Surface halogen-functionalized low-dimensional bismuth nanomaterials, their preparation methods, and applications
The surface halogen-functionalized low-dimensional bismuth nanomaterials were prepared by electrochemical exfoliation, which solved the problem of instability of low-dimensional bismuth nanomaterials in air and achieved high stability and excellent electrochemical performance of the materials.
Patent Information
- Application Number
- CN202311675177.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-08
AI Technical Summary
Low-dimensional bismuth nanomaterials are unstable in air and are easily oxidized into oxides, which limits their applications.
Low-dimensional bismuth nanomaterials with surface halogen functionalization were prepared by electrochemical exfoliation. The surface of the bismuth nanomaterials was halogenated by electrolysis of tetraalkylammonium halide solution, which improved their stability in air.
It effectively prevents bismuth nanomaterials from being oxidized in air, exhibiting excellent stability and superior electrochemical performance.
Smart Images

Figure CN117655342B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of new materials and energy storage, and in particular to a surface halogen-functionalized low-dimensional bismuth nanomaterial, its preparation method, and its applications. Background Technology
[0002] Due to their unique physicochemical properties, low-dimensional (zero-dimensional, one-dimensional, and two-dimensional) semiconductor or semi-metallic nanomaterials (such as antimony quantum dots, phosphorene, arsene, antimonene, and bismuthene) have important applications in semiconductors, optoelectronic devices, biosensors, catalysis, energy conversion, and storage. However, because these low-dimensional materials are extremely small in size, they are very unstable in air after preparation and are easily oxidized into oxides by atmospheric oxygen, thus limiting their applications. The same applies to bismuth low-dimensional materials such as bismuthene and bismuth nanoparticles; they are also easily oxidized into oxides in air, further restricting their applications.
[0003] In view of this, the present invention is hereby proposed. Summary of the Invention
[0004] One of the objectives of this invention is to provide a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials, which is simple and easy to operate, and enables the low-dimensional bismuth nanomaterials to have excellent stability in air.
[0005] The second objective of this invention is to provide a surface halogen-functionalized low-dimensional bismuth nanomaterial that exhibits excellent stability in air and superior electrochemical performance.
[0006] The third objective of this invention is to provide an application of surface halogen-functionalized low-dimensional bismuth nanomaterials, which can improve electrochemical performance and has outstanding application effects.
[0007] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted:
[0008] In a first aspect, a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials includes the following steps:
[0009] (a) Bismuth metal rods and platinum sheets are used as cathode and anode respectively for electrolysis to obtain bismuth nanomaterials generated by the cathode and halogen molecules generated by the anode;
[0010] The electrolyte for electrolysis is selected from a tetraalkylammonium halide organic solution;
[0011] (b) The bismuth nanomaterials generated by the cathode and the halogen molecules generated by the anode obtained in step (a) are mixed and left to stand to obtain the surface halogen functionalized low-dimensional bismuth nanomaterials.
[0012] Furthermore, in step (a), the electrolytic cell for electrolysis includes an H-type sand core electrolytic cell.
[0013] Furthermore, the tetraalkylammonium halide includes at least one of tetraalkylammonium chloride, tetraalkylammonium bromide, and tetraalkylammonium iodide.
[0014] Furthermore, the tetraalkylammonium halide includes at least one of tetramethylammonium chloride, tetraethylammonium chloride, tetrapropylammonium chloride, tetrabutylammonium chloride, tetraheptylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, tetrapropylammonium bromide, tetrabutylammonium bromide, tetraheptylammonium bromide, tetramethylammonium iodide, tetraethylammonium iodide, tetrapropylammonium iodide, tetrabutylammonium iodide, and tetraheptylammonium iodide.
[0015] Furthermore, in step (a), the concentration of the tetraalkylammonium halide organic solution is 0.05–2 mol / L.
[0016] Furthermore, in step (a), the cathode potential applied during electrolysis is -3 to -30V.
[0017] Furthermore, in step (a), the halogen molecules generated by the anode include at least one of Cl2, Br2, and I2.
[0018] Furthermore, in step (b), the settling time is 5 minutes to 2 hours.
[0019] Secondly, a surface halogen-functionalized low-dimensional bismuth nanomaterial prepared by any of the above preparation methods.
[0020] Thirdly, the application of the aforementioned surface halogen-functionalized low-dimensional bismuth nanomaterial in sodium-ion battery anode materials.
