Anti-crosstalk reflective filler, anti-crosstalk potting glue, medical CT scintillator ceramic array

The problem of signal crosstalk in the scintillator ceramic surface array is solved by using anti-crosstalk reflective potting adhesive that combines alumina, zirconia, silica microbeads and spherical titanium dioxide reflective particles in the medical CT scintillator ceramic surface array. A balance between efficient anti-crosstalk performance and optical output performance is achieved.

CN117777890BActive Publication Date: 2024-11-05YIRUI NEW MATERIAL TECH (TAICANG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311615163.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-11-05
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

In the medical CT scintillator ceramic surface array, an overly thin inter-pixel reflective layer causes signal crosstalk, reducing image quality, and it is difficult for the prior art to maintain light reflection ability while improving the anti-crosstalk capability.

Method used

Light absorption fillers such as alumina, zirconia, silica microbeads, etc. are combined with spherical titanium dioxide reflective particles of specific particle size, and mixed with transparent epoxy resin to make anti-crosstalt reflective potting adhesive for potting scintillators for CT Ceramic surface array enhances the anti-crosstalk performance of the reflective layer.

Benefits of technology

The crosstalk value between pixels is significantly reduced to less than 5%, maintaining the original light output intensity, and improving the image quality of the scintillator ceramic surface array.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117777890B_ABST
    Figure CN117777890B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of radiation detection and medical CT technology, and specifically relates to an anti-crosstalk reflective filler, an anti-crosstalk potting glue, and a medical CT scintillator ceramic array. The anti-crosstalk reflective filler of the present invention comprises a light absorbing filler, a light reflecting filler and a silane coupling agent; the light absorbing filler and the light reflecting filler are obtained by surface treatment of the silane coupling agent. The light reflecting filler is selected from one or more of R-103, R-104, R-960, and R-902+titanium dioxide, and the light absorbing filler is selected from one or more of alumina, zirconium dioxide, and silica microbeads. On this basis, the present invention also provides an anti-crosstalk potting glue and a medical CT scintillator ceramic array, which have excellent anti-crosstalk performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of radiation detection and medical CT, and in particular relates to an anti-crosstalk reflective filler, an anti-crosstalk potting glue, and a medical CT scintillator ceramic array. Background Art

[0002] The scintillator ceramic array for medical CT is the core component of the X-ray computed tomography (X-CT). Its principle is to convert high-energy rays into visible light signals and use them in conjunction with the detector array and photoelectric converter to obtain images.

[0003] In order to pursue image resolution, it is necessary to reduce the size of a single scintillator pixel as much as possible in the design of the scintillator array, and at the same time reduce the thickness of the reflective layer as much as possible. However, a too thin inter-pixel reflective layer will cause the transmission of light signals between single pixels, that is, signal crosstalk, which will reduce image quality. Therefore, how to improve the anti-crosstalk ability of the reflective layer without losing other parameter performance such as light reflection ability is the key to improving the image quality of the scintillator ceramic array. Summary of the invention

[0004] In order to suppress the crosstalk between pixels of scintillator ceramic array and improve the image of scintillator ceramic array, the present invention provides an anti-crosstalk reflective filler. The anti-crosstalk reflective filler is further mixed with epoxy resin to prepare an anti-crosstalk reflective potting glue. The potting glue can be used to pot the scintillator ceramic array for CT, which significantly reduces the crosstalk value. The measured crosstalk between pixels can be less than 5%.

[0005] In the experiment, the inventor found that the potting glue prepared by coupling and matching light absorbing fillers such as alumina, zirconium dioxide, and silica microbeads with titanium dioxide reflective particles in a specific particle size range in a certain proportion and mixing with transparent epoxy resin can significantly improve the anti-crosstalk ability of the CT scintillator ceramic array and maintain the original light output intensity. Among them, the reflective filler is selected from one or more of R-103, R-104, R-960, and R-902+titanium dioxide produced by Chemours, providing light reflection and scattering. Most of the CT scintillator ceramic arrays use gadolinium oxysulfide ceramics, and the main luminescence peak is near 512nm. The reflective filler of the present invention is a spherical titanium dioxide powder within a certain particle size range, which has a strong ability to scatter and reflect sub-wavelengths. Considering that the reflective layer of the ceramic array is relatively thin, in order to reduce the transmission of the light signal between the reflective layers, a filler that can block the light signal but does not reduce the light signal reflection at the contact surface between the ceramic pixel and the reflective layer is added, so that it has both good reflection ability and can fill the gaps between the reflective particles, so that the scattered light cannot continue to propagate. In addition, the light absorbing filler is selected from one or more of alumina, zirconium dioxide, and silicon dioxide microbeads, and cooperates with the light reflecting filler to suppress pipeline crosstalk.

