A near-infrared full-band shielding ferrous-doped colorless highly transparent silicate energy-saving glass and a preparation method thereof
By doping ferrous ions in the glass and using the melt quenching method to prepare it, the problems of poor transparency and high production complexity of existing energy-saving glass when shielding near-infrared light are solved, and high-efficiency, low-cost near-infrared full-band imaging is achieved. Balance of shielding effect and high visible light transmittance.
Patent Information
- Application Number
- CN202410052065.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-12
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-01-12
AI Technical Summary
Existing energy-saving glass has poor transparency while shielding near-infrared light, affecting visible light transmittance. The production process is complex and costly, and there are problems such as oxidation problems and poor chemical stability.
It uses ferrous iron-doped colorless high-transparent silicate glass, which is prepared in an air atmosphere through a simple melting and quenching method. Iron compounds and reducing agents are used to generate ferrous ions, which are wrapped in the glass to reduce oxygen contact and avoid oxidation. Simplify processes and reduce costs.
It achieves a balance between near-infrared full-band shielding effect and high visible transmittance, reduces production complexity and cost, reduces heavy metal pollution, is suitable for mass production, and improves the chemical stability of the glass.
Smart Images

Figure CN117865476B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass manufacturing, and in particular to a near-infrared full-band shielding ferrous-doped colorless high-transmittance silicate energy-saving glass and a preparation method thereof. Background Art
[0002] Glass is made of quartz sand, soda ash, feldspar and limestone. After mixing, high-temperature melting, homogenization, processing and forming, and then annealing, it is a silicate non-metallic material. It has the characteristics of transparency, non-flammability, high temperature resistance, impact resistance, and non-conductivity. It can be seen everywhere in daily life, such as large glass windows and car glass used in buildings. However, ordinary glass has a high sunlight transmittance and a low infrared reflectivity. Most of the sunlight passes through the glass, which will cause the room, car interior, greenhouse and other spaces to overheat; at the same time, the energy of indoor objects will be lost through the glass in the form of radiation. Therefore, the load of air conditioning becomes heavier and heavier. In order to prevent the global greenhouse effect, both homes and offices have strengthened energy-saving measures, and the demand for energy-saving glass is growing year by year. At present, traditional energy-saving glass can be divided into colored glass, low-emissivity (Low-E) glass, film glass, laminated glass, etc. Colored glass is colored by metal ions or metal particles, and has the advantages of simple process, low cost, durability, and anti-glare. However, it has poor selectivity for absorbing sunlight, and has low visible light transmittance while absorbing infrared light. It has limited application value for houses in cities that urgently need more natural lighting. In addition, living in a house with colored glass for a long time will damage eyesight and have adverse effects on the mental state of the residents. Low-emissivity (Low-E) glass can be divided into online and offline types. The coating of online Low-E glass is exposed to the outside, and it is easy to fall off partially due to scratches or "pinhole" defects caused by sputtering during transportation and installation; the core functional layer of offline Low-E glass is a metal silver layer, but it usually needs to be sealed in the interlayer of double-layer glass. It is a kind of laminated glass. Once the glass interlayer is damaged, the metal silver layer is quickly oxidized, the infrared shielding effect disappears, and the visible transmittance is significantly reduced. In addition, the production process of offline low-E glass is complicated, and the price can reach several times or even dozens of times that of single-layer glass. VO2 film glass for smart windows can automatically adjust the transmittance according to the external temperature, but its chemical stability is poor and its service life is short. How to prepare an energy-saving glass with excellent performance has become a technical problem that technicians in this field need to solve urgently. Summary of the invention
[0003] The purpose of the present invention is to provide a near-infrared full-band shielding ferrous-doped colorless high-transparent silicate energy-saving glass and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art.