[0021] Compared with the prior art, the present invention has at least the following beneficial effects:
[0022] The present invention provides a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The method involves electrochemical exfoliation to prepare bismuth nanomaterials. After electrolysis begins, quaternary ammonium salt cations in the electrolyte insert into the interlayer of metallic bismuth under the influence of the cathode potential, thereby disrupting the interlayer forces and causing the bismuth electrode to be gradually exfoliated, generating black bismuth nanomaterials. Simultaneously, halogen ions in the electrolyte around the anode are oxidized to generate halogen molecules. After electrolysis, the halogen molecules generated near the anode and the bismuth nanomaterials generated in the cathode region are mixed and allowed to react statically to halogenate the surface of the bismuth nanomaterials, thus obtaining surface halogen-functionalized low-dimensional bismuth nanomaterials, which effectively improves their stability in air.
[0023] The surface halogenated low-dimensional bismuth nanomaterials provided by this invention can effectively prevent bismuth nanomaterials from being oxidized in air due to their surface halogenation, thus exhibiting excellent stability and good electrochemical performance.
[0024] The application of the surface halogen-functionalized low-dimensional bismuth nanomaterials provided by this invention can improve electrochemical performance and has outstanding application effects. Attached Figure Description
[0025] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0026] Figure 1 This is a TEM image of the Bi-ene-Cl material provided in Embodiment 1 of the present invention;
[0027] Figure 2 The Bi-ene-Cl material provided in Example 1 of this invention and its XRD pattern after being placed at room temperature for 90 days;
[0028] Figure 3 The high-resolution XPS spectrum of Cl2p of the Bi-ene-Cl material provided in Example 1 of this invention;
[0029] Figure 4 This is a TEM image of the surface halogen-functionalized low-dimensional bismuth nanomaterial provided in Example 2 of the present invention.
[0030] Figure 5 This is a TEM image of the surface halogen-functionalized low-dimensional bismuth nanomaterial provided in Example 3 of the present invention.
[0031] Figure 6 This is a TEM image of the bismuthene product provided in Comparative Example 1 of the present invention.
[0032] Figure 7 The image shows the bismuthene product provided in Comparative Example 1 of this invention and its XRD pattern after being placed at room temperature for seven days.
[0033] Figure 8 These are charge-discharge curves at different rates obtained from the experimental examples of this invention.
[0034] Figure 9 This is a graph showing the cycle performance obtained from the experimental examples of this invention. Detailed Implementation
[0035] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0036] According to a first aspect of the present invention, a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials is provided, comprising the following steps:
[0037] (a) Bismuth metal rods and platinum sheets are used as cathode and anode respectively for electrolysis to obtain bismuth nanomaterials generated by the cathode and halogen molecules generated by the anode;
[0038] The electrolyte for electrolysis can be selected from a tetraalkylammonium halide organic solution;
[0039] (b) The bismuth nanomaterials generated from the cathode and the halogen molecules generated from the anode obtained in step (a) are mixed and left to stand to obtain surface halogen-functionalized low-dimensional bismuth nanomaterials.
[0040] The present invention provides a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The method involves electrochemical exfoliation to prepare bismuth nanomaterials. After electrolysis begins, quaternary ammonium salt cations in the electrolyte insert into the interlayer of metallic bismuth under the influence of the cathode potential, thereby disrupting the interlayer forces and causing the bismuth electrode to be gradually exfoliated, generating black bismuth nanomaterials. Simultaneously, halogen ions in the electrolyte around the anode are oxidized to generate halogen molecules. After electrolysis, the halogen molecules generated near the anode and the bismuth nanomaterials generated in the cathode region are mixed and allowed to react statically to halogenate the surface of the bismuth nanomaterials, thus obtaining surface halogen-functionalized low-dimensional bismuth nanomaterials, which effectively improves their stability in air.
[0041] In a preferred embodiment, in step (a), the electrolytic cell used for electrolysis includes, but is not limited to, an H-type sand core electrolytic cell, which is more conducive to further improving the reaction effect of electrolysis.
[0042] In a preferred embodiment, the tetraalkylammonium halide includes, but is not limited to, at least one of tetraalkylammonium chloride, tetraalkylammonium bromide and tetraalkylammonium iodide, which is more conducive to the gradual stripping of the bismuth metal rod (i.e., bismuth electrode) to generate bismuth nanomaterials, and is also more conducive to the oxidation of halide ions in the electrolyte into halogen molecules (e.g., they can be oxidized into at least one of Cl2, Br2 and I2, but are not limited thereto).
