethanol and stir until homogeneous to obtain solution B.
[0008] (2) First, heat liquid A and liquid B separately, then mix liquid A and liquid B, heat to react, cool to room temperature, wash the product, dry it, and obtain precursor powder;
[0009] (4) The precursor powder was annealed under a nitrogen atmosphere to obtain a three-dimensional egg yolk shell structure V2O3 electrode material.
[0010] Further, in step (2), the molar ratio of glucose to V2O5 is 0.2 to 0.6:1.
[0011] Furthermore, in step (2), heating liquid A and liquid B separately involves placing liquid A and liquid B in the two chambers of a double-chamber reactor with a tetrafluoroethylene liner to ensure that liquid A and liquid B do not come into contact before reaching the reaction temperature. Once the reaction temperature is reached, the reactor is rotated to allow liquid A and liquid B in the two chambers to come into contact and mix, and the reaction temperature is maintained to continue the reaction.
[0012] Further, in step (2), the mixture is heated separately to the reaction temperature, which is 180℃~240℃, and the heating time is 1~6h.
[0013] Furthermore, in step (2), the drying temperature is 60℃~80℃ and the drying time is 12~24h.
[0014] Furthermore, in step (3), the annealing temperature is 500-700℃, the heating rate is 5-10℃ / min, and the annealing interval is 1-2h.
[0015] Furthermore, in step (3), the precursor is a spherical eggshell structure composed of vanadium oxide nanosheets, and the average particle size of the precursor is 1 to 2 μm.
[0016] The application of the three-dimensional eggshell structure V2O3 electrode material described in this invention in the preparation of lithium-ion batteries.
[0017] Furthermore, the three-dimensional egg yolk shell structure V2O3 electrode material is used as the negative electrode material for lithium-ion batteries.
[0018] Preparation principle: See Figure 1 A high-temperature mixed solvothermal method was employed, utilizing a specially designed dual-chamber reactor liner to prevent V₂O₅ (vanadium source) and glucose (surfactant) from contacting each other during heating, ensuring complete hydrolysis of V₂O₅. Once the reaction temperature was reached, the reactor was rotated to bring the solutions in the two chambers into contact. Glucose reduced pentavalent vanadium ions and participated in the crystallization and assembly of vanadium oxide, yielding microspheres composed of vanadium oxide nanosheets. As the reaction proceeded, the microspheres gradually grew and formed a yolk-shell structure due to the Ostwald ripening mechanism. After annealing under a nitrogen atmosphere, the vanadium oxide nanosheets were further reduced to V₂O₃ nanoparticles, retaining the three-dimensional yolk-shell structure.
[0019] The three-dimensional egg yolk shell structure V2O3 electrode material prepared in this invention is a micron-scale material with a three-dimensional micro-nano structure formed by the orderly assembly of V2O3 nanoparticles. Compared with the traditional core-shell structure, the egg yolk shell structure has a certain space (i.e., cavity) between the core layer and the shell layer, which can alleviate volume changes during charging and discharging and improve the structural stability of the material. Compared with hollow spheres, the presence of the core layer increases the tap density of the material, thereby increasing its volumetric capacity. The V2O3 nanoparticles in the core layer have many pores, which are conducive to electrolyte penetration and lithium ion diffusion, thereby further improving its electrochemical performance.
[0020] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0021] (1) The three-dimensional egg yolk shell structure V2O3 electrode material prepared by high temperature mixed solvothermal method combined with heat treatment has a special egg yolk shell structure micro-nano structure. The micro-nano structure can overcome the disadvantage of easy aggregation while retaining the advantages of high specific surface area of nanomaterials. At the same time, the egg yolk shell structure has a certain space between the core layer and the shell layer, which can buffer the volume change during charging and discharging, thereby improving the structural stability. The porous structure between V2O3 nanoparticles ensures the penetration of electrolyte and lithium ion diffusion, which is beneficial to improving electrochemical performance and provides an excellent choice for lithium-ion battery anode material.