[0004] To achieve the above object, the present invention provides the following solutions:
[0005] One of the technical solutions of the present invention is: a near-infrared full-band shielding ferrous-doped colorless high-transmittance silicate energy-saving glass, which comprises the following components by weight percentage: SiO2 20-80%, P2O5 0.5-35%, M2O 10-40%, FeO0.1-5%, B2O3 5-15%, GeO2 1-10%, Al2O3 5-15% and CaO1-10%;
[0006] The M element in the M2O is selected from one or more of Li, Na, K, Rb and Cs.
[0007] The second technical solution of the present invention is a method for preparing the above-mentioned ferrous-doped colorless high-transmittance silicate energy-saving glass with near-infrared full-band shielding, comprising the following steps:
[0008] (1) mixing raw materials of compounds other than FeO and subjecting them to heat treatment, cooling and then preheating, heating to a melting temperature, and then quenching and forming after heat preservation to obtain a glass block;
[0009] (2) crushing the glass blocks, mixing them with the raw material of FeO and the reducing agent, preheating and heating them to the melting temperature, keeping them warm and then quenching and forming them, and annealing them to obtain the ferrous-doped colorless high-transmittance silicate energy-saving glass with near-infrared full-band shielding.
[0010] Further, SiO2 is introduced through silicon dioxide;
[0011] P2O5 is introduced through phosphorus pentoxide, ammonium hydrogen phosphate or phosphate;
[0012] M2O is introduced through carbonates or phosphates containing M elements;
[0013] B2O3 is introduced via boron oxide or boric acid;
[0014] GeO2 is introduced through germanium oxide;
[0015] Al2O3 is introduced through aluminum oxide or phosphate containing Al element;
[0016] CaO is introduced via calcium carbonate;
[0017] The raw material of FeO includes iron compounds or iron alone.
[0018] Furthermore, the iron compound includes FeCl2, FeCl3, FeO, Fe2O3 or FeSO4; the FeCl2 is anhydrous ferrous chloride or ferrous chloride hydrate; the FeCl3 is anhydrous ferric chloride or ferric chloride hydrate.
[0019] Further, the reducing agent includes ammonium salt, carbon powder and silicon powder;
[0020] The weight ratio of the ammonium salt, carbon powder and silicon powder is (1-10): (0.5-5): (0.1-1);
[0021] The amount of the reducing agent used is 1.6-16% of the total weight of the raw materials.
[0022] Furthermore, the ammonium salt is ammonium chloride.
[0023] Furthermore, in step (1), the heating rate of the heat treatment is 5-10°C / min, the temperature is 600°C, and the time is 1h;
[0024] The preheating temperature is 300-500°C and the time is 5-10 minutes;
[0025] The melting temperature is 1100-1700° C.; the insulation time is 1-3 hours.
[0026] Furthermore, in step (2), the preheating temperature is 400-600° C. and the time is 5-10 min;
[0027] The melting temperature is 1100-1700° C.; the insulation time is 1-5 hours.
[0028] Furthermore, in step (2), the annealing temperature is 400-600° C., and the time is 2-12 hours.
[0029] Furthermore, the raw materials in step (1) are ground and sieved (100-300 mesh sieve) before mixing; the grinding time is 10-30 minutes.
[0030] Furthermore, in step (2), the crushing is performed by pulverizing or ball-milling into glass powder passing through a 100-300 mesh sieve.
[0031] Furthermore, in step (2), the FeO raw material and the reducing agent are ground and sieved (100-300 mesh sieve) before mixing; the grinding time is 20-60 minutes.
[0032] Furthermore, in step (2), the mold temperature used in the quenching forming is 300-600°C.
[0033] Furthermore, after the annealing in step (2), the temperature is further reduced to room temperature at a cooling rate of 1 to 5° C. / min.
