Forming method of large valve body forging for nuclear power

By employing upsetting, drawing deformation, and finishing processes, the forming challenges of large valve body forgings for nuclear power plants have been solved, enabling precise control of complex shapes and improved grain size, thereby reducing manufacturing costs.

CN117696826BActive Publication Date: 2026-05-29GUIZHOU AEROSPACE XINLI CASTINGSAND FORGINGS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311813665.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-05-29
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

The conformal forging of large valve body forgings for nuclear power plants is difficult to form, involves multiple deformation forging processes, has small local deformation, is prone to cracking, and the coarse grain of X6CrNiTi18-10 stainless steel makes it difficult to meet the grain size requirements.

Method used

It is manufactured using square solid blanks with grain refinement through upsetting and drawing deformation. The pre-formed round cross-sections at both ends are formed by drawing octagons and upsetting deformation, combined with punching and finishing. The initial forging temperature and holding time are controlled to ensure that the grain size reaches grade 5.5.

Benefits of technology

It enables precise forming of complex-shaped forgings, solves the problems of uneven local deformation and cracking, improves material utilization and forming quality, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117696826B_ABST
    Figure CN117696826B_ABST
Patent Text Reader

Abstract

The application discloses a forming method of a large valve body forging for nuclear power, which comprises the following steps: S1, selecting a blank, performing upsetting and elongation deformation, refining the grain structure of the forging, and obtaining a square solid blank; S2, heating the square solid blank in S1 by re-melting, and deforming the two end portions from a square surface into a circular cross section after heat preservation; the initial forging temperature is 1100±20 DEG C, the heat preservation time is calculated according to the thickness of the square solid blank when entering the furnace, and is 0.2-0.4 min / mm, and the final forging temperature needs to be greater than 850 DEG C; S3, heating and heat preserving the forging after processing in S2 by a reversing furnace, and then performing the next fire forging; the initial forging temperature is 1080±20 DEG C, the heat preservation time is calculated according to the thickness of the blank when entering the furnace, and is 0.2-0.4 min / mm; the final forging temperature needs to be greater than 850 DEG C; and in the finishing forming process, the middle square cross section part is elongated to the size of the forging first, and then the two circular cross section parts are respectively rolled and elongated to the size of the forging. The scheme solves the problem of coarse grains of the profiled forging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of forging technology, and more specifically to a method for forming large valve body forgings for nuclear power plants. Background Technology

[0002] Large valve body forgings made of X6CrNiTi18-10 material for nuclear power projects. The forging shape is a hollow circular cross-section at both ends and a square outer and circular inner cross-section in the middle. See the product illustration. Figure 1 The performance indicators of this forging must meet the standard requirements, including a grain size requirement of not less than level 4.

[0003] Valve bodies have complex shapes, and to improve material utilization, reduce machining removal, and lower manufacturing costs, they are often designed as conformal forgings. However, conformal forgings are characterized by high forming difficulty, multiple deformation processes, and small local deformation. The forming process needs to address challenges such as large dimensional allowances, irregular shapes and easy cracking when forming rounded ends, and coarse grains in X6CrNiTi18-10 stainless steel. Summary of the Invention

[0004] The present invention aims to provide a forming method for large valve body forgings for nuclear power plants, in order to solve the problem of coarse grains in current conformal forgings.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for forming a large valve body forging for nuclear power plants, comprising the following steps:

[0006] S1, manufacturing of square solid billets: Select stainless steel material with chemical composition that meets the standards as billet, perform upsetting and drawing deformation to refine the grain structure of the forging and obtain square solid billets; the initial forging temperature is 1180±20℃, and the holding time is calculated according to the thickness of the billet entering the furnace at 0.6~1min / mm; the final forging temperature must be greater than 850℃;

[0007] S2, pre-forming with rounded cross-sections at both ends: The square solid billet in S1 is returned to the furnace for heating, and after holding at the temperature, the two ends are deformed from square surfaces into rounded cross-sections; Initial forging temperature: reduced to 1100±20℃, grain growth is not obvious; Holding time: calculated according to the thickness of the square solid billet when it enters the furnace, at 0.2~0.4min / mm; the final forging temperature must be greater than 850℃.