[0022] (2) The preparation method of the present invention has the characteristics of simple process, low cost, simple equipment and fast synthesis speed, which is conducive to large-scale preparation and application. Attached Figure Description
[0023] Figure 1 This is a schematic diagram illustrating the preparation process of the three-dimensional egg yolk shell structure V2O3 electrode material of the present invention;
[0024] Figure 2 SEM image of the three-dimensional egg yolk shell structure V2O3 precursor prepared in Example 1;
[0025] Figure 3 SEM image of the three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 1;
[0026] Figure 4 TEM image of the three-dimensional egg yolk shell structure V2O3 precursor prepared in Example 1;
[0027] Figure 5 TEM image of the three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 1;
[0028] Figure 6 SEM image of the three-dimensional egg yolk shell structure V2O3 precursor prepared in Example 2;
[0029] Figure 7 SEM image of the three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 2;
[0030] Figure 8 SEM image of the three-dimensional egg yolk shell structure V2O3 precursor prepared in Example 3;
[0031] Figure 9 SEM image of the three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 3;
[0032] Figure 10 SEM image of the precursor prepared in Comparative Example 1;
[0033] Figure 11 SEM image of the electrode material prepared in Comparative Example 1;
[0034] Figure 12 SEM image of the precursor prepared in Comparative Example 2;
[0035] Figure 13 SEM image of the electrode material prepared in Comparative Example 2;
[0036] Figure 14 The images show the XRD patterns of the electrode materials in Examples 1-3 and Comparative Examples 1-3.
[0037] Figure 15 The graphs show the cycle performance of batteries prepared with electrode materials from Examples 1-3 and Comparative Examples 1-2.
[0038] Figure 16 The graph shows the cycling performance of a battery prepared using the electrode material prepared in Example 1 under high current. Detailed Implementation Plan
[0039] The technical solution of the present invention will be further described below with reference to the accompanying drawings.
[0040] Example 1
[0041] Preparation process as follows Figure 1 As shown:
[0042] (1) Weigh 0.364g of V2O5 and add it to 10mL of anhydrous ethanol, stir well to make solution A. Separately weigh 0.1568g of glucose monohydrate and add it to 10mL of anhydrous ethanol, stir well to make solution B;
[0043] (2) Place solution A and solution B into two chambers of the PTFE-lined container, with each chamber having a volume of 10.8 mL and the total volume of the liner being 41.1 mL. Seal the PTFE-lined container in a hydrothermal reactor and place it in a hydrothermal oven to heat to 240 °C, ensuring that solution A and solution B do not come into contact before reaching 240 °C.
[0044] (3) When the reaction temperature in step (2) rises to 240°C, rotate the hydrothermal reactor to mix liquid A and liquid B, and continue to rotate the reactor to react at 240°C for 1 hour.
[0045] (4) After the reaction in step (3) is completed and the reactor is cooled to room temperature, open the reactor and wash the precipitate in the liner with deionized water and anhydrous ethanol alternately, filter it three times, and dry it in an 80°C vacuum drying oven for 12 hours to obtain the precursor powder.
[0046] (5) The precursor powder obtained in step (4) is heated to 600°C at a heating rate of 5°C / min under a nitrogen atmosphere and kept at that temperature for 2 hours. Then it is cooled to room temperature and removed to obtain a three-dimensional egg yolk shell structure V2O3 electrode material.
[0047] Scanning electron microscopy analysis was performed on the precursor and the three-dimensional yolk shell structure V2O3 electrode material prepared in this embodiment. The results are as follows: Figure 2-3 As shown. Figure 2 This is a SEM image of the three-dimensional egg yolk shell structure V2O3 precursor prepared in Example 1. Figure 2 As can be seen, the precursor has the morphology of spherical particles with a diameter of 1 to 2 μm composed of nanosheets. Figure 3 This is a SEM image of the three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 1. Figure 3 As can be seen, the morphology of the three-dimensional egg yolk shell structure V2O3 electrode material consists of spherical particles with a diameter of 1 to 2 μm composed of V2O3 nanoparticles.
[0048] Transmission electron microscopy analysis was performed on the precursor and the three-dimensional yolk shell structure V2O3 electrode material prepared in this embodiment. The results are as follows: Figure 4-5 As shown. Figure 4This is a TEM image of the three-dimensional egg yolk shell structure V2O3 precursor prepared in Example 1. Figure 4 As can be seen, the precursor has a yolk-shell structure consisting of a core layer, a cavity, and a shell layer, and both the core layer and the shell layer are composed of vanadium oxide nanosheets. Figure 5 TEM images of the three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 1 are provided by Figure 5 As can be seen, the three-dimensional egg yolk shell structure V2O3 electrode material inherits the egg yolk shell structure of the precursor before annealing, and both the core layer and the shell layer are composed of V2O3 nanoparticles.
[0049] Example 2
[0050] The preparation process is the same as in Example 1:
[0051] (1) Weigh 0.364g of V2O5 and add it to 10mL of anhydrous ethanol, stir well to make solution A. Separately weigh 0.0784g of glucose monohydrate and add it to 10mL of anhydrous ethanol, stir well to make solution B;
[0052] (2) Place solution A and solution B into two chambers of the PTFE-lined container, with each chamber having a volume of 10.8 mL and the total volume of the liner being 41.1 mL. Seal the PTFE-lined container in a hydrothermal reactor and place it in a hydrothermal oven to heat to 200 °C, ensuring that solution A and solution B do not come into contact before reaching 200 °C.
