Positive electrode sheet and its preparation method, sodium-ion battery
By alternately forming polycrystalline and monocrystalline layered oxide positive electrode active material layers on the surface of a conductive substrate, the problem of the fragility of sodium-ion battery positive electrode materials during processing is solved, thereby improving the battery cycle life and capacity.
Patent Information
- Application Number
- CN202311535461.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-17
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-17
AI Technical Summary
Existing sodium-ion battery cathode materials are easily cracked or crushed during processing, leading to an increased contact area with the electrolyte, resulting in side reactions and deterioration of battery cycle performance. Furthermore, single-crystal layered transition metal oxides have insufficient capacity.
A positive electrode active material layer consisting of alternating polycrystalline and monocrystalline layered oxides is formed on the surface of a conductive substrate. The monocrystalline layered oxides protect the polycrystalline layered oxides, reducing electrolyte contact, and the polycrystalline layered oxides compensate for the insufficient capacity of the monocrystalline layered oxides.
It significantly reduces side reactions on the positive electrode surface and electrolyte consumption, thereby improving the cycle life and capacity of sodium-ion batteries.
Smart Images

Figure CN117637985B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of sodium-ion battery technology, and in particular to a positive electrode sheet and its preparation method, and a sodium-ion battery. Background Technology
[0002] In recent years, the new energy vehicle and energy storage sectors have flourished, leading to a surge in demand for lithium-ion batteries. However, this surge in demand coupled with a severe shortage of lithium resources has resulted in a sharp rise in lithium salt prices, significantly increasing the cost of lithium-ion batteries and hindering the healthy and sustainable development of the industry. Sodium, a mineral in the same group as lithium, is abundant and inexpensive. The research and development of sodium-ion batteries can, to some extent, alleviate the limitations on battery development caused by lithium resource shortages.
[0003] Layered transition metal oxides are the most mature cathode materials used in sodium-ion battery research and industrialization, mainly including monocrystalline and polycrystalline layered transition metal oxides. However, monocrystalline layered transition metal oxides have low capacity, which cannot meet the requirements of battery use; although polycrystalline layered transition metal oxides have high capacity, they are difficult to process and use. In addition, polycrystalline layered transition metal oxides have a large specific surface area, resulting in a large contact area with the electrolyte. The rolling process in battery manufacturing is prone to cracking or crushing of the cathode material, which further increases the contact area between the cathode and the electrolyte, making it difficult to solve the problems of gas generation and cycle degradation. Summary of the Invention
[0004] Therefore, it is necessary to provide a positive electrode sheet and its preparation method that can reduce the contact between the positive electrode material and the electrolyte and improve the cycle life and capacity of sodium-ion batteries, as well as a sodium-ion battery.
[0005] In a first aspect, this application provides a positive electrode sheet, comprising a conductive substrate and a first positive electrode active material layer and a second positive electrode active material layer sequentially formed on a first surface of the conductive substrate;
[0006] The first positive electrode active material layer is composed of polycrystalline layered oxide, and the second positive electrode active material layer is composed of monocrystalline layered oxide.
[0007] In some embodiments, a third positive electrode active material layer and a fourth positive electrode active material layer are sequentially formed on the second surface of the conductive substrate;
[0008] The material of the third positive electrode active material layer comprises a polycrystalline layered oxide, and the material of the fourth positive electrode active material layer comprises a monocrystalline layered oxide.
[0009] In some embodiments, the positive electrode sheet satisfies at least one of the following characteristics:
[0010] 1) The areal density of the first positive electrode active material layer and the third positive electrode active material layer is independently 2.5 mg / cm³. 2 ~7.5mg / cm 2 The surface density of both sides is 5 mg / cm³. 2 ~15mg / cm 2 ;
[0011] 2) The areal density of the second positive electrode active material layer and the fourth positive electrode active material layer is independently 5 mg / cm³. 2 ~12.5mg / cm 2 The surface density of both sides is 10 mg / cm³. 2 ~25mg / cm 2 .
[0012] In some embodiments, the polycrystalline layered oxide and the single-crystal layered oxide each have the chemical formula Na. x Ni a Fe b Mn c M d O2, where 0<x≤1,a+b+c+d=1,a> 0, b>0, c>0, d≥0, M is one or more of Cu, Ti, Zr, Co, Zn, Mg, Al and Ca.
[0013] In some embodiments, the positive electrode sheet satisfies at least one of the following characteristics:
[0014] 1) The polycrystalline layered oxide is a secondary particle, and the particle size of the polycrystalline layered oxide satisfies: D10 is 1μm~5μm, D50 is 5μm~10μm, and D90 is 15μm~25μm; in the secondary particles, the particle size of the primary particles is 50nm~500nm.
[0015] 2) The single-crystal layered oxide is a primary particle, and the particle size of the single-crystal layered oxide satisfies: D10 is 1μm~3μm, D50 is 3μm~15μm, and D90 is 15μm~25μm;
[0016] 3) The compacted density of the positive electrode sheet is 2.8 mg / cm³. 3 ~3.3mg / cm 3 .
[0017] Secondly, this application provides a method for preparing a positive electrode sheet as described in the first aspect, which includes the following steps:
[0018] The first positive electrode active material layer and the second positive electrode active material layer are sequentially formed on the first surface of the conductive substrate to prepare the positive electrode sheet.
[0019] In some embodiments, the preparation method further includes the step of sequentially forming the third positive electrode active material layer and the fourth positive electrode active material layer on the second surface of the conductive substrate.
[0020] In some embodiments, the method for forming the first positive electrode active material layer, the second positive electrode active material layer, the third positive electrode active material layer, and the fourth positive electrode active material layer includes:
[0021] The first positive electrode slurry is coated onto the first surface of the conductive substrate to form the first positive electrode active material layer;
[0022] A second positive electrode slurry is coated on the side of the first positive electrode active material layer that is away from the first surface of the conductive substrate to form the second positive electrode active material layer;
[0023] The third positive electrode slurry is coated onto the second surface of the conductive substrate to form the third positive electrode active material layer;
[0024] A fourth positive electrode slurry is coated on the side of the third positive electrode active material layer that is opposite to the second surface of the conductive substrate to form the fourth positive electrode active material layer.