[0034] The present invention realizes the production of energy-saving glass by adopting a simple melting quenching method. Under the premise of not using a sulfur-carbon reducing agent and not requiring a protective atmosphere, the glass melt can quickly wrap the ferrous ions, greatly reducing the direct contact between oxygen and the ferrous ions, and inhibiting the conversion of the ferrous ions into ferric ions. The method of the present invention is applicable to a traditional float glass production line, can greatly reduce the complexity and danger of production, and is helpful for the rapid, large-scale and convenient production of ferrous heat-absorbing energy-saving glass. At the same time, the produced near-infrared full-band shielding ferrous-doped colorless high-transmittance silicate energy-saving glass can be transparent and colorless to a large extent. Compared with the original ferrous-doped soda-lime-silicon energy-saving glass, it can better respond to ambient light and does not affect the transmission of visible light.
[0035] The third technical solution of the present invention: Application of the above-mentioned ferrous-doped colorless high-transmittance silicate energy-saving glass with full-band near-infrared shielding in the fields of construction, automobile manufacturing or aerospace.
[0036] The present invention discloses the following technical effects:
[0037] (1) The ferrous-doped colorless, highly transparent silicate energy-saving glass with full-band near-infrared shielding prepared by the present invention can shield near-infrared light while maintaining high visible transmittance, and does not affect visible light transmittance to a certain extent, truly reflecting ambient light. Compared with similar products, the raw materials for production are cheap and easy to obtain, the production process is greatly simplified, and it is suitable for popularization and use.
[0038] (2) The present invention uses iron compounds or single iron as the iron source, and uses a reducing agent to generate reducing gas during melting, thereby producing glass with a higher ferrous iron ratio; the raw materials used in the present invention are cheap and easy to obtain, with low pollution, and can reduce heavy metal pollution compared to the current Low-E silver film or ITO coated glass, thereby greatly reducing costs.
[0039] (3) The present invention uses high temperature rapidly melted broken glass (glass powder) to coat low-valent iron elements, eliminating the additional process of coating treatment and shortening the production cycle. The present invention does not require a protective atmosphere and adopts a melt quenching process, which can be adapted to ordinary float glass production lines.
[0040] (4) The present invention uses ammonium salt, carbon powder and silicon powder as a mixed reducing agent, thereby avoiding the influence of abnormal sulfur and carbon coloring on glass performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 This is a physical picture of the ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding prepared in Example 1 of the present invention.
[0043] Figure 2 This is a rendering of the transmission spectrum performance of the ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding prepared in Examples 1 to 6 of the present invention. DETAILED DESCRIPTION
[0044] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0045] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0046] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0047] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0048] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0049] Example 1
[0050] A preparation method of ferrous-doped colorless highly transparent silicate energy-saving glass with near-infrared full-band shielding:
[0051] The ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding is composed of the following raw materials, calculated by weight percentage: 33.03% of sodium dihydrogen phosphate (NaH2PO4), 0.87% of ferrous chloride (FeCl2·4H2O), 3.75% of ammonium chloride (NH4Cl), 1.88% of carbon powder, 0.56% of silicon powder, 19.54% of silicon dioxide (SiO2), 7.07% of boron oxide (B2O3), 5.32% of germanium oxide (GeO2), 8.27% of aluminum oxide (Al2O3), 16.2% of sodium carbonate (Na2CO3) and 3.51% of calcium carbonate (CaCO3).
[0052] (1) Ingredients of Mixture 1: Sodium dihydrogen phosphate, silicon dioxide, boron oxide, germanium oxide, aluminum oxide, sodium carbonate and calcium carbonate were crushed and passed through a 200-mesh sieve respectively, and then fully mixed for 10 minutes to obtain Mixture 1 (main raw material).
[0053] (2) Degassing: Pour the mixture 1 obtained in step (1) into a crucible, place the crucible in a muffle furnace, and heat it to 600° C. at a heating rate of 10° C. / min in an air atmosphere, keep the temperature for 1 h, and then cool it to room temperature.