[0008] S3, finishing and forming: After the forgings processed in S2 are heated and held in the furnace, they are forged for the next forging. The initial forging temperature is 1080±20℃, and the holding time is calculated according to the thickness of the billet when it enters the furnace, at 0.2~0.4min / mm. The final forging temperature must be greater than 850℃. During the finishing and forming process, the square section in the middle section is first drawn to the size of the forging, and then the two round sections are rolled and drawn to the size of the forging.

[0009] Furthermore, when manufacturing the square solid blank in S1, an allowance of 15% to 20% is added to the square cross-sectional dimensions based on the size of the square solid blank.

[0010] Furthermore, during the deformation process of S2, the material at both ends is drawn into an octagon. After the two square sections are deformed into octagons, the end faces are petal-shaped because there is more material at the diagonal positions than at the other sides. Then, one octagonal section is inserted into a circular cavity placed on the lower anvil, and the other circular cavity is placed at the upper octagonal section. Then, upsetting deformation is performed to make the ends of the forging flush, and the material fills the upper and lower circular cavities. The conical section has a regular shape, and its size is controlled by the cavity. A 5% to 10% allowance is reserved based on the forging size. Then, a punch is used to punch holes to obtain a forging with a shape that meets the requirements, with two circular ends and a square hollow middle section.

[0011] Furthermore, during heat preservation in S1, the heat preservation time is calculated based on the thickness of the blank entering the furnace at 0.8 min / mm.

[0012] Furthermore, during heat preservation in S2, the heat preservation time is calculated based on the thickness of the square solid blank when it enters the furnace, at a rate of 0.3 min / mm.

[0013] The beneficial effects of this invention are:

[0014] 1. By pre-setting a 10%–20% allowance for the square cross-section in the first step, and a 5%–10% allowance in the second step, while controlling the initial forging temperature in the second step at 1100℃±20℃ and the initial forging temperature in the third step at 1080℃±20℃, the grain size of the forging can reach approximately grade 5.5. Without adjusting the initial forging temperature and deformation amount, it is difficult to achieve grade 4 grain size. This method achieves effective control of the grain structure of valve body forgings with multiple forging cycles and small deformation amounts.

[0015] 2. By designing a forming process scheme of forging a square section billet - drawing octagons at both ends - upsetting using upper and lower circular ring tooling - punching - finishing, the petal-shaped end and folding cracking caused by the deformation of the square section at both ends into a circular section are solved, and the shape and size of the conformal forging are precisely controlled. Attached Figure Description

[0016] Figure 1 The images show a sectional view and a top view of a large valve body forging in the background art.

[0017] Figure 2 This is a schematic diagram of the forging structure after upsetting in the embodiment;

[0018] Figure 3 This is a schematic diagram of the forging structure after punching in the embodiment. Detailed Implementation

[0019] Example 1

[0020] A method for forming a large valve body forging for nuclear power plants includes the following steps:

[0021] S1, Manufacturing of Square Solid Billet: Select stainless steel material with chemical composition conforming to the standard as billet, perform upsetting and drawing deformation to refine the grain structure of the forging, and obtain a square solid billet. Based on the size of the square solid billet, add a 15% allowance to the square cross-sectional dimensions; the initial forging temperature is 1160℃, and the holding time is calculated based on the thickness of the billet entering the furnace at 0.6min / mm; the final forging temperature must be greater than 850℃.