[0025] In some embodiments, the first positive electrode slurry and the third positive electrode slurry comprise: a polycrystalline layered oxide, a first conductive agent, a first binder, and a first solvent;
[0026] The second positive electrode slurry and the fourth positive electrode slurry comprise: a single-crystal layered oxide, a second conductive agent, a second binder, and a second solvent;
[0027] Optionally, the first conductive agent and the second conductive agent each independently include one or more of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene;
[0028] Optionally, the first adhesive and the second adhesive are each independently polyvinylidene fluoride;
[0029] Optionally, the first solvent and the second solvent are each independently N-methylpyrrolidone.
[0030] In some embodiments, the preparation process further includes pressing the positive electrode sheet to achieve a compaction density of 2.8 mg / cm³. 3 ~3.3mg / cm 3 The steps.
[0031] Thirdly, this application provides a sodium-ion battery comprising the positive electrode sheet described in the first aspect.
[0032] The positive electrode sheet provided in this application forms positive electrode active material layers with different crystal forms on the surface of a conductive substrate. A second positive electrode active material layer with a single-crystal structure is placed outside a first positive electrode active material layer with a polycrystalline structure. This achieves the protective effect of the single-crystal positive electrode active material layer on the polycrystalline positive electrode active material layer, significantly reducing the contact between the electrolyte and the polycrystalline layered oxide. This significantly reduces side reactions and associated gases occurring on the battery's positive electrode surface, while also significantly reducing electrolyte consumption during battery cycling, resulting in a substantial improvement in the cycle life of sodium-ion batteries. Furthermore, the polycrystalline layered oxide can compensate for the insufficient capacity of the single-crystal layered oxide, thus comprehensively improving both the cycle life and capacity of the sodium-ion battery. Attached Figure Description
[0033] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0034] Figure 1 A schematic diagram of the structure of the positive electrode sheet in one embodiment;
[0035] Figure 2 This is a scanning electron microscope image of the positive electrode sheet prepared in Example 1;
[0036] Figure 3 This is a scanning electron microscope image of the positive electrode sheet prepared in Example 2;
[0037] Figure 4 This is a scanning electron microscope image of the positive electrode sheet prepared in Example 3;
[0038] Figure 5 This is a scanning electron microscope image of the positive electrode sheet prepared in Example 4;
[0039] Figure 6 This is a scanning electron microscope image of the positive electrode sheet prepared in Example 5;
[0040] Figure 7 The image shows a scanning electron microscope (SEM) image of the positive electrode sheet prepared in Comparative Example 1.
[0041] Figure 8 The image shows a scanning electron microscope (SEM) image of the positive electrode sheet prepared in Comparative Example 2.
[0042] Figure 9The graphs show the cycle performance test results of the positive electrode sheets prepared in Examples 1-5 and Comparative Examples 1-2.
[0043] Explanation of reference numerals in the attached figures: 100, conductive substrate; 200, first positive electrode active material layer; 300, second positive electrode active material layer; 400, third positive electrode active material layer; 500, fourth positive electrode active material layer. Detailed Implementation
[0044] To facilitate understanding of this application, a more complete description is provided below. However, this application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of this application.
[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.
[0046] the term:
[0047] As used herein, the term "and / or" encompasses any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" includes three parallel options: A, B, and "a combination of A and B".
[0048] In this document, unless otherwise stated, "one or more" means any one of the listed items or any combination of the listed items. Similarly, "one or more" and other instances of "one or more" are to be understood in the same way unless otherwise stated.
[0049] In this document, terms such as "further," "even further," "especially," "for example," "like," "example," and "exemplary" are used for descriptive purposes to indicate a connection in the coverage of different technical solutions presented earlier and later. However, they should not be construed as limitations on the preceding technical solution or on the scope of protection of this document. Unless otherwise specified, in this document, A (e.g., B) indicates that B is a non-limiting example of A, and it can be understood that A is not limited to B.
[0050] In this document, "optionally," "optionally," and "optional" mean that something is optional, that is, it is selected from either "present" or "absent." If multiple "options" appear in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "option" is independent. In this application, descriptions such as "optionally contains" and "optionally includes" indicate "contains or does not contain." "Optional component X" indicates whether component X exists or does not exist, or whether component X is contained or not.
[0051] In this document, the terms "first aspect," "second aspect," "third aspect," and "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," and "fourth" serve only as a non-exhaustive enumeration and should be understood as not constituting a closed limitation on quantity.
[0052] In this article, the technical features described in an open-ended manner include both closed technical solutions composed of the listed features and open technical solutions that include the listed features.
[0053] In this document, when referring to numerical intervals (i.e., numerical ranges), unless otherwise specified, the distribution of selectable values within a numerical interval is considered continuous, and includes the two endpoints (i.e., the minimum and maximum values) of the numerical interval, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints, which is equivalent to directly listing every integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all subranges included therein. The "numerical value" in this numerical interval can be any quantitative value, such as a number, percentage, ratio, etc. The term "numerical interval" can be broadly included to include percentage intervals, ratio intervals, proportion intervals, and other numerical interval types.
[0054] In this document, for methods involving multiple steps, unless otherwise explicitly stated herein, there is no strict order constraint on the execution of these steps; they may be executed in any order other than those described. Moreover, any step may include multiple sub-steps or multiple stages, which are not necessarily completed at the same time, but may be executed at different times, and their execution order is not necessarily sequential, but may be executed in turn, alternately, or simultaneously with other steps or parts of the sub-steps or stages of other steps.
[0055] Traditional cathode materials made from single-crystal layered transition metal oxides or polycrystalline layered transition metal oxides suffer from low capacity or poor cycle performance. Therefore, this application provides a cathode electrode to improve the cycle life and increase the capacity of sodium-ion batteries.
[0056] In a first aspect, this application provides a positive electrode sheet, comprising a conductive substrate and a first positive electrode active material layer and a second positive electrode active material layer sequentially formed on a first surface of the conductive substrate;
[0057] The first positive electrode active material layer is composed of polycrystalline layered oxide, and the second positive electrode active material layer is composed of monocrystalline layered oxide.
[0058] The positive electrode sheet provided in this application forms positive electrode active material layers with different crystal forms on the surface of a conductive substrate. A second positive electrode active material layer with a single-crystal structure is placed outside a first positive electrode active material layer with a polycrystalline structure. This achieves the protective effect of the single-crystal positive electrode active material layer on the polycrystalline positive electrode active material layer, significantly reducing the contact between the electrolyte and the polycrystalline layered oxide. This significantly reduces side reactions and associated gases occurring on the battery's positive electrode surface, while also significantly reducing electrolyte consumption during battery cycling, resulting in a substantial improvement in the cycle life of sodium-ion batteries. Furthermore, the polycrystalline layered oxide can compensate for the insufficient capacity of the single-crystal layered oxide, thus comprehensively improving both the cycle life and capacity of the sodium-ion battery.