[0054] (3) Preparation of glass liquid 1: The crucible containing the degassed mixture 1 obtained in step (2) is preheated at 500° C. for 10 min in an air atmosphere, and then placed in a lifting furnace and kept at 1250° C. for 1 h to melt the mixture 1 into glass liquid 1.
[0055] (4) Quenching and forming treatment of the glass liquid 1: The glass liquid 1 obtained in step (3) is placed in a cold container for quenching and forming to obtain a cracked glass block and a crucible for storing the residual glass liquid 1 (the glass block explodes due to internal stress).
[0056] (5) Preparation of glass powder: Grind the glass block obtained in step (4) and pass it through a 300-mesh sieve to obtain glass powder.
[0057] (6) Mixture 2 ingredients: ferrous chloride, ammonium chloride, carbon powder and silicon powder were crushed and passed through a 300-mesh sieve respectively, and then fully mixed for 20 minutes to obtain mixture 2 (additive materials).
[0058] (7) Preparation of glass liquid 2: Add glass powder and mixed material 2 to the crucible storing the residual glass liquid 1 in step (4), preheat at 500°C for 10 min in an air atmosphere, then put into a lifting furnace and keep at 1250°C for 2 h to melt into glass liquid 2.
[0059] (8) Quenching and forming the glass liquid 2: The glass liquid 2 obtained in step (7) is placed in a preheated mold (temperature is 430°C) for quenching and forming, and then the quenched and formed sample is placed in an annealing furnace at 430°C for annealing for 12 hours, and finally cooled to room temperature at a cooling rate of 1°C / min to obtain a ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding (a high-transmittance, high near-infrared shielding, colorless, heat-insulating and energy-saving glass product).
[0060] Table 1 Theoretical component contents of ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding prepared from 100 g of raw materials
[0061]
[0062]
[0063] Example 2
[0064] A preparation method of ferrous-doped colorless highly transparent silicate energy-saving glass with near-infrared full-band shielding:
[0065] The ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding is composed of the following raw materials, calculated by weight percentage: 25.60% of sodium dihydrogen phosphate (NaH2PO4), 0.88% of ferrous chloride (FeCl2·4H2O), 3.75% of ammonium chloride (NH4Cl), 1.88% of carbon powder, 0.56% of silicon powder, 24.60% of silicon dioxide (SiO2), 7.01% of boron oxide (B2O3), 5.45% of germanium oxide (GeO2), 8.14% of aluminum oxide (Al2O3), 18.65% of sodium carbonate (Na2CO3) and 3.48% of calcium carbonate (CaCO3).
[0066] (1) Ingredients of Mixture 1: Sodium dihydrogen phosphate, silicon dioxide, boron oxide, germanium oxide, aluminum oxide, sodium carbonate and calcium carbonate were crushed and passed through a 200-mesh sieve respectively, and then fully mixed for 10 minutes to obtain Mixture 1 (main raw material).
[0067] (2) Degassing: Pour the mixture 1 obtained in step (1) into a crucible, place the crucible in a muffle furnace, and heat it to 600° C. at a heating rate of 10° C. / min in an air atmosphere, keep the temperature for 1 h, and then cool it to room temperature.
[0068] (3) Preparation of glass liquid 1: The crucible containing the degassed mixture 1 obtained in step (2) is preheated at 500° C. for 10 min in an air atmosphere, and then placed in a lifting furnace and kept at 1250° C. for 1 h to melt the mixture 1 into glass liquid 1.
[0069] (4) Quenching and forming treatment of the glass liquid 1: The glass liquid 1 obtained in step (3) is placed in a cold container for quenching and forming to obtain a cracked glass block and a crucible for storing the residual glass liquid 1 (the glass block explodes due to internal stress).
[0070] (5) Preparation of glass powder: Grind the glass block obtained in step (4) and pass it through a 300-mesh sieve to obtain glass powder.
[0071] (6) Mixture 2 ingredients: ferrous chloride, ammonium chloride, carbon powder and silicon powder were crushed and passed through a 300-mesh sieve respectively, and then fully mixed for 20 minutes to obtain mixture 2 (additive materials).