[0022] S2, pre-forming of rounded sections at both ends: The square solid billet from S1 is returned to the furnace for heating. After holding at the temperature, the material at both ends is drawn into octagons. At this point, after the two square sections are deformed into octagons, the end faces are petal-shaped because there is more material at the diagonal positions than at the other sides. Then, one octagonal section is inserted into a circular cavity placed on the lower anvil, and the other circular cavity is placed at the upper octagonal section. Then, upsetting deformation is performed to make the ends of the forging flush, and the material fills the upper and lower circular cavities. The conical section has a regular shape, and the size is controlled by the cavity. A 5% allowance is reserved based on the forging size. Then, a punch is used to punch holes to obtain a forging with rounded ends and a square hollow middle section that meets the required shape. Initial forging temperature: reduced to 1080℃, grain growth is not obvious. Holding time: calculated at 0.2min / mm based on the thickness of the square solid billet when entering the furnace. The final forging temperature must be greater than 850℃.

[0023] S3, finishing and forming: After the forgings processed in S2 are reheated and held in the furnace, they are forged for the next heat. The initial forging temperature is 1060℃, and the holding time is calculated at 0.2min / mm based on the thickness of the billet when it enters the furnace. The final forging temperature must be greater than 850℃. During the finishing and forming process, the square section in the middle is first drawn to the size of the forging, and then the two round sections are rolled and drawn to the size of the forging.

[0024] Example 2

[0025] A method for forming a large valve body forging for nuclear power plants includes the following steps:

[0026] S1, Manufacturing of Square Solid Billet: Select stainless steel material with chemical composition that meets the standards as billet, perform upsetting and drawing deformation to refine the grain structure of the forging, and obtain a square solid billet. Based on the size of the square solid billet, add a 20% allowance to the square cross-sectional dimensions; the initial forging temperature is 1200℃, and the holding time is calculated based on the thickness of the billet entering the furnace at 1min / mm; the final forging temperature must be greater than 850℃.

[0027] S2, pre-forming of rounded sections at both ends: The square solid billet from S1 is returned to the furnace for heating. After holding at that temperature, the material at both ends is drawn into octagons. At this point, after the two square sections are deformed into octagons, the end faces are petal-shaped because there is more material at the diagonal positions than at the other sides. Then, one octagonal section is inserted into a circular cavity placed on the lower anvil, and the other circular cavity is placed at the upper octagonal section. Then, upsetting deformation is performed to make the ends of the forging flush, and the material fills the upper and lower circular cavities. The conical section has a regular shape, and its size is controlled by the cavity. A 10% allowance is reserved based on the forging size. Then, a punch is used to punch holes to obtain a forging with rounded ends and a square hollow middle section that meets the required shape. Initial forging temperature: reduced to 1120℃, grain growth is not obvious. Holding time: calculated at 0.4min / mm based on the thickness of the square solid billet when it enters the furnace. The final forging temperature needs to be greater than 850℃.

[0028] S3, finishing and forming: After the forgings processed in S2 are heated and held in the furnace, they are forged for the next heat. The initial forging temperature is 1100℃, and the holding time is calculated at 0.4min / mm based on the thickness of the billet when it enters the furnace. The final forging temperature must be greater than 850℃. During the finishing and forming process, the square section in the middle is first drawn to the size of the forging, and then the two round sections are rolled and drawn to the size of the forging.

[0029] Example 3

[0030] A method for forming a large valve body forging for nuclear power plants includes the following steps:

[0031] S1, Manufacturing of Square Solid Billet: Select stainless steel material with chemical composition conforming to the standard as billet, perform upsetting and drawing deformation to refine the grain structure of the forging, and obtain a square solid billet. Based on the size of the square solid billet, add an 18% allowance to the square cross-sectional dimensions; the initial forging temperature is 1190℃, and the holding time is calculated based on the thickness of the billet entering the furnace at 0.8min / mm; the final forging temperature must be greater than 850℃.