[0059] In this application, the conductive substrate can be a material commonly used in the positive electrode of sodium-ion batteries, such as metal foil. More specifically, the conductive substrate can be aluminum foil.
[0060] In some embodiments, a third positive electrode active material layer and a fourth positive electrode active material layer are sequentially formed on the second surface of the conductive substrate;
[0061] The material of the third positive electrode active material layer comprises a polycrystalline layered oxide, and the material of the fourth positive electrode active material layer comprises a monocrystalline layered oxide.
[0062] It is understood that in this application, the positive electrode active material layer may be formed only on one side of the conductive substrate, or it may be formed on both sides of the conductive substrate simultaneously.
[0063] Please see Figure 1In one embodiment, the positive electrode includes a conductive substrate 100, a first positive electrode active material layer 200, a second positive electrode active material layer 300, a third positive electrode active material layer 400, and a fourth positive electrode active material layer 500. The first positive electrode active material layer 200 and the third positive electrode active material layer 400 are located on opposite sides of the conductive substrate 100, the second positive electrode active material layer 300 is located on the side of the first positive electrode active material layer 200 facing away from the conductive substrate 100, and the fourth positive electrode active material layer 500 is located on the side of the third positive electrode active material layer 400 facing away from the conductive substrate 100.
[0064] It can be understood that single-sided areal density refers to the weight of the positive electrode active material layer per unit area of the substrate when one side of the conductive substrate is coated with the positive electrode slurry; double-sided areal density refers to the weight of the positive electrode active material layer per unit area of the substrate when both sides of the conductive substrate are coated with the same positive electrode slurry. In some embodiments, the single-sided areal density of the first positive electrode active material layer and the third positive electrode active material layer are each independently 2.5 mg / cm³. 2 ~7.5mg / cm 2 The surface density of both sides is 5 mg / cm³. 2 ~15mg / cm 2 .
[0065] In some embodiments, the areal density of the second and fourth positive electrode active material layers is independently 5 mg / cm³. 2 ~12.5mg / cm 2 The surface density of both sides is 10 mg / cm³. 2 ~25mg / cm 2 .
[0066] In some embodiments, the polycrystalline layered oxide and the monocrystalline layered oxide each have the chemical formula Na. x Ni a Fe b Mn c M d O2, where 0<x≤1,a+b+c+d=1,a> 0, b>0, c>0, d≥0, M is one or more of Cu, Ti, Zr, Co, Zn, Mg, Al and Ca.
[0067] Furthermore, the polycrystalline layered oxide and the monocrystalline layered oxide have the same chemical formula, differing only in their crystal form. As an example, the polycrystalline layered oxide and the monocrystalline layered oxide are sodium nickel iron manganese oxide (NaNi). 1 / 3 Fe 1 / 3 Mn 1 / 3O2), sodium copper-nickel-iron-manganese oxide (NaCu) 1 / 9 Ni 2 / 9 Fe1 / 3 Mn 1 / 3 O2) or sodium nickel manganese aluminum oxide (NaNi) 3 / 10 Fe 1 / 3 Mn 1 / 3 Al 1 / 30 O2).
[0068] In this application, the polycrystalline layered oxide is a secondary particle, and the polycrystalline layered oxide contains particles of various sizes. In some embodiments, the particle size of the polycrystalline layered oxide satisfies: D10 is 1μm~5μm, D50 is 5μm~10μm, and D90 is 15μm~25μm; among the secondary particles, the primary particles have a particle size of 50nm~500nm.
[0069] It is understandable that secondary particles are formed by the aggregation of primary particles.
[0070] In some embodiments, the coin cell composed of polycrystalline layered oxide as the positive electrode material has a specific capacity of 135 mAh / g to 180 mAh / g in the voltage range of 2.0V to 4.0V.
[0071] In this application, the single-crystal layered oxide is a primary particle, and the single-crystal layered oxide contains particles of various sizes. In some embodiments, the particle sizes of the single-crystal layered oxide satisfy the following: D10 is 1μm~3μm, D50 is 3μm~15μm, and D90 is 15μm~25μm.
[0072] In some embodiments, the coin cell composed of a single-crystal layered oxide as the positive electrode material has a specific capacity of 75 mAh / g to 135 mAh / g in the voltage range of 2.0V to 4.0V.
[0073] In some embodiments, the compaction density of the positive electrode sheet is 2.8 mg / cm³. 3 ~3.3mg / cm 3 .
[0074] Secondly, this application provides a method for preparing a positive electrode sheet as described in the first aspect, which includes the following steps:
[0075] The first positive electrode active material layer and the second positive electrode active material layer are sequentially formed on the first surface of the conductive substrate to prepare the positive electrode sheet.
[0076] In some embodiments, the preparation method further includes the step of sequentially forming the third positive electrode active material layer and the fourth positive electrode active material layer on the second surface of the conductive substrate.
[0077] In this application, the method for forming the positive electrode active material layer on the surface of the conductive substrate is not limited, and any coating forming process known in the field of sodium-ion battery manufacturing can be used. As an example, a coating process can be used to form the positive electrode active material layer.
[0078] In some embodiments, the method for forming the first positive electrode active material layer and the second positive electrode active material layer includes:
[0079] The first positive electrode slurry is coated onto the first surface of the conductive substrate to form the first positive electrode active material layer;
[0080] A second positive electrode slurry is coated on the side of the first positive electrode active material layer that is away from the first surface of the conductive substrate to form the second positive electrode active material layer.
[0081] In some embodiments, the method for forming the third positive electrode active material layer and the fourth positive electrode active material layer includes:
[0082] The third positive electrode slurry is coated onto the second surface of the conductive substrate to form the third positive electrode active material layer;
[0083] A fourth positive electrode slurry is coated on the side of the third positive electrode active material layer that is opposite to the second surface of the conductive substrate to form the fourth positive electrode active material layer.
[0084] In some embodiments, the first positive electrode slurry and the third positive electrode slurry each independently comprise: a polycrystalline layered oxide, a first conductive agent, a first binder, and a first solvent;
[0085] The second positive electrode slurry and the fourth positive electrode slurry each independently comprise: a single-crystal layered oxide, a second conductive agent, a second binder, and a second solvent.