[0006] Based on this, the present invention provides an anti-crosstalk reflective filler, an anti-crosstalk potting glue, and a medical CT scintillator ceramic array.

[0007] The anti-crosstalk reflective filler of the present invention comprises a light absorbing filler, a light reflecting filler and a silane coupling agent; the light absorbing filler and the light reflecting filler are obtained by surface treatment with the silane coupling agent.

[0008] Furthermore, the light-reflecting filler is selected from one or more of R-103, R-104, R-960, and R-902+titanium dioxide, and the light-absorbing filler is selected from one or more of alumina, zirconium dioxide, and silica microbeads.

[0009] Furthermore, the anti-crosstalk reflective filler is prepared by the following scheme: drying the powder raw materials of the components involved in the light-reflecting filler and the light-absorbing filler until the mass content of water is 3% to 5%; preparing the silane coupling agent into an ethanol solution with a mass content of 18% to 25%; mixing the dried components involved in the light-reflecting filler and the dried components involved in the light-absorbing filler, adding the ethanol solution of the silane coupling agent while stirring, and controlling the amount of the ethanol solution of the silane coupling agent to be 1.5 to 3.0% of the total mass of the powder raw materials; and then heating and drying to obtain the anti-crosstalk reflective filler.

[0010] As a preferred solution for anti-crosstalk reflective filler:

[0011] The powder raw material is composed of the following components based on the mass after drying: 60 parts by mass of R-104, 25 parts by mass of R-960, and 15 parts by mass of silicon dioxide;

[0012] Silane coupling agent KH560, dosage is 0.4% of the total mass of powder raw materials.

[0013] As another preferred solution for anti-crosstalk reflective filler:

[0014] The powder raw material is composed of the following components based on the mass after drying: 50 parts by mass of R-104, 30 parts by mass of R-902+, and 20 parts by mass of zirconium dioxide;

[0015] Silane coupling agent KH560, dosage is 0.4% of the total mass of powder raw materials.

[0016] The anti-crosstalk potting glue of the present invention comprises, by weight percentage, 40% to 60% of epoxy resin and 40% to 60% of the above-mentioned anti-crosstalk reflective filler.

[0017] Furthermore, the anti-crosstalk potting glue is prepared by the following method: adding epoxy resin and anti-crosstalk reflective filler into a vacuum planetary glue mixer tank, mixing the glue for 2.5min to 4.0min under vacuum state, and obtaining a uniform glue material, namely the anti-crosstalk potting glue.

[0018] The present invention also provides a medical CT scintillator ceramic array, comprising a scintillator array, which is composed of a plurality of cubic GOS scintillating ceramics distributed in an array on a plane; a gap is formed between adjacent GOS scintillating ceramics, the gap is filled with anti-crosstalk potting glue, and one surface of the scintillator array is also covered with the anti-crosstalk potting glue, and the remaining un-potted surface of the scintillator array is exposed for coupling with a photoelectric conversion device.

[0019] Furthermore, the length and width of the GOS scintillating ceramic are both 0.9 mm, and the height is 1.6 mm; the width of the gap between adjacent GOS scintillating ceramics is 0.1 mm, and the thickness of the glue layer of the anti-crosstalk potting glue covering one surface of the scintillator array is 0.3 mm.

[0020] Beneficial Effects

[0021] The anti-crosstalk reflective filler and anti-crosstalk potting glue provided by the present invention are suitable for CT ceramic scintillator arrays, so that excellent anti-crosstalk performance is formed between ceramic pixels.

[0022] The anti-crosstalk reflective filler and anti-crosstalk potting glue provided by the present invention have reflective fillers in epoxy resin to maintain reasonable reflection and scattering spacing, and absorbent fillers are filled between particles to block signal crosstalk caused by subsequent scattering, and have high light output performance after packaging. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Shown is the composition of the raw material powder in the anti-crosstalk reflection potting glue of each embodiment.

[0024] Figure 2 Shown is a schematic diagram of the scintillating ceramic array test.

[0025] Figure 3 Shown is the numbering of the test points on the Shuo ceramic array.

[0026] Figure 4 Shown are the crosstalk value test results of the samples of Example 1.

[0027] Figure 5 Shown are the crosstalk value test results of the samples of Example 2.