[0072] (7) Preparation of glass liquid 2: Add glass powder and mixed material 2 to the crucible storing the residual glass liquid 1 in step (4), preheat at 500°C for 10 min in an air atmosphere, then put into a lifting furnace and keep at 1250°C for 2 h to melt into glass liquid 2.
[0073] (8) Quenching and forming the glass liquid 2: The glass liquid 2 obtained in step (7) is placed in a preheated mold (temperature is 430°C) for quenching and forming, and then the quenched and formed sample is placed in an annealing furnace at 430°C for annealing for 12 hours, and finally cooled to room temperature at a cooling rate of 1°C / min to obtain a ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding (a high-transmittance, high near-infrared shielding, colorless, heat-insulating and energy-saving glass product).
[0074] Table 2 Theoretical component contents of ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding prepared from 100 g of raw materials
[0075] Components Weight(g) Weight percentage (%) <![CDATA[SiO2]]> 25.80 31.72 <![CDATA[P2O5]]> 15.15 18.63 <![CDATA[M2O(Na2O)]]> 17.52 21.54 FeO 0.32 0.38 <![CDATA[B2O3]]> 7.01 8.62 <![CDATA[GeO2]]> 5.45 6.70 <![CDATA[Al2O3]]> 8.14 10.01 CaO 1.95 2.40 total 81.34 100
[0076] Example 3
[0077] A preparation method of ferrous-doped colorless highly transparent silicate energy-saving glass with near-infrared full-band shielding:
[0078] The ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding is composed of the following raw materials, calculated by weight percentage: 15.80% of sodium dihydrogen phosphate (NaH2PO4), 0.88% of ferrous chloride (FeCl2·4H2O), 3.75% of ammonium chloride (NH4Cl), 1.88% of carbon powder, 0.56% of silicon powder, 30.60% of silicon dioxide (SiO2), 7.11% of boron oxide (B2O3), 5.35% of germanium oxide (GeO2), 8.11% of aluminum oxide (Al2O3), 22.45% of sodium carbonate (Na2CO3) and 3.51% of calcium carbonate (CaCO3).
[0079] (1) Ingredients of Mixture 1: Sodium dihydrogen phosphate, silicon dioxide, boron oxide, germanium oxide, aluminum oxide, sodium carbonate and calcium carbonate were crushed and passed through a 200-mesh sieve respectively, and then fully mixed for 10 minutes to obtain Mixture 1 (main raw material).
[0080] (2) Degassing: Pour the mixture 1 obtained in step (1) into a crucible, place the crucible in a muffle furnace, and heat it to 600° C. at a heating rate of 10° C. / min in an air atmosphere, keep the temperature for 1 h, and then cool it to room temperature.
[0081] (3) Preparation of glass liquid 1: The crucible containing the degassed mixture 1 obtained in step (2) is preheated at 500° C. for 10 min in an air atmosphere, and then placed in a lifting furnace and kept at 1250° C. for 1 h to melt the mixture 1 into glass liquid 1.
[0082] (4) Quenching and forming treatment of the glass liquid 1: The glass liquid 1 obtained in step (3) is placed in a cold container for quenching and forming to obtain a cracked glass block and a crucible for storing the residual glass liquid 1 (the glass block explodes due to internal stress).
[0083] (5) Preparation of glass powder: Grind the glass block obtained in step (4) and pass it through a 300-mesh sieve to obtain glass powder.
[0084] (6) Mixture 2 ingredients: ferrous chloride, ammonium chloride, carbon powder and silicon powder were crushed and passed through a 300-mesh sieve respectively, and then fully mixed for 20 minutes to obtain mixture 2 (additive materials).