[0086] In this application, the selection of the first conductive agent, the second conductive agent, the first binder, the second binder, the first solvent, and the second solvent is not limited, and any materials commonly used in the preparation of positive electrode slurry in the field of sodium-ion battery preparation can be selected.
[0087] In some embodiments, the first conductive agent and the second conductive agent each independently include one or more of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes, and graphene.
[0088] In some embodiments, the first adhesive and the second adhesive are each independently polyvinylidene fluoride (PVDF).
[0089] In some embodiments, the first solvent and the second solvent are each independently N-methylpyrrolidone (NMP).
[0090] In some embodiments, in the first positive electrode slurry and the third positive electrode slurry, the mass percentage of the polycrystalline layered oxide is 90% to 98%, the mass percentage of the first conductive agent is 1% to 5%, and the mass percentage of the first binder is 1% to 5%. The first solvent accounts for 50% to 70% of the total mass of the polycrystalline layered oxide, the first conductive agent, and the first binder.
[0091] In some embodiments, in the second and fourth cathode slurries, the mass percentage of the single-crystal layered oxide is 90% to 98%, the mass percentage of the second conductive agent is 1% to 5%, and the mass percentage of the second binder is 1% to 5%. The second solvent accounts for 50% to 70% of the total mass of the single-crystal layered oxide, the second conductive agent, and the second binder.
[0092] It is understandable that, in order to ensure uniform mixing of the positive electrode slurry, a step of stirring each positive electrode slurry separately is included before coating. The stirring method can be simultaneous stirring with a stirring paddle and a dispersing wheel. Furthermore, the stirring paddle speed can be 30 rpm to 60 rpm, the dispersing wheel speed can be 1000 rpm to 3000 rpm, and the stirring time can be 120 min to 240 min.
[0093] In some embodiments, the temperature of the first positive electrode slurry, the second positive electrode slurry, the third positive electrode slurry, and the fourth positive electrode slurry is 30°C to 50°C, the ambient temperature is 15°C to 30°C, and the dew point temperature is -10°C to -50°C.
[0094] It is understandable that, in order to shape the coated positive electrode slurries, a drying step may be included after coating. This drying can be achieved through heating. Furthermore, the heating temperature can be between 80℃ and 120℃.
[0095] In some embodiments, the preparation process further includes pressing the positive electrode sheet to achieve a compaction density of 2.8 mg / cm³. 3 ~3.3mg / cm 3 The steps.
[0096] In some embodiments, the pressing method is roll pressing. Further, the ambient temperature for roll pressing is 15°C to 30°C, and the dew point temperature is -10°C to -50°C.
[0097] According to a specific implementation method, the preparation method of the positive electrode sheet includes the following steps:
[0098] 1) A polycrystalline layered oxide, a first conductive agent, a first binder, and a first solvent are mixed to form a first positive electrode slurry and a third positive electrode slurry;
[0099] 2) Mix the single-crystal layered oxide, the second conductive agent, the second binder, and the second solvent to form the second positive electrode slurry and the fourth positive electrode slurry;
[0100] 3) Coat the first positive electrode slurry on the first surface of the conductive substrate and coat the third positive electrode slurry on the second surface of the conductive substrate, and dry them to form the first positive electrode active material layer and the third positive electrode active material layer, respectively;
[0101] 4) Coat the first positive electrode active material layer and the third positive electrode active material layer on the side away from the conductive substrate with the second positive electrode slurry and the fourth positive electrode slurry respectively, and dry them to form the second positive electrode active material layer and the fourth positive electrode active material layer respectively;
[0102] 5) Roll-press the conductive substrate obtained in step 4) to achieve a compaction density of 2.8 mg / cm³. 3 ~3.3mg / cm 3 .
[0103] Thirdly, this application provides a sodium-ion battery comprising the positive electrode sheet described in the first aspect.
[0104] It is understandable that sodium-ion batteries, in addition to the positive electrode, may also include other components necessary for batteries, such as the negative electrode, separator, and electrolyte.
[0105] In this application, the selection of the negative electrode, separator, and electrolyte is not limited. For example, the negative electrode can be hard carbon; the separator can be an insulating porous polymer film or an inorganic porous film, such as porous polypropylene film, porous polyethylene film, porous composite polymer film, glass fiber paper, or porous ceramic separator; the electrolyte specifically includes a sodium salt and a solvent. The sodium salt used as the electrolyte is not particularly limited, as long as it can dissociate into cations and anions. Examples include sodium chloride, sodium fluoride, sodium sulfate, sodium carbonate, sodium phosphate, sodium nitrate, sodium difluorooxalate borate, sodium pyrophosphate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, and trichlorocitric acid. Sodium, sodium metaborate, sodium borate, sodium molybdate, sodium tungstate, sodium bromide, sodium nitrite, sodium iodate, sodium iodide, sodium silicate, sodium lignosulfonate, sodium hexafluorophosphate, sodium oxalate, sodium aluminate, sodium methanesulfonate, sodium acetate, sodium dichromate, sodium hexafluoroarsenate, sodium tetrafluoroborate, sodium perchlorate, and sodium trifluoromethanesulfonylimide. The solvent may specifically include esters, sulfones, ethers, or nitrile organic solvents, including propylene carbonate, ethylene carbonate, butene carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, dimethyl ethyl carbonate, dimethyl sulfone, and dimethyl ether, or one or more of these.
[0106] The present application will be further described in detail below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application. For experimental methods in the following embodiments where specific conditions are not specified, please refer to the guidelines given in this application, or follow experimental manuals or conventional conditions in the art, or follow the conditions recommended by the manufacturer, or refer to experimental methods known in the art.
[0107] In the specific embodiments described below, the measurement parameters involving raw material components may have slight deviations within the weighing accuracy range unless otherwise specified. Temperature and time parameters are subject to acceptable deviations due to instrument testing accuracy or operational precision.
[0108] Example 1
[0109] 1) Preparation of the first positive electrode slurry:
[0110] Based on mass percentage, 96% of polycrystalline sodium nickel iron manganate (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2) was dissolved in N-methylpyrrolidone (NMP) along with 2% conductive carbon black and 2% binder PVDF to form the first positive electrode slurry. The polycrystalline sodium nickel iron manganese oxide had particle sizes D10 of 4 μm, D50 of 9 μm, and D90 of 19 μm, and its specific capacity at 2.0V~4.0V, measured using a coin cell, was 140 mAh / g. The preparation method of the third positive electrode slurry was the same as that of the first positive electrode slurry.