[0028] Figure 6 Shown is the average value of the crosstalk value of each example sample.

[0029] Figure 7The figure shows the crosstalk comparison in the X direction between Examples 7 and 8 and foreign competing products.

[0030] Figure 8 The figure shows the crosstalk comparison in the Y direction between Examples 7 and 8 and foreign competing products. DETAILED DESCRIPTION

[0031] The present invention is further illustrated by specific examples below. These examples are exemplary and are intended to illustrate the problem and explain the present invention, but are not intended to be limiting.

[0032] Embodiments 1 to 8

[0033] The GOS scintillator ceramic array is manufactured according to the following production process.

[0034] Step S1

[0035] The GOS ceramic substrate is heated and pasted on the fixed glass substrate with rosin. The scintillator substrate used is a GOS ceramic sheet with a length of 35 mm, a width of 22 mm, and a thickness of 2.2 mm.

[0036] Step S2

[0037] Use a precision scriber to cut and groove the surface, with a groove depth of 1.8mm. 20 grooves are made 1mm inward from the edge of the ceramic substrate and parallel to the long side 35mm. The groove width is 0.1mm and the spacing is 0.9mm.

[0038] Step S3

[0039] The GOS ceramic substrate and the glass substrate were rotated 90° as a whole, and 33 grooves were made at equal distances in a direction parallel to the short side 22 mm, with a groove width of 0.1 mm and a spacing of 0.9 mm.

[0040] Step S4

[0041] The grooved GOS ceramic substrate was ultrasonically cleaned with anhydrous ethanol for 3 minutes, vacuum dried at 60° C., and plasma cleaned for 5 minutes before use.

[0042] Step S5

[0043] To prepare the anti-crosstalk reflective potting glue, epoxy resin and filler are added in a vacuum planetary glue mixer tank according to a mass ratio of 1:1, and the glue is mixed in a vacuum for about 3 minutes to obtain the anti-crosstalk reflective potting glue.

[0044] Step S6

[0045] Wrap the ceramic substrate and the glass substrate with high temperature tape, slowly drip the potting glue obtained in step 5 into the surface groove of the GOS ceramic substrate to fill the groove, and then fill it with a thickness of 1mm, and vacuum degassing for 10 minutes.

[0046] Step S7

[0047] The GOS ceramic substrate filled with potting glue was placed in an oven and heated at 80°C for 20 hours, then heated to 100°C for 20 hours, and then taken out after stopping heating and cooling naturally.

[0048] Step S8

[0049] Remove the high-temperature tape around the glass substrate, fix the glass substrate on the grinder, and grind the glue layer to a thickness of 0.3mm; heat and melt the rosin, remove the ceramic substrate with the reflective layer, and grind on the grinder to remove about 0.5mm of excess unfilled crystals, exposing the reflective layer surface with chessboard grooves, so that the overall thickness becomes 1.6mm. Then use a precision dicing machine to cut off the excess crystals around the edges to obtain a CT scintillating ceramic array with a pixel specification of 32×16.

[0050] The operation steps of Examples 1 to 8 are basically the same, the only difference is the filler used in preparing the anti-crosstalk reflection potting glue, which is specifically referred to Figure 1 The recipe quantity in is implemented.

[0051] In step S5, the filler used to prepare the anti-crosstalk reflection potting glue is prepared according to the following steps. Figure 1 Prepare raw material powders of the raw material types shown, and bake each raw material powder in an oven at 60°C until the water content of each raw material is adjusted to 3%~5%. Then prepare KH560 coupling agent and ethanol into a uniform solution with a mass ratio of 1:4. Figure 1 Add the dried reflective filler powder and light absorbing filler powder to the powder mixer according to the formula ratio shown, and evenly spray the prepared coupling agent ethanol mixture at the same time as the mixing, with the amount being 2% of the total weight of the powder. Pour out after mixing for 20 minutes, and vacuum dry at 100℃ for 12 hours to obtain the filler.

[0052] Performance Testing

[0053] like Figure 2 As shown, an X-ray tube is used to emit initial X-rays, which are collimated by a ray collimator to obtain direct X-rays. The rays pass through the hole array in the tungsten plate to illuminate the scintillating ceramic array to test its crosstalk value. Figure 2 In the figure, A represents the X-ray tube, B represents the initial X-ray, C represents the collimator, D represents the direct X-ray, E represents the tungsten plate, and F represents the scintillating ceramic array. The tungsten plate has an aperture of 0.3 mm and is arranged in a 3×5 array. Irradiation conditions: X-ray 135 kV-1.5 mA-SID 32 cm, irradiation time 1 s.