[0085] (7) Preparation of glass liquid 2: Add glass powder and mixed material 2 to the crucible storing the residual glass liquid 1 in step (4), preheat at 500°C for 10 minutes in an air atmosphere, and then put into a lifting furnace and keep it at 1600°C for 2 hours to melt into glass liquid 2.
[0086] (8) Quenching and forming the glass liquid 2: placing the glass liquid 2 obtained in step (7) in a preheated mold (temperature is 430°C) for quenching and forming, and then placing the quenched and formed sample in an annealing furnace at 430°C for annealing for 12 hours, and finally cooling to room temperature at a rate of 1°C / min to obtain a ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding (a high-transmittance, high near-infrared shielding, colorless, heat-insulating, energy-saving glass product).
[0087] Table 3 Theoretical component contents of ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding prepared from 100 g of raw materials
[0088] Components Weight(g) Weight percentage (%) <![CDATA[SiO2]]> 31.80 39.15 <![CDATA[P2O5]]> 9.35 11.51 <![CDATA[M2O(Na2O)]]> 17.21 21.19 FeO 0.32 0.39 <![CDATA[B2O3]]> 7.11 8.75 <![CDATA[GeO2]]> 5.35 6.59 <![CDATA[Al2O3]]> 8.11 9.99 CaO 1.97 2.43 total 81.22 100
[0089] Example 4
[0090] The same as Example 1, except that the ferrous-doped colorless high-transmittance silicate energy-saving glass with near-infrared full-band shielding has the following raw materials, measured by weight percentage: 34.53% of potassium dihydrogen phosphate (KH2PO4), 0.87% of ferrous chloride (FeCl2·4H2O), 3.75% of ammonium chloride (NH4Cl), 1.88% of carbon powder, 0.56% of silicon powder, 19.04% of silicon dioxide (SiO2), 6.55% of boron oxide (B2O3), 5.34% of germanium oxide (GeO2), 7.76% of aluminum oxide (Al2O3), 16.2% of potassium carbonate (K2CO3) and 3.52% of calcium carbonate (CaCO3).
[0091] Table 4 Theoretical component contents of ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding prepared from 100 g of raw materials
[0092]
[0093]
[0094] Example 5
[0095] The same as Example 1, except that the ferrous-doped colorless high-transmittance silicate energy-saving glass with near-infrared full-band shielding has the following raw materials, measured by weight percentage: 34.53% of lithium dihydrogen phosphate (LiH2PO4), 0.87% of ferrous chloride (FeCl2·4H2O), 3.75% of ammonium chloride (NH4Cl), 1.88% of carbon powder, 0.56% of silicon powder, 19.04% of silicon dioxide (SiO2), 6.55% of boron oxide (B2O3), 5.34% of germanium oxide (GeO2), 7.76% of aluminum oxide (Al2O3), 16.2% of lithium carbonate (Li2CO3) and 3.52% of calcium carbonate (CaCO3).
[0096] Table 5 Theoretical component contents of ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding prepared from 100 g of raw materials
[0097] Components Weight(g) Weight percentage (%) <![CDATA[SiO2]]> 20.24 26.09 <![CDATA[P2O5]]> 23.58 30.40 <![CDATA[M2O(Li2O)]]> 11.52 14.85 FeO 0.31 0.40 <![CDATA[B2O3]]> 6.65 8.57 <![CDATA[GeO2]]> 5.34 6.88 <![CDATA[Al2O3]]> 7.96 10.26 CaO 1.97 2.55 total 77.57 100
[0098] Example 6
[0099] The same as Example 3, the only difference is that step (8) is specifically as follows: placing the glass liquid 2 obtained in step (7) in a preheated mold (temperature is 430°C) for quenching and forming, and then placing the quenched and formed sample in an annealing furnace at 430°C for annealing for 6 hours, cooling to room temperature, and obtaining a ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding (a high-transmittance, high near-infrared shielding, colorless, heat-insulating and energy-saving glass product).
[0100] The glass product prepared in this embodiment will break due to excessive internal stress.