[0111] 2) Preparation of the second positive electrode slurry:
[0112] Based on mass percentage, 96% of the single-crystal sodium nickel iron manganate (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2) is dissolved in N-methylpyrrolidone (NMP) along with 2% conductive carbon black and 2% binder PVDF to form the second positive electrode slurry. The monocrystalline sodium nickel iron manganese oxide has particle sizes D10 of 2 μm, D50 of 7.6 μm, and D90 of 17 μm, and its specific capacity at 2.0V~4.0V, measured using a coin cell, is 127 mAh / g. The fourth positive electrode slurry is prepared using the same method as the second positive electrode slurry.
[0113] 3) Preparation of positive electrode sheet
[0114] The stirring paddle speed was controlled at 50 rpm, the dispersion wheel speed at 2500 rpm, and the stirring time at 180 min. The temperatures of both the first and third positive electrode slurries were 40℃. The first and third positive electrode slurries were coated onto both sides of an aluminum foil and dried at 100℃ to form polycrystalline first and third positive electrode active material layers on the aluminum foil surface. The areal density of both the first and third positive electrode active material layers was 7 mg / cm³. 2 The sum of the single-sided areal densities of the first and third positive electrode active material layers, i.e., the double-sided areal density, is 14 mg / cm³. 2 .
[0115] Subsequently, a second positive electrode slurry and a fourth positive electrode slurry were coated onto the surfaces of the first and third positive electrode active material layers, respectively, and dried at 110°C to form a single-crystal second positive electrode active material layer and a single-crystal fourth positive electrode active material layer on the surfaces of the first and third positive electrode active material layers, respectively. The areal density of both the second and fourth positive electrode active material layers is 8 mg / cm³. 2 The sum of the single-sided areal densities of the second and fourth positive electrode active material layers, i.e., the double-sided areal density, is 16 mg / cm³. 2 .
[0116] The conductive substrate with the positive electrode active material layer formed thereon is rolled to obtain the positive electrode sheet, while ensuring that the compaction density of the positive electrode sheet is 3.1 mg / cm³. 3 It should be noted that all processes in this embodiment were performed at an ambient temperature of 25°C and a dew point temperature of -30°C. The scanning electron microscope (SEM) image of the positive electrode sheet obtained in this embodiment is shown below. Figure 2 As shown. By Figure 2 It can be seen that the positive electrode sheet prepared in this embodiment has intact single crystal particles, and no particles were crushed by rolling. Furthermore, no polycrystalline material was observed, indicating that the polycrystalline material was completely covered.
[0117] Example 2
[0118] 1) Preparation of the first positive electrode slurry:
[0119] The preparation method is the same as in Example 1. The preparation method of the third positive electrode slurry is the same as that of the first positive electrode slurry.
[0120] 2) Preparation of the second positive electrode slurry:
[0121] The preparation method is basically the same as in Example 1, except that the particle size of the single-crystal sodium nickel iron manganese oxide is 3 μm for D10, 7.6 μm for D50, and 17 μm for D90. The preparation methods of the fourth cathode slurry and the second cathode slurry are the same.
[0122] 3) Preparation of positive electrode sheet
[0123] The stirring paddle speed was controlled at 50 rpm, the dispersion wheel speed at 2500 rpm, and the stirring time at 180 min. The temperatures of both the first and third positive electrode slurries were 40℃. The first and third positive electrode slurries were coated onto both sides of an aluminum foil and dried at 95℃ to form polycrystalline first and third positive electrode active material layers on the aluminum foil surface. The areal density of both the first and third positive electrode active material layers was 5 mg / cm³. 2 The sum of the single-sided areal densities of the first and third positive electrode active material layers, i.e., the double-sided areal density, is 10 mg / cm³. 2 .
[0124] Subsequently, a second positive electrode slurry and a fourth positive electrode slurry were coated onto the surfaces of the first and third positive electrode active material layers, respectively, and dried at 115°C to form a single-crystal second positive electrode active material layer and a single-crystal fourth positive electrode active material layer on the surfaces of the first and third positive electrode active material layers, respectively. The areal density of both the second and fourth positive electrode active material layers is 10 mg / cm³. 2 The sum of the single-sided areal densities of the second and fourth positive electrode active material layers, i.e., the double-sided areal density, is 20 mg / cm³. 2 .
[0125] The conductive substrate with the positive electrode active material layer formed thereon is rolled to obtain the positive electrode sheet, while ensuring that the compaction density of the positive electrode sheet is 3.1 mg / cm³. 3 It should be noted that all processes in this embodiment were performed at an ambient temperature of 25°C and a dew point temperature of -30°C. The scanning electron microscope (SEM) image of the positive electrode sheet obtained in this embodiment is shown below. Figure 3 As shown. By Figure 3 It can be seen that the positive electrode sheet prepared in this embodiment has intact single crystal particles, no particles are crushed by rolling, and no polycrystalline material is observed, indicating that the polycrystalline material has been completely covered.
[0126] Example 3
[0127] 1) Preparation of the first positive electrode slurry:
[0128] Same as in Example 1. The preparation method of the third positive electrode slurry is the same as that of the first positive electrode slurry.
[0129] 2) Preparation of the second positive electrode slurry:
[0130] The process is basically the same as in Example 1, except that the particle sizes of the single-crystal sodium nickel iron manganese oxide are D10 3 μm, D50 7.6 μm, and D90 17 μm. The preparation methods for the fourth cathode slurry and the second cathode slurry are the same.
[0131] 3) Preparation of positive electrode sheet
[0132] The stirring paddle speed was controlled at 50 rpm, the dispersion wheel speed at 2500 rpm, and the stirring time at 180 min. The temperatures of both the first and third positive electrode slurries were 40℃. The first and third positive electrode slurries were coated onto both sides of an aluminum foil and dried at 90℃ to form a polycrystalline first and third positive electrode active material layer on the aluminum foil surface. The areal density of both the first and third positive electrode active material layers was 3 mg / cm³. 2 The sum of the single-sided areal densities of the first and third positive electrode active material layers, i.e., the double-sided areal density, is 6 mg / cm³. 2 .
[0133] Subsequently, a second positive electrode slurry and a fourth positive electrode slurry were coated onto the surfaces of the first and third positive electrode active material layers, respectively, and dried at 120°C to form a single-crystal second positive electrode active material layer and a single-crystal fourth positive electrode active material layer on the surfaces of the first and third positive electrode active material layers, respectively. The areal density of both the second and fourth positive electrode active material layers is 12 mg / cm³. 2 The sum of the single-sided areal densities of the second and fourth positive electrode active material layers, i.e., the double-sided areal density, is 24 mg / cm³. 2 .