[0043] In this invention, bismuth nanomaterials are prepared by electrochemical exfoliation. Depending on the difference in the alkyl chain length of the quaternary ammonium salt, the obtained material is either bismuth nanoparticles or two-dimensional bismuthene. At the same time, by controlling the reaction time between the bismuth nanomaterials and the halogen molecules generated by electrolysis, the surface of the bismuth nanomaterials can be halogenated, thereby improving its stability in air and making it less prone to oxidation.
[0044] In a preferred embodiment, the tetraalkylammonium halide includes, but is not limited to, at least one of tetramethylammonium chloride, tetraethylammonium chloride, tetrapropylammonium chloride, tetrabutylammonium chloride, tetraheptylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, tetrapropylammonium bromide, tetrabutylammonium bromide, tetraheptylammonium bromide, tetramethylammonium iodide, tetraethylammonium iodide, tetrapropylammonium iodide, tetrabutylammonium iodide, and tetraheptylammonium iodide.
[0045] In a preferred embodiment, in step (a), the concentration of the tetraalkylammonium halide organic solution can be 0.05 to 2 mol / L, with typical but non-limiting concentrations such as 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, and 2 mol / L.
[0046] In this invention, a suitable concentration of the tetraalkylammonium halide organic solution is more conducive to further improving the effect of bismuth metal exfoliation into bismuth nanomaterials and surface halogen functionalization. If the concentration of the tetraalkylammonium halide organic solution is too high, it will result in nanoparticles that are too large or two-dimensional bismuthene that is too thick. If the concentration of the tetraalkylammonium halide organic solution is too low, it will result in bismuth metal exfoliation speed that is too slow and surface halogen functionalization degree that is too low.
[0047] In a preferred embodiment, in step (a), the cathode potential applied to the bismuth metal rod during electrolysis can be -3 to -30V, with typical but non-limiting cathode potentials being, for example, -3V, -4V, -5V, -10V, -15V, -20V, -25V, and -30V.
[0048] In this invention, a suitable cathode potential is more conducive to the gradual and controllable stripping of bismuth metal into bismuth nanomaterials; if the cathode potential is too high, some bismuth metal will not be completely stripped; if the cathode potential is too low, the reaction rate will be too slow.
[0049] After electrolysis, the products (halogen molecules) near the anode and the electrolyte (containing bismuth nanomaterials) in the cathode region can be transferred to the same beaker for mixing. After standing for a while, the surface of the bismuth nanomaterials can be halogenated. Then, it can be washed with ethanol, followed by ultrasonic dispersion and centrifugation, and then washed and vacuum dried to obtain surface halogen-functionalized low-dimensional bismuth nanomaterials.
[0050] In this invention, by controlling the static reaction time of bismuth nanomaterials with halogen molecules generated by electrolysis, the surface of bismuth nanomaterials can be halogenated, thereby improving their stability in air.
[0051] In a preferred embodiment, in step (b), the settling time can be from 5 min to 2 h, with typical but non-limiting times such as 5 min, 10 min, 20 min, 30 min, 40 min, 50 min, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, and 2 h. This is more conducive to fully halogenating the surface of the bismuth nanomaterial to maximize its stability in air. If the settling time is too short, the degree of surface halogen functionalization will be too low; if the settling time is too long, the production efficiency will be reduced.
[0052] According to a second aspect of the present invention, a surface halogen-functionalized low-dimensional bismuth nanomaterial prepared by any of the above-described preparation methods is provided.
[0053] The surface halogenated low-dimensional bismuth nanomaterials provided by this invention can effectively prevent bismuth nanomaterials from being oxidized in air due to their surface halogenation, thus exhibiting excellent stability and good electrochemical performance.
[0054] According to a third aspect of the present invention, an application of the surface halogen-functionalized low-dimensional bismuth nanomaterials described above in sodium-ion battery anode materials is provided.
[0055] The application provided by this invention, that surface halogen-functionalized low-dimensional bismuth nanomaterials are used as anode materials for sodium-ion batteries, can achieve good electrochemical performance and has outstanding application effects.
[0056] The present invention will be further illustrated below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or purchased directly from the market.
[0057] Example 1
[0058] A method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials includes the following steps:
[0059] (a) Using an H-type sand core electrolytic cell as the electrolytic cell, with a bismuth metal rod and a platinum sheet electrode as the cathode and anode respectively, and a 0.2 mol / L tetraethylammonium chloride N,N-dimethylformamide solution as the electrolyte, electrolysis was carried out for 2 hours. The cathode potential applied to the bismuth metal rod was -5V. The bismuth electrode at the cathode gradually dispersed into black bismuth nanomaterials, and the electrolyte around the anode gradually turned light green. Bismuth nanomaterials generated at the cathode and halogen molecules generated at the anode were obtained.