[0101] Table 6 Theoretical component contents of ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding prepared from 100 g of raw materials
[0102] Components Weight(g) Weight percentage (%) <![CDATA[SiO2]]> 31.80 39.15 <![CDATA[P2O5]]> 9.35 11.51 <![CDATA[M2O(Na2O)]]> 17.21 21.19 FeO 0.32 0.39 <![CDATA[B2O3]]> 7.11 8.75 <![CDATA[GeO2]]> 5.35 6.59 <![CDATA[Al2O3]]> 8.11 9.99 CaO 1.97 2.43 total 81.22 100
[0103] Comparative Example 1
[0104] Same as Example 1, except that only one reducing agent, ammonium chloride (NH4Cl) 6.19%, is used.
[0105] The glass product prepared in this comparative example has a visible light transmittance of 78.2% and a near infrared transmittance of 13.2%.
[0106] Comparative Example 2
[0107] The same as Example 1, the only difference is that the two-step method is not adopted, and the first step is direct sintering. Specifically:
[0108] (1) Mixture preparation: All raw materials were crushed and passed through a 200-mesh sieve, and then fully mixed for 10 minutes to obtain a mixture.
[0109] (2) Degassing: Pour the mixture obtained in step (1) into a crucible, place the crucible in a muffle furnace, and heat it to 600° C. at a heating rate of 10° C. / min in an air atmosphere, keep the temperature for 1 h, and then cool it to room temperature.
[0110] (3) Preparation of molten glass: The crucible containing the degassed mixture obtained in step (2) was preheated at 500° C. for 10 min in an air atmosphere, and then placed in a lifting furnace and kept at 1250° C. for 1 h to melt the mixture into molten glass.
[0111] (4) Quenching and forming of glass liquid: The glass liquid obtained in step (3) is placed in a preheated mold (temperature is 430°C) for quenching and forming, and then the quenched and formed sample is placed in an annealing furnace at 430°C for annealing for 12 hours, and finally cooled to room temperature at a cooling rate of 1°C / min to obtain a glass product.
[0112] The glass product prepared in this comparative example is yellow, has a visible light transmittance of 75.2%, and a near infrared transmittance of 17.6%.
[0113] Comparative Example 3
[0114] The same as Example 1, except that only one reducing agent, 6.19% carbon powder, is used.
[0115] The glass product prepared in this comparative example has a visible light transmittance of 75.1% and a near infrared transmittance of 9.7%.
[0116] Effect Example 1
[0117] The actual picture of the near-infrared full-band shielding ferrous-doped colorless high-transparent silicate energy-saving glass prepared in Example 1 is shown in Figure 1 .
[0118] The transmission spectrum performance effect diagram of the near-infrared full-band shielding ferrous-doped colorless high-transmittance silicate energy-saving glass prepared in Examples 1 to 6 is shown in Figure 2 .
[0119] Figure 2 Among them, 1 is embodiment 1, 2 is embodiment 2, 3 is embodiment 3, 4 is embodiment 4, 5 is embodiment 5, and 6 is embodiment 6.
[0120] Effect Example 2
[0121] The visible light and near infrared light transmittance of the ferrous-doped colorless high-transmittance silicate energy-saving glass with near infrared full-band shielding prepared in Examples 1 to 6 were measured. The results are shown in Table 7.
[0122] (1) Test sample: the ferrous-doped colorless high-transmittance silicate energy-saving glass with near-infrared full-band shielding prepared in Examples 1 to 6, with a thickness of 4 mm.
[0123] (2) Test method: The transmittance was measured using a UV-Visible / NIR spectrophotometer from Japan's HITACHI Company. The wavelength range for the visible light transmittance test was 380 to 780 nm, and the wavelength range for the near infrared light transmittance test was 780 to 2500 nm.