[0054] According to the above method, the scintillating ceramic arrays of Examples 1 to 8 and samples a and b purchased from abroad were tested respectively. Samples a and b were purchased from well-known foreign companies, representing the best anti-crosstalk level currently achievable in the industry. The scintillators used are the same scintillating ceramics used in the present invention, and the formula and preparation process of the potting glue used are kept confidential, and there is currently no complete public information.

[0055] Each scintillating ceramic array is as follows Figure 3 The test points shown record the crosstalk values ​​in the X and Y directions. For example, the test results of Example 1 are as follows: Figure 4 As shown, the test results of Example 2 are as follows Figure 5 According to the test results, the average crosstalk value of all test points of each test sample is obtained, and the result is shown in Figure 6 Shown

[0056] The results show that the scintillating ceramic arrays for medical CT of Examples 1 to 8 of the present invention have excellent radiation resistance as a whole, and can meet the use requirements of medical CT scintillating ceramic arrays at a relatively low cost. In particular, the samples of Examples 7 and 8 have better anti-crosstalk performance than foreign comparative samples a and b. A detailed comparison of the anti-crosstalk values ​​of each test point in the X and Y directions of Example 7, Example 8, Sample a and Sample b is shown in Figure 2. Figure 7 and Figure 8 shown.

[0057] The above embodiments are exemplary, and their purpose is to illustrate the technical concept and features of the present invention so that people familiar with the technology in this field can understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. An anti-crosstalk potting glue, characterized by: Measured by mass percentage, it includes 40% to 60% of epoxy resin and 40% to 60% of anti-crosstalk reflective filler; The anti-crosstalk reflective filler comprises a light absorbing filler, a light reflecting filler and a silane coupling agent; the light absorbing filler and the light reflecting filler are obtained by surface treatment with the silane coupling agent; The light-reflecting filler is spherical titanium dioxide powder selected from R-104, R-960, R-902+titanium dioxide, and the light-absorbing filler is selected from zirconium dioxide and silicon dioxide microbeads; The anti-crosstalk reflective filler is prepared by the following scheme: The powder raw materials of the components involved in the light-reflecting filler and the light-absorbing filler are dried until the water content is 3% to 5% by mass; the silane coupling agent is prepared into an ethanol solution with a mass content of 18% to 25%; the dried components involved in the light-reflecting filler and the dried components involved in the light-absorbing filler are mixed, and the ethanol solution of the silane coupling agent is added while stirring, and the amount of the ethanol solution of the silane coupling agent is controlled to be 1.5 to 3.0% of the total mass of the powder raw materials; and then heated and dried to obtain the anti-crosstalk reflective filler; The powder raw material is composed of the following components based on the mass after drying: 60 parts by mass of R-104, 25 parts by mass of R-960, and 15 parts by mass of silicon dioxide, or the following components: 50 parts by mass of R-104, 30 parts by mass of R-902+, and 20 parts by mass of zirconium dioxide; The silane coupling agent KH560 is used in an amount of 0.4% of the total mass of the powder raw material.

2. The anti-crosstalk potting adhesive according to claim 1, characterized in that: The anti-crosstalk potting glue is prepared by the following method: adding epoxy resin and anti-crosstalk reflective filler into a vacuum planetary glue mixer tank, mixing the glue for 2.5min to 4.0min under vacuum state, and obtaining a uniform glue material, namely the anti-crosstalk potting glue.

3. A medical CT scintillator ceramic array, characterized in that: The invention comprises a scintillator array, which is composed of a plurality of cubic GOS scintillator ceramics distributed in an array on a plane; a gap is formed between adjacent GOS scintillator ceramics, the gap is filled with an anti-crosstalk potting glue, and one surface of the scintillator array is also covered with the anti-crosstalk potting glue, and the remaining un-potted surface of the scintillator array is exposed for coupling with a photoelectric conversion device; the anti-crosstalk potting glue is the anti-crosstalk potting glue according to claim 1 or 2.

4. The medical CT scintillator ceramic array according to claim 3, characterized in that: The length and width of the GOS scintillating ceramics are both 0.9 mm, and the height is 1.6 mm; the width of the gap between adjacent GOS scintillating ceramics is 0.1 mm, and the thickness of the glue layer of the anti-crosstalk potting glue covering one surface of the scintillator array is 0.3 mm.