[0060] (b) After electrolysis, the electrolyte and precipitate in the anode and cathode regions are transferred to the same beaker for mixing and allowed to stand for 10 min. The surface of the bismuth nanomaterial is chlorinated, then washed with ethanol, ultrasonically dispersed for 3 min, centrifuged at 8000 r / min, washed with ethanol 6 times, and then vacuum dried at 60 °C for 8 h to obtain the surface-chlorinated bismuthene (which can be denoted as Bi-ene-Cl), which is the surface halogen-functionalized low-dimensional bismuth nanomaterial.
[0061] The TEM image of the Bi-ene-Cl material in this embodiment is shown below. Figure 1 ,Depend on Figure 1 As can be seen, the Bi-ene-Cl material synthesized in this embodiment has a layered structure; meanwhile, the XRD pattern of the Bi-ene-Cl material synthesized in this embodiment and its XRD pattern after being placed at room temperature for 90 days are shown below. Figure 2 ,from Figure 2 As can be seen from the image, the newly synthesized Bi-ene-C material is in the phase of hexagonal bismuth. After being placed at room temperature for 90 days, its phase did not change and remained hexagonal bismuth, indicating that the Bi-ene-Cl material is very stable. The high-resolution XPS spectrum of the Cl2p of the Bi-ene-Cl material in this embodiment is shown in the image. Figure 3 The figure shows Cl - The chemical states of ions are inorganic and two types of Cl in organic compounds. - The inorganic Cl- - The content was 71%, indicating that Bi-Cl bonds had been formed on the bismuth surface, confirming the successful synthesis of surface-chlorinated bismuthene materials.
[0062] Example 2
[0063] This embodiment provides a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The difference from Example 1 is that in step (a) of this embodiment, tetrabutylammonium chloride is used instead of tetraethylammonium chloride in Example 1. The remaining steps and process parameters are the same as in Example 1, yielding surface halogen-functionalized low-dimensional bismuth nanomaterials, the morphology of which is shown in […]. Figure 4 It can be seen that it is granular.
[0064] Example 3
[0065] This embodiment provides a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The difference from Example 1 is that in step (a) of this embodiment, tetraethylammonium bromide is used instead of tetraethylammonium chloride in Example 1. The remaining steps and process parameters are the same as in Example 1, yielding surface halogen-functionalized low-dimensional bismuth nanomaterials, the morphology of which is shown in [see attached image]. Figure 5 It can be seen that it has a two-dimensional layered bismuthene structure.
[0066] Examples 4-6
[0067] Examples 4-6 provide a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The difference from Example 1 is that in step (a) of Examples 4-6, tetramethylammonium chloride, tetrabutylammonium bromide and tetraethylammonium iodide are used to replace tetraethylammonium chloride in Example 1, respectively. The remaining steps and process parameters are the same as in Example 1, and surface halogen-functionalized low-dimensional bismuth nanomaterials are obtained.
[0068] Examples 7-9
[0069] Examples 7-9 provide a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The difference from Example 1 is that the concentration of the electrolyte in step (a) of Examples 7-9 is 0.05 mol / L, 1 mol / L and 2 mol / L, respectively. The remaining steps and process parameters are the same as those in Example 1, and surface halogen-functionalized low-dimensional bismuth nanomaterials are obtained.
[0070] Examples 10-12
[0071] Examples 10-12 provide a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The difference from Example 1 is that the cathode potentials applied to the bismuth metal rod in step (a) of Examples 10-12 are -3V, -16V and -30V, respectively. The remaining steps and process parameters are the same as those in Example 1, and surface halogen-functionalized low-dimensional bismuth nanomaterials are obtained.
[0072] Examples 13-15
[0073] Examples 13-15 provide a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The difference from Example 1 is that the standing time in step (b) of Examples 13-15 is 5 min, 1 h and 2 h respectively. The remaining steps and process parameters are the same as those in Example 1, and surface halogen-functionalized low-dimensional bismuth nanomaterials are obtained.
[0074] Comparative Example 1
[0075] This comparative example provides a method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials. The difference from Example 1 is that in step (a) of this comparative example, tetraethylammonium hexafluorophosphate is used instead of tetraethylammonium chloride in Example 1. The remaining steps and process parameters are the same as in Example 1, and bismuthene products are obtained.