[0134] The conductive substrate with the positive electrode active material layer formed thereon is rolled to obtain the positive electrode sheet, while ensuring that the compaction density of the positive electrode sheet is 3.1 mg / cm³. 3 It should be noted that all processes in this embodiment were performed at an ambient temperature of 25°C and a dew point temperature of -30°C. The scanning electron microscope (SEM) image of the positive electrode sheet obtained in this embodiment is shown below. Figure 4 As shown. By Figure 4 It can be seen that the positive electrode sheet prepared in this embodiment has intact single crystal particles, and no particles were crushed by rolling. Furthermore, no polycrystalline material was observed, indicating that the polycrystalline material was completely covered.
[0135] Example 4
[0136] The preparation method in this embodiment is basically the same as that in Example 1, except that: a single-crystal sodium nickel iron manganese aluminate (NaNi) is used. 3 / 10 Fe 1 / 3 Mn 1 / 3 Al1 / 30 O2) replaces monocrystalline sodium nickel manganate (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2), using polycrystalline sodium nickel iron manganese aluminum oxide (NaNi) 3 / 10 Fe 1 / 3 Mn 1 / 3 Al 1 / 30 O2) replaces polycrystalline sodium nickel manganese oxide (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2).
[0137] 1) Preparation of the first positive electrode slurry:
[0138] Based on mass percentage, 96% of the polycrystalline sodium nickel iron manganese aluminate (NaNi) 3 / 10 Fe 1 / 3 Mn 1 / 3 Al 1 / 30 O2) was dissolved in N-methylpyrrolidone (NMP) along with 2% conductive carbon black and 2% binder PVDF to form the first positive electrode slurry. The polycrystalline sodium nickel iron manganese aluminate had particle sizes D10 of 3 μm, D50 of 8 μm, and D90 of 17 μm, and its specific capacity at 2.0V~4.0V, measured using a coin cell, was 145 mAh / g. The preparation method of the third positive electrode slurry was the same as that of the first positive electrode slurry.
[0139] 2) Preparation of the second positive electrode slurry:
[0140] Based on mass percentage, 96% of the single-crystal sodium nickel iron manganese aluminate (NaNi) 3 / 10 Fe 1 / 3 Mn 1 / 3 Al 1 / 30 O2) is dissolved in N-methylpyrrolidone (NMP) along with 2% conductive carbon black and 2% binder PVDF to form the second positive electrode slurry. The monocrystalline sodium nickel iron manganese aluminate has a particle size of D10 of 3 μm, D50 of 9 μm, and D90 of 20 μm, and its specific capacity at 2.0V~4.0V, measured using a coin cell, is 123 mAh / g. The fourth positive electrode slurry is prepared using the same method as the second positive electrode slurry.
[0141] 3) Preparation of positive electrode sheet
[0142] The stirring paddle speed was controlled at 50 rpm, the dispersion wheel speed at 2500 rpm, and the stirring time at 180 min. The temperature of both the first and third positive electrode slurries was 40℃. The first and third positive electrode slurries were coated onto both sides of an aluminum foil and dried at 100℃. The surface density of both the first and third positive electrode active material layers was 7 mg / cm³.2 The surface density of both sides is 14 mg / cm³. 2 .
[0143] Subsequently, a second positive electrode slurry and a fourth positive electrode slurry were coated onto the surfaces of the first and third positive electrode active material layers, respectively, and dried at 110°C to form a single-crystal second positive electrode active material layer and a single-crystal fourth positive electrode active material layer on the surfaces of the first and third positive electrode active material layers, respectively. The areal density of both the second and fourth positive electrode active material layers is 8 mg / cm³. 2 The sum of the single-sided areal densities of the second and fourth positive electrode active material layers, i.e., the double-sided areal density, is 16 mg / cm³. 2 .
[0144] The conductive substrate with the positive electrode active material layer formed thereon is rolled to obtain the positive electrode sheet, while ensuring that the compaction density of the positive electrode sheet is 3.1 mg / cm³. 3 It should be noted that all processes in this embodiment were performed at an ambient temperature of 25°C and a dew point temperature of -30°C. The scanning electron microscope (SEM) image of the positive electrode sheet obtained in this embodiment is shown below. Figure 5 As shown. By Figure 5 It can be seen that the positive electrode sheet prepared in this embodiment has intact single crystal particles, and no particles were crushed by rolling. Furthermore, no polycrystalline material was observed, indicating that the polycrystalline material was completely covered.
[0145] Example 5
[0146] The preparation method in this embodiment is basically the same as that in Example 1, except that: a single-crystal sodium copper-nickel-iron-manganese oxide (NaCu) is used. 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2) replaces monocrystalline sodium nickel manganate (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2), using polycrystalline sodium copper-nickel-iron-manganese oxide (NaCu) 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2) replaces polycrystalline sodium nickel manganese oxide (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2).
[0147] 1) Preparation of the first positive electrode slurry:
[0148] Based on mass percentage, 96% of the polycrystalline sodium copper-nickel-iron-manganese oxide (NaCu) 1 / 9 Ni 2 / 9Fe 1 / 3 Mn 1 / 3 O2) was dissolved in N-methylpyrrolidone (NMP) along with 2% conductive carbon black and 2% binder PVDF to form the first positive electrode slurry. The polycrystalline sodium copper-nickel-iron-manganese oxide had particle sizes D10 of 2.5 μm, D50 of 7 μm, and D90 of 16 μm, and its specific capacity at 2.0V~4.0V, measured using a coin cell, was 146 mAh / g. The preparation method of the third positive electrode slurry was the same as that of the first positive electrode slurry.
[0149] 2) Preparation of the second positive electrode slurry:
[0150] Based on mass percentage, 96% of the single-crystal sodium copper-nickel-iron-manganese oxide (NaCu) 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2) is dissolved in N-methylpyrrolidone (NMP) along with 2% conductive carbon black and 2% binder PVDF to form the second positive electrode slurry. The single-crystal sodium copper-nickel-iron-manganese oxide has a particle size of D10 of 3 μm, D50 of 10 μm, and D90 of 22 μm, and its specific capacity at 2.0V~4.0V, measured using a coin cell, is 121 mAh / g. The fourth positive electrode slurry is prepared using the same method as the second positive electrode slurry.