[0053] (3) When the reaction temperature in step (2) rises to 200°C, rotate the hydrothermal reactor to mix liquid A and liquid B, and continue to rotate the reactor to react at 200°C for 3 hours.
[0054] (4) After the reaction in step (3) is completed and the reactor is cooled to room temperature, open the reactor and wash the precipitate in the liner with deionized water and anhydrous ethanol alternately, filter it three times, and dry it in a vacuum drying oven at 60°C for 24 hours to obtain the precursor powder.
[0055] (5) The precursor powder obtained in step (4) is heated to 600°C at a heating rate of 5°C / min under a nitrogen atmosphere and kept at that temperature for 2 hours. Then it is cooled to room temperature and removed to obtain a three-dimensional egg yolk shell structure V2O3 electrode material.
[0056] Scanning electron microscopy analysis was performed on the precursor and the three-dimensional yolk shell structure V2O3 electrode material prepared in this embodiment. The results are as follows: Figure 6-7 As shown. Figure 6 The image shows a SEM image of the three-dimensional egg yolk shell structure V2O3 precursor prepared in Example 2. Figure 6 As can be seen, the precursor has the morphology of spherical particles with a diameter of 1 to 2 μm composed of nanosheets. Figure 7This is a SEM image of the three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 2. Figure 7 As can be seen, the morphology of the three-dimensional egg yolk shell structure V2O3 electrode material is composed of spherical particles with a diameter of 1 to 2 μm composed of V2O3 nanoparticles.
[0057] Example 3
[0058] (1) Weigh 0.364g of V2O5 and add it to 10mL of anhydrous ethanol, stir well to make solution A. Separately weigh 0.2352g of glucose monohydrate and add it to 10mL of anhydrous ethanol, stir well to make solution B;
[0059] (2) Place solution A and solution B into two chambers of the PTFE-lined container, with each chamber having a volume of 10.8 mL and the total volume of the liner being 41.1 mL. Seal the PTFE-lined container in a hydrothermal reactor and place it in a hydrothermal oven to heat to 180 °C, ensuring that solution A and solution B do not come into contact before reaching 180 °C.
[0060] (3) When the reaction temperature in step (2) rises to 180°C, rotate the hydrothermal reactor to mix liquid A and liquid B, and continue to rotate the reactor to react at 180°C for 6 hours.
[0061] (4) After the reaction in step (3) is completed and the reactor is cooled to room temperature, open the reactor and wash the precipitate in the liner with deionized water and anhydrous ethanol alternately, filter it three times, and dry it in an 80°C vacuum drying oven for 12 hours to obtain the precursor powder.
[0062] (5) The precursor powder obtained in step (4) is heated to 700°C at a heating rate of 10°C / min under a nitrogen atmosphere and kept at that temperature for 1 hour. Then it is cooled to room temperature and removed to obtain a three-dimensional egg yolk shell structure V2O3 electrode material.
[0063] Scanning electron microscopy analysis was performed on the precursor and the three-dimensional yolk shell structure V2O3 electrode material prepared in this embodiment. The results are as follows: Figure 8-9 As shown. Figure 8 This is a SEM image of the three-dimensional egg yolk shell structure V2O3 precursor prepared in Example 3. Figure 8 As can be seen, the precursor has the morphology of spherical particles with a diameter of 1 to 2 μm composed of nanosheets. Figure 9 The image shows a SEM image of the three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 3. Figure 9 As can be seen, the morphology of the three-dimensional egg yolk shell structure V2O3 electrode material consists of spherical particles with a diameter of 1 to 2 μm composed of V2O3 nanoparticles.
[0064] Comparative Example 1
[0065] The specific preparation process is the same as in Example 1, except that the amount of glucose monohydrate added in step (1) is 0g, that is, no glucose monohydrate is added.
[0066] Scanning electron microscopy analysis was performed on the precursor and electrode materials prepared in this comparative example. The results are as follows: Figure 10-11 As shown. Figure 10 SEM images of the precursor samples prepared for Comparative Example 1, by Figure 10 As can be seen, the precursor morphology consists of dispersed nanosheets, rather than spherical particles with a three-dimensional eggshell structure. This demonstrates that the addition of glucose monohydrate plays a role in regulating morphology and enabling the self-assembly of nanosheets. Figure 11 The image shows a SEM image of the electrode material prepared in Comparative Example 1. Figure 11 It can be seen that without the addition of glucose monohydrate, the final electrode material obtained is also a dispersed nanosheet, and no spherical particles with a three-dimensional egg yolk shell structure are obtained.