[0076] In this comparative example, because the hexafluorophosphate anion is relatively stable, although the reaction phenomenon of the bismuth cathode during electrolysis is similar to that in Example 1, the color of the electrolyte around the anode does not change. The morphology of the resulting product is shown in the figure. Figure 6 It can be seen that it also has a two-dimensional layered bismuthene structure; the XRD pattern of the product synthesized in this comparative example and its XRD pattern after being placed at room temperature for seven days are shown in the figure. Figure 7 By comparing with the standard card of Bi2O2CO3 (JCPDS No. 41-1488), it was found that the phase of the newly synthesized product was hexagonal metallic bismuth. After being placed at room temperature for seven days, the characteristic diffraction peaks of hexagonal metallic bismuth disappeared and all changed to the characteristic peaks of Bi2O2CO3. This indicates that the surface of the bismuthene material synthesized in this comparative example is not functionalized, so it is unstable in air and easily turns into oxide.
[0077] Test case
[0078] The Bi-ene-Cl material obtained in Example 1 was mixed with the binder polyvinylidene fluoride (PVDF) and the conductive agent in a mass ratio of 8:1:1 using nitrogen-methylpyrrolidone to form an electrode slurry, which was then stirred and mixed evenly. The electrode slurry was then coated onto a copper foil and dried under vacuum at 60°C to obtain an electrode sheet.
[0079] A CR2025 coin cell was assembled using a sodium sheet as the counter electrode and 1 mol / L NaPF6EC+DMC+5% FEC as the electrolyte for testing. The test voltage range was 1.5–0.01 V.
[0080] Figure 8 The charge-discharge curves are shown at different rates. At 0.1, 0.2, 0.5, 1, and 2 A / g, the specific capacity of the Bi-ene-Cl electrode reaches 327, 281, 241, 224, and 208 mAh / g, respectively.
[0081] Figure 9 The cycling performance curve is shown at 1A / g. After 1000 charge-discharge cycles, the capacity retention rate is 85.9%, demonstrating excellent cycle stability.
[0082] The materials (products) obtained in Examples 2-15 and Comparative Example 1 were tested using the same methods described above, and the results are shown in Table 1.
[0083]
[0084] Table 1
[0085] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing surface halogen-functionalized low-dimensional bismuth nanomaterials, characterized in that, Includes the following steps: (a) Bismuth metal rods and platinum sheets are used as cathode and anode respectively for electrolysis to obtain bismuth nanomaterials generated by the cathode and halogen molecules generated by the anode; The electrolyte for electrolysis is selected from a tetraalkylammonium halide organic solution; The electrolytic cell used for electrolysis is an H-type sand core electrolytic cell; (b) The bismuth nanomaterials generated by the cathode and the halogen molecules generated by the anode obtained in step (a) are mixed and left to stand to obtain the surface halogen functionalized low-dimensional bismuth nanomaterials.
2. The preparation method according to claim 1, characterized in that, The tetraalkyl ammonium halide includes at least one of tetraalkyl ammonium chloride, tetraalkyl ammonium bromide, and tetraalkyl ammonium iodide.
3. The preparation method according to claim 2, characterized in that, The tetraalkylammonium halide includes at least one of tetramethylammonium chloride, tetraethylammonium chloride, tetrapropylammonium chloride, tetrabutylammonium chloride, tetraheptylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, tetrapropylammonium bromide, tetrabutylammonium bromide, tetraheptylammonium bromide, tetramethylammonium iodide, tetraethylammonium iodide, tetrapropylammonium iodide, tetrabutylammonium iodide, and tetraheptylammonium iodide.
4. The preparation method according to claim 1, characterized in that, In step (a), the concentration of the tetraalkylammonium halide organic solution is 0.05~2 mol / L.
5. The preparation method according to claim 4, characterized in that, In step (a), the cathode potential applied during electrolysis is -3 to -30V.
6. The preparation method according to claim 1, characterized in that, In step (a), the halogen molecules generated by the anode include at least one of Cl2, Br2 and I2.
7. The preparation method according to claim 1, characterized in that, In step (b), the settling time is 5 min to 2 h.
8. A surface halogen-functionalized low-dimensional bismuth nanomaterial prepared by the preparation method according to any one of claims 1-7.
9. The application of the surface halogen-functionalized low-dimensional bismuth nanomaterial according to claim 8 in sodium-ion battery anode materials.
Citation Information
Patent Citations
Method for preparing bismuth oxyhalide nanosheets by electrochemical method
CN111701603A
Photocatalyst as well as preparation method and application thereof
CN111744508A