[0151] 3) Preparation of positive electrode sheet
[0152] The stirring paddle speed was controlled at 50 rpm, the dispersion wheel speed at 2500 rpm, and the stirring time at 180 min. The temperature of both the first and third positive electrode slurries was 40℃. The first and third positive electrode slurries were coated onto both sides of an aluminum foil and dried at 100℃. The surface density of both the first and third positive electrode active material layers was 7 mg / cm³. 2 The surface density of both sides is 14 mg / cm³. 2 .
[0153] Subsequently, a second positive electrode slurry and a fourth positive electrode slurry were coated onto the surfaces of the first and third positive electrode active material layers, respectively, and dried at 110°C to form a single-crystal second positive electrode active material layer and a single-crystal fourth positive electrode active material layer on the surfaces of the first and third positive electrode active material layers, respectively. The areal density of both the second and fourth positive electrode active material layers is 8 mg / cm³. 2 The sum of the single-sided areal densities of the second and fourth positive electrode active material layers, i.e., the double-sided areal density, is 16 mg / cm³. 2 .
[0154] The conductive substrate with the positive electrode active material layer formed thereon is rolled to obtain the positive electrode sheet, while ensuring that the compaction density of the positive electrode sheet is 3.1 mg / cm³. 3 It should be noted that all processes in this embodiment were performed at an ambient temperature of 25°C and a dew point temperature of -30°C. The scanning electron microscope (SEM) image of the positive electrode sheet obtained in this embodiment is shown below. Figure 6 As shown. By Figure 6 It can be seen that the positive electrode sheet prepared in this embodiment has intact single crystal particles, and no particles were crushed by rolling. Furthermore, no polycrystalline material was observed, indicating that the polycrystalline material was completely covered.
[0155] Example 6
[0156] The preparation method of this embodiment is basically the same as that of Example 1, except that the positive electrode active material layer is formed only on one side of the aluminum foil.
[0157] Example 7
[0158] The preparation method of this embodiment is basically the same as that of Example 2, except that the positive electrode active material layer is formed only on one side of the aluminum foil.
[0159] Example 8
[0160] The preparation method of this embodiment is basically the same as that of Example 3, except that the positive electrode active material layer is formed only on one side of the aluminum foil.
[0161] Example 9
[0162] The preparation method of this embodiment is basically the same as that of Example 4, except that the positive electrode active material layer is formed only on one side of the aluminum foil.
[0163] Example 10
[0164] The preparation method of this embodiment is basically the same as that of embodiment 5, except that the positive electrode active material layer is formed only on one side of the aluminum foil.
[0165] Comparative Example 1
[0166] The preparation method of Comparative Example 1 is basically the same as that of Example 2, except that a single-crystal positive electrode active material layer is formed only on the surface of the aluminum foil. The specific steps are as follows:
[0167] 1) Preparation of the second positive electrode slurry:
[0168] Based on mass percentage, 96% of the single-crystal sodium nickel iron manganate (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3O2) is dissolved in N-methylpyrrolidone (NMP) along with 2% conductive carbon black and 2% binder PVDF to form the first positive electrode slurry. The monocrystalline sodium nickel iron manganese oxide has a particle size of D10 of 3 μm, D50 of 7.6 μm, and D90 of 17 μm, and its specific capacity at 2.0V~4.0V, measured using a coin cell, is 127 mAh / g. The fourth positive electrode slurry is prepared using the same method as the second positive electrode slurry.
[0169] 2) Preparation of positive electrode sheet
[0170] The stirring paddle speed was controlled at 50 rpm, the dispersion wheel speed at 2500 rpm, and the stirring time at 180 min. The temperatures of both the second and fourth positive electrode slurries were 40℃. The second and fourth positive electrode slurries were coated onto both sides of an aluminum foil and dried at 120℃ to form a single-crystal second and fourth positive electrode active material layer on the aluminum foil surface, respectively. The areal density of both the second and fourth positive electrode active material layers was 15 mg / cm³. 2 The sum of the single-sided areal densities of the second and fourth positive electrode active material layers, i.e., the double-sided areal density, is 30 mg / cm³. 2 .
[0171] The conductive substrate with the positive electrode active material layer formed thereon is rolled to obtain the positive electrode sheet, ensuring that the compaction density of the positive electrode sheet is 3.1 mg / cm³. 3 It should be noted that all processes in this comparative example were performed at an ambient temperature of 25°C and a dew point temperature of -30°C. The scanning electron microscope (SEM) image of the positive electrode sheet prepared in this comparative example is shown below. Figure 7 As shown. By Figure 7 It can be seen that the positive electrode sheet prepared in this comparative example has intact single crystal particles, and there is no phenomenon of particles being crushed by rolling.
[0172] Comparative Example 2
[0173] The preparation method of Comparative Example 2 is basically the same as that of Example 2, except that a polycrystalline positive electrode active material layer is formed only on the surface of the aluminum foil. The specific steps are as follows:
[0174] 1) Preparation of the first positive electrode slurry:
[0175] Based on mass percentage, 96% of polycrystalline sodium nickel iron manganate (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3O2) is dissolved in N-methylpyrrolidone (NMP) along with 2% conductive carbon black and 2% binder PVDF to form the second positive electrode slurry. The polycrystalline sodium nickel iron manganese oxide has particle sizes D10 of 4 μm, D50 of 9 μm, and D90 of 19 μm, and its specific capacity at 2.0V~4.0V, measured using a coin cell, is 140 mAh / g. The preparation method of the third positive electrode slurry is the same as that of the first positive electrode slurry.
[0176] 2) Preparation of positive electrode sheet
[0177] The stirring paddle speed was controlled at 50 rpm, the dispersion wheel speed at 2500 rpm, and the stirring time at 180 min. The temperatures of both the first and third positive electrode slurries were 40℃. The first and third positive electrode slurries were coated onto both sides of an aluminum foil and dried at 95℃ to form a polycrystalline first positive electrode active material layer and a polycrystalline third positive electrode active material layer on the aluminum foil surface, respectively. The areal density of both the first and third positive electrode active material layers was 15 mg / cm³. 2 The sum of the single-sided areal densities of the first and third positive electrode active material layers, i.e., the double-sided areal density, is 30 mg / cm³. 2 .