[0067] Comparative Example 2
[0068] The specific preparation process is the same as in Example 1, except that in step (2), the reactor liner is a common single-cavity liner. Liquid A and liquid B are added to the single-cavity liner before heating and mixed. After mixing and heating, the reaction is carried out at the same reaction temperature as in Example 1.
[0069] Scanning electron microscopy analysis was performed on the precursor and electrode materials prepared in this comparative example. The results are as follows: Figure 12-13 As shown. Figure 12 SEM images of the precursor samples prepared for Comparative Example 2, by Figure 12 As can be seen, the precursor exhibits an irregular flower-like morphology composed of nanosheets, rather than spherical particles forming a three-dimensional egg yolk shell structure. This demonstrates that the high-temperature mixing solvothermal method (i.e., mixing before heating and then reacting) is a key factor in the preparation of the three-dimensional egg yolk shell structure. Figure 13 Here is a SEM image of the electrode material prepared in Comparative Example 2, by... Figure 13 It is evident that mixing solutions A and B before the reaction temperature results in an irregular flower-like morphology, and an electrode material with a three-dimensional eggshell structure cannot be obtained.
[0070] Comparative Example 3
[0071] The specific preparation process is the same as in Example 1, except that the annealing temperature in step (5) is 500°C.
[0072] Example 4
[0073] The products of Examples 1-3 and Comparative Examples 1-3 were characterized by phase analysis, including SEM analysis and XRD analysis (XRD patterns are shown in Figure 1-3). Figure 14 As shown in the figure, the result is as follows: Figure 14 As shown in Table 1.
[0074] Table 1. Phase characterization test results
[0075]
[0076] Depend on Figure 14 It can be seen that pure-phase V2O3 was obtained in Examples 1-3 and Comparative Examples 1-2, while Comparative Example 3 did not yield a pure-phase V2O3 final product. Table 1 shows that when the molar ratio of glucose monohydrate to V2O5 is 0.2–0.6:1, the hydrothermal temperature is 180–240℃, the hydrothermal time is 1–6 h, and a high-temperature mixed solvothermal method is used, a three-dimensional eggshell structure can be obtained. When the annealing temperature is 600–700℃, the pure-phase V2O3 final product can be successfully prepared.
[0077] Example 5
[0078] The three-dimensional egg yolk shell structure V2O3 electrode material prepared in Example 1 and the materials prepared in Comparative Examples 1-3 were used as negative electrode materials for lithium-ion batteries. The specific steps are as follows:
[0079] (1) Weigh 70 mg of V2O3 electrode material, 20 mg of acetylene black and 10 mg of PVDF prepared in Example 1, add an appropriate amount of N-methylpyrrolidone as a solvent, and grind thoroughly into a uniform slurry.
[0080] (2) The slurry prepared in step (1) is uniformly coated onto a 316.7 cm thick surface using a casting coating machine. 2 The active material loading on the copper foil is approximately 0.221 mg / cm³. 2 Then, the copper foil coated with the slurry is placed in a vacuum drying oven at 80°C and dried for 12 hours.
[0081] (3) Take out the dried copper foil from step (2) and cut it into a circular piece with a diameter of 12mm using a punching machine, which will serve as the working electrode.
[0082] (4) The 12mm circular electrode obtained in step (3) is used as the working electrode, the lithium metal sheet is used as the reference electrode, the Celgard disc is used as the separator, and the organic electrolyte containing 1M LiPF6 (EC:DEC:DMC=1:1:1) is used as the electrolyte. The 2016 battery case is used to assemble the coin cell in an argon glove box. After standing for 24 hours, the electrochemical performance is tested.
[0083] Batteries using the electrode materials of Examples 2-3 and Comparative Examples 1-2 were prepared using the above method, and their electrochemical performance was tested.