[0032] S2, pre-forming of circular cross-sections at both ends: The square solid billet from S1 is reheated in the furnace. After holding at that temperature, the material at both ends is drawn into octagons. At this point, after the two square cross-sections are deformed into octagons, the end faces are petal-shaped because there is more material at the diagonal positions than at the other sides. Then, one octagonal segment is inserted into a circular cavity placed on the lower anvil, and the other circular cavity is placed at the upper octagonal segment. Then, upsetting deformation is performed to make the ends of the forging flush, and the material fills the upper and lower circular cavities. The conical segment has a regular shape, and its size is controlled by the cavity. An 8% allowance is reserved based on the forging size, as shown in the attached figure. Figure 2 As shown; then, a punch is used to punch holes, resulting in a forging with round ends, a square middle section, and a hollow shape, as shown in the attached figure. Figure 3As shown; Initial forging temperature: reduced to 1110℃, grain growth is not obvious; Holding time: calculated at 0.3min / mm based on the thickness of the square solid billet when it enters the furnace; Final forging temperature must be greater than 850℃;

[0033] S3, Finishing and Forming: After the forgings processed in S2 are reheated and held at a certain temperature in the furnace, they are then forged in the next forging process; the initial forging temperature is 1090℃, and the holding time is calculated at 0.3min / mm based on the thickness of the billet when it enters the furnace; the final forging temperature must be greater than 850℃. During the finishing and forming process, the square section in the middle is first drawn to the size of the forging, and then the two round sections are rolled and drawn to the size of the forging, as shown in the attached figure. Figure 2 As shown.

Claims

1. A method for forming a large valve body forging for nuclear power plants, characterized in that: Includes the following steps: S1, manufacturing of square solid billet: Select stainless steel material with chemical composition that meets the standard as billet, perform upsetting and drawing deformation to refine the grain structure of the forging and obtain square solid billet; the initial forging temperature is 1180±20℃, and the holding time is calculated according to the thickness of the billet entering the furnace at 0.6~1min / mm; the final forging temperature must be greater than 850℃; S2, pre-forming with rounded ends: The square solid billet in S1 is returned to the furnace for heating. After holding at the temperature, the two ends are deformed from square surfaces into rounded sections. Initial forging temperature: Reduced to 1100±20℃, grain growth is not obvious. Holding time: Calculated according to the thickness of the square solid billet when it enters the furnace, at 0.2~0.4min / mm. The final forging temperature must be greater than 850℃. During the deformation process, the material at both ends is drawn into an octagon. After the two square sections are deformed into octagons, the end faces are petal-shaped because there is more material at the diagonal positions than at other positions on the opposite sides. Then, one octagonal section is inserted into a circular cavity placed on the lower anvil, and the other circular cavity is placed at the upper octagonal section. Then, upsetting deformation is performed to make the ends of the forging flush, and the material fills the upper and lower circular cavities. The conical section has a regular shape, and its size is controlled by the cavity. A 5% to 10% allowance is reserved based on the forging size. Then, a punch is used to punch holes to obtain a forging with a shape that meets the requirements: circular at both ends and square in the middle with a hollow center. S3, finishing and forming: After the forgings processed in S2 are heated and held in the furnace, they are forged for the next forging. The initial forging temperature is 1080±20℃, and the holding time is calculated according to the thickness of the billet when it enters the furnace, at 0.2~0.4min / mm. The final forging temperature must be greater than 850℃. During the finishing and forming process, the square section in the middle section is first drawn to the size of the forging, and then the two round sections are rolled and drawn to the size of the forging.

2. The forming method of a large valve body forging for nuclear power plants according to claim 1, characterized in that: When manufacturing a square solid blank in S1, an allowance of 15% to 20% is added to the square cross-sectional dimensions based on the size of the square solid blank.

3. The forming method of a large valve body forging for nuclear power plants according to claim 2, characterized in that: When heat preservation is carried out in S1, the heat preservation time is calculated based on the thickness of the blank entering the furnace at 0.8 min / mm.

4. The forming method of a large valve body forging for nuclear power plants according to claim 3, characterized in that: When heat preservation is carried out in S2, the heat preservation time is calculated based on the thickness of the square solid blank when it enters the furnace, at 0.3 min / mm.

Citation Information

Patent Citations

  • Method for forging cake series forgeable piece with different directions

    CN101176906A

  • Forging process for heading middle of long bar

    CN103691861A