[0178] The conductive substrate with the positive electrode active material layer formed thereon is rolled to obtain the positive electrode sheet, while ensuring that the compaction density of the positive electrode sheet is 3.1 mg / cm³. 3 It should be noted that all processes in this comparative example were performed at an ambient temperature of 25°C and a dew point temperature of -30°C. The scanning electron microscope (SEM) image of the positive electrode sheet prepared in this comparative example is shown below. Figure 8 As shown. By Figure 8 It can be seen that the positive electrode sheet prepared in this comparative example shows that the material particles are crushed and broken.
[0179] Comparative Example 3
[0180] The preparation method of this comparative example is basically the same as that of comparative example 1, except that a single-crystal positive electrode active material layer is formed only on one side of the aluminum foil.
[0181] Comparative Example 4
[0182] The preparation methods of this comparative example are basically the same as those of comparative example 2, except that a polycrystalline positive electrode active material layer is formed only on one side of the aluminum foil.
[0183] The positive electrode sheets prepared in Examples 1-5 and Comparative Examples 1-2 were assembled to form a full cell (cylindrical 33138-8.5Ah), and the positive electrode sheets prepared in Examples 6-10 and Comparative Examples 3-4 were assembled to form a coin cell (CR2025). The capacity of the full cell and the coin cell were then tested. The capacity test results are shown in Table 1 below. The cycle performance of the full cell was tested, and the test results are as follows. Figure 9 As shown. By Figure 9 It is known that coating the surface of polycrystalline materials with monocrystalline materials can effectively protect the polycrystalline materials and significantly improve their cycle performance.
[0184] Table 1
[0185]
[0186] As shown in Table 1 above, the positive electrode sheet prepared in this application has a higher capacity compared to Comparative Example 1. Although the capacity of the positive electrode sheet prepared in this application is lower than that of Comparative Example 2, please refer to... Figure 9 As can be seen, the cycle performance of the positive electrode sheet prepared in this application is significantly higher than that of Comparative Example 2, indicating that it has higher cycle performance. Therefore, in summary, the positive electrode sheet prepared in this application has both high capacity and high cycle performance.
[0187] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0188] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims, and the specification can be used to interpret the scope of the claims.
Claims
1. A positive electrode sheet for a sodium-ion battery, characterized in that, It includes a conductive substrate and a first positive electrode active material layer and a second positive electrode active material layer sequentially formed on a first surface of the conductive substrate; The first positive electrode active material layer is composed of a polycrystalline layered oxide, and the second positive electrode active material layer is composed of a monocrystalline layered oxide. The second surface of the conductive substrate is sequentially formed with a third positive electrode active material layer and a fourth positive electrode active material layer; The material of the third positive electrode active material layer comprises a polycrystalline layered oxide, and the material of the fourth positive electrode active material layer comprises a monocrystalline layered oxide. The areal density of the first positive electrode active material layer and the third positive electrode active material layer is 5 mg / cm³. 2 ~15mg / cm 2 ; The areal density of the second positive electrode active material layer and the fourth positive electrode active material layer is 10 mg / cm³. 2 ~25mg / cm 2 .
2. The positive electrode sheet as described in claim 1, characterized in that, The chemical formulas of the polycrystalline layered oxide and the single-crystal layered oxide are independently Na. x Ni a Fe b Mn c M d O2, where 0<x≤1,a+b+c+d=1,a> 0, b>0, c>0, d≥0, M is one or more of Cu, Ti, Zr, Co, Zn, Mg, Al and Ca.
3. The positive electrode sheet as described in claim 1 or 2, characterized in that, It meets at least one of the following characteristics: 1) The polycrystalline layered oxide is a secondary particle, and the particle size of the polycrystalline layered oxide satisfies: D10 is 1μm~5μm, D50 is 5μm~10μm, and D90 is 15μm~25μm; in the secondary particles, the particle size of the primary particles is 50nm~500nm. 2) The single-crystal layered oxide is a primary particle, and the particle size of the single-crystal layered oxide satisfies: D10 is 1μm~3μm, D50 is 3μm~15μm, and D90 is 15μm~25μm; 3) The compacted density of the positive electrode sheet is 2.8 mg / cm³. 3 ~3.3mg / cm 3 .
4. The method for preparing the positive electrode sheet according to any one of claims 1 to 3, characterized in that, Includes the following steps: The first positive electrode active material layer and the second positive electrode active material layer are sequentially formed on the first surface of the conductive substrate; The third positive electrode active material layer and the fourth positive electrode active material layer are sequentially formed on the second surface of the conductive substrate; the positive electrode sheet is then prepared.
5. The preparation method according to claim 4, characterized in that, The method for forming the first positive electrode active material layer, the second positive electrode active material layer, the third positive electrode active material layer, and the fourth positive electrode active material layer includes: The first positive electrode slurry is coated onto the first surface of the conductive substrate to form the first positive electrode active material layer; A second positive electrode slurry is coated on the side of the first positive electrode active material layer that is away from the first surface of the conductive substrate to form the second positive electrode active material layer; The third positive electrode slurry is coated onto the second surface of the conductive substrate to form the third positive electrode active material layer; A fourth positive electrode slurry is coated on the side of the third positive electrode active material layer that is opposite to the second surface of the conductive substrate to form the fourth positive electrode active material layer.
6. The preparation method according to claim 5, characterized in that, The first positive electrode slurry and the third positive electrode slurry comprise: a polycrystalline layered oxide, a first conductive agent, a first binder, and a first solvent; The second positive electrode slurry and the fourth positive electrode slurry comprise: a single-crystal layered oxide, a second conductive agent, a second binder, and a second solvent; Optionally, the first conductive agent and the second conductive agent each independently include one or more of conductive carbon black, conductive graphite, carbon fiber, carbon nanotubes and graphene; Optionally, the first adhesive and the second adhesive are each independently polyvinylidene fluoride; Optionally, the first solvent and the second solvent are each independently N-methylpyrrolidone.
7. The preparation method according to any one of claims 4 to 6, characterized in that, It also includes pressing the positive electrode sheet to achieve a compaction density of 2.8 mg / cm³. 3 ~3.3mg / cm 3 The steps.
8. A sodium-ion battery, characterized in that, Includes the positive electrode sheet as described in any one of claims 1 to 3.
Citation Information
Patent Citations
Monocrystalline sodium ion battery positive electrode material, preparation method thereof and battery
CN115275178A
Positive pole piece, energy storage device and electric equipment
CN116053408A
Electrode plate, secondary battery and terminal equipment
CN116895741A