[0124] Table 7 Visible light and near infrared light transmittance
[0125] Group Visible light transmittance (%) Near infrared light transmittance (%) Example 1 83.8 3.5 Example 2 82.7 2.5 Example 3 63.7 0.1 Example 4 81.5 1.4 Example 5 84.0 9.1 Example 6 83.8 3.5
[0126] It can be seen from Table 7 that the component types and proportions of the ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding have a significant impact on the performance of the glass. Comparison of Examples 1 to 3 shows that with the change in the concentration of phosphorus and silicon elements in the glass matrix, the near-infrared shielding ability has a certain change, and the absorption peak becomes wider as the phosphorus element decreases and the silicon element increases. Comparison of Examples 1, 4, and 5 shows that with the change in the radius of the alkali metal ions, the near-infrared shielding ability has a certain change. The larger the ion radius, the stronger the near-infrared shielding ability. Comparison of Example 3 and Example 6 shows that the length of the annealing time affects the molding of the glass. Too short an annealing time will cause the glass to break due to excessive internal stress.
Claims
1. A near-infrared full-band shielding ferrous-doped colorless highly transparent silicate energy-saving glass, characterized in that: The invention comprises the following components by weight percentage: SiO2 20-31.72%, P2O5 18.63-35%, M2O 10-40%, FeO 0.1-5%, B2O3 5-15%, GeO2 1-10%, Al2O3 5-15% and CaO 1-10%; The M element in the M2O is selected from one or more of Na, K, Rb and Cs; The preparation method of the near-infrared full-band shielding ferrous-doped colorless highly transparent silicate energy-saving glass comprises the following steps: (1) mixing raw materials of compounds other than FeO and subjecting them to heat treatment, cooling and then preheating, heating to a melting temperature, and then quenching and forming after heat preservation to obtain a glass block; (2) crushing the glass blocks, mixing them with FeO raw materials and a reducing agent, preheating and heating them to a melting temperature, keeping them warm and then quenching and forming them, and annealing them to obtain the ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding; The reducing agent includes ammonium salt, carbon powder and silicon powder; The weight ratio of the ammonium salt, carbon powder and silicon powder is (1-10): (0.5-5): (0.1-1); The amount of the reducing agent used is 1.6-16% of the total weight of the raw materials.
2. The near-infrared full-band shielding ferrous-doped colorless highly transparent silicate energy-saving glass according to claim 1, characterized in that: SiO2 is introduced through silicon dioxide; P2O5 is introduced through phosphorus pentoxide, ammonium hydrogen phosphate or phosphate; M2O is introduced through carbonates or phosphates containing M elements; B2O3 is introduced via boron oxide or boric acid; GeO2 is introduced through germanium oxide; Al2O3 is introduced through aluminum oxide or phosphate containing Al element; CaO is introduced via calcium carbonate; The raw material of FeO includes iron compounds or iron alone.
3. The near-infrared full-band shielding ferrous-doped colorless highly transparent silicate energy-saving glass according to claim 1, characterized in that: In step (1), the heating rate of the heat treatment is 5-10°C / min, the temperature is 600°C, and the time is 1h; The preheating temperature is 300-500°C and the time is 5-10 minutes; The melting temperature is 1100-1700° C.; the insulation time is 1-3 hours.
4. The near-infrared full-band shielding ferrous-doped colorless highly transparent silicate energy-saving glass according to claim 1, characterized in that: In step (2), the preheating temperature is 400-600° C. and the time is 5-10 min; The melting temperature is 1100-1700° C.; the insulation time is 1-5 hours.
5. The ferrous-doped colorless high-transmittance silicate energy-saving glass with near-infrared full-band shielding according to claim 1 is characterized in that: In step (2), the annealing temperature is 400-600° C. and the time is 2-12 hours.
6. Use of the ferrous-doped colorless, highly transparent silicate energy-saving glass with near-infrared full-band shielding as claimed in any one of claims 1 to 5 in the fields of construction, automobile manufacturing or aerospace.