[0084] After electrochemical performance cycling tests, the performance of Examples 1-3 is as follows: Figure 15 As shown, Figure 15The graphs show the cycle performance of batteries prepared using electrode materials from Examples 1-3 and Comparative Examples 1-2. Figure 15 As can be seen, when the current density is 100 mA / g and the cycle length is around 500 cycles, the capacities of Examples 1-3 are as high as 650.1, 653.7, and 621.6 mAh / g, respectively, exceeding the theoretical specific capacity of V2O3 (356 mAh / g). Furthermore, the batteries exhibit a significant capacity increase during cycling, demonstrating that the three-dimensional micro / nano porous structure of the material provides abundant active sites and high pseudocapacitance. In contrast, the two-dimensional nanosheet V2O3 electrode material of Comparative Example 1 has a much lower initial capacity than the three-dimensional eggshell V2O3 electrode materials of Examples 1-3. Although it also shows some capacity increase in subsequent cycles, capacity decay occurs only around 400 cycles, with a capacity of approximately 355.8 mAh / g after 550 cycles. This is because while the morphology of the nanosheets provides a large specific surface area, they are prone to stacking and aggregation during cycling, resulting in unsatisfactory cycling performance. The initial capacity of the irregular nanoflower-shaped V2O3 electrode material in Comparative Example 2 was comparable to that of the three-dimensional egg yolk shell V2O3 electrode materials in Examples 1-3, indicating that the assembly of nanosheets into a three-dimensional structure has a significant effect on capacity improvement. However, its capacity increase was not significant in subsequent cycles, reaching 420.8 mAh / g at around 450 cycles, with the capacity gap gradually widening compared to Examples 1-3. This demonstrates that the three-dimensional egg yolk shell structure can provide high pseudocapacitance, fully utilize the electrode material, and exhibit superior cycling performance.
[0085] The battery prepared with the material in Example 1 was then subjected to a high-current cycling test, and the results are as follows: Figure 16 As shown, by Figure 16 As can be seen, when the current densities are 1A / g, 2A / g, and 5A / g, after 1000 cycles, the battery capacities are 472mAh / g, 315.9mAh / g, and 213mAh / g, respectively, demonstrating the long-term cycling stability of the three-dimensional eggshell structure under high current.
[0086] In summary, the three-dimensional eggshell-structured V2O3 electrode material prepared by this invention exhibits high capacity and long-term cycle stability under high current when used as a negative electrode in lithium-ion batteries, making it a very promising lithium-ion battery electrode material.
Claims
1. A three-dimensional yolk-shell structure V2O3 electrode material, characterized in that, The V2O3 electrode material is a spherical particle with a three-dimensional yolk shell structure consisting of a core layer, a cavity, and a shell layer, wherein both the shell layer and the core layer are V2O3 nanoparticles. Its preparation method includes the following steps: (1) Add V2O5 to anhydrous ethanol and stir until homogeneous to obtain solution A. Add glucose to anhydrous ethanol and stir until homogeneous to obtain solution B. (2) First, heat solution A and solution B separately, then mix solution A and solution B, heat to react, cool to room temperature, wash and dry the product to obtain precursor powder; the molar ratio of glucose to V2O5 is 0.2~0.6:1; heat separately to the reaction temperature, the reaction temperature is 180℃~240℃, and the heating reaction time is 1~6h; (3) The precursor powder was annealed under a nitrogen atmosphere to obtain a three-dimensional egg yolk shell structure V2O3 electrode material; the annealing temperature was 500~700℃, the heating rate was 5~10℃ / min, and the annealing time was 1~2h.
2. The three-dimensional yolk-shell structure V2O3 electrode material of claim 1, wherein, The diameter of the spherical particles is 1~2μm.
3. The method of producing a three-dimensional yolk-shell structure V2O3 electrode material according to claim 1 or 2, characterized in that, Includes the following steps: (1) Add V2O5 to anhydrous ethanol and stir until homogeneous to obtain solution A. Add glucose to anhydrous ethanol and stir until homogeneous to obtain solution B. (2) First, heat solution A and solution B separately, then mix solution A and solution B, heat to react, cool to room temperature, wash and dry the product to obtain precursor powder; the molar ratio of glucose to V2O5 is 0.2~0.6:1; heat separately to the reaction temperature, the reaction temperature is 180℃~240℃, and the heating reaction time is 1~6h; (3) The precursor powder was annealed under a nitrogen atmosphere to obtain a three-dimensional egg yolk shell structure V2O3 electrode material; the annealing temperature was 500~700℃, the heating rate was 5~10℃ / min, and the annealing time was 1~2h.
4. The production method according to claim 3, characterized by, In step (2), the drying temperature is 60℃~80℃ and the drying time is 12~24h.
5. The preparation method according to claim 3, characterized in that, In step (3), the precursor is a spherical eggshell structure composed of vanadium oxide nanosheets, and the average particle size of the precursor is 1~2μm.
6. The application of the three-dimensional eggshell structure V2O3 electrode material as described in claim 1 or 2 in the preparation of lithium-ion batteries.
7. The application according to claim 6, characterized in that, The three-dimensional eggshell-structured V2O3 electrode material is used as the negative electrode material for lithium-ion batteries.
Citation Information
Patent Citations
Carbon-coated vanadium trioxide nano material preparing method and lithium ion batteries
CN106025276A