A weathering vanadium-titanium iron ore dressing process

Through the flash roasting and reducing iron oxide process, the problem of close relationship between iron ore and titanium mineral embedded in weathered vanadium ilmenite is solved, efficient separation and recovery of titanium and iron are achieved, and the cost of ore dressing is reduced, and it is suitable for large-scale promotion.

CN118045697BActive Publication Date: 2024-12-03GUANGDONG UBRIDGE NEW MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410135033.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2024-12-03
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

The iron ore in weathered vanadium ilmenite is closely related to the titanium mineral embedded, which makes it difficult to achieve efficient separation and recovery of titanium and iron in traditional strong magnetic + flotation or strong magnetic + reselection processes. The recovery rate of the existing technology is low and cannot be achieved. Economic use.

Method used

Flash roasting and reducing iron oxide technology, including magnetic separation after crushing and grinding, high-gradient magnetic separation, flash roasting, magnetic separation after grinding and shaker reselecting, and improved by magnetic separation pre-enrichment and flash magnetization roasting. Recovery rate of titanium and iron.

Benefits of technology

It significantly improves the recovery rate and grade of titanium and iron, reduces the reduction cost, and realizes the comprehensive recycling of vanadium, titanium and iron, with low ore dressing costs, making it easier to promote on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118045697B_ABST
    Figure CN118045697B_ABST
Patent Text Reader

Abstract

The present invention discloses a process for beneficiating weathered vanadium-titanium iron ore, comprising the following steps: (1) crushing and grinding the raw ore, and then feeding it into a bucket magnetic separator for magnetic separation; (2) using a high gradient magnetic separator to magnetically separate the non-magnetic product; (3) flash roasting the mixed coarse concentrate; (4) grinding the roasted product and then feeding it into a bucket magnetic separator for magnetic separation; (5) feeding the tailings into a shaking table for re-selection to obtain titanium concentrate and shaking table tailings. The present invention adopts a magnetic separation pre-enrichment process flow, and the pre-selection effect is very significant, the selected grade is also greatly improved, the reduction cost and the total cost are greatly reduced, and the efficiency is high and the reduction product has high magnetic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing, and in particular to a weathering type vanadium-titanium iron ore dressing process. Background Art

[0002] Weathered vanadium-titanium iron ore has high vanadium, titanium and iron valuable metal contents, and is an important supplement to vanadium and titanium resources. It is rich in reserves in Russia, Australia, Africa, New Zealand and other places. Since the iron and titanium minerals in weathered vanadium-titanium iron ore are closely interwoven, conventional beneficiation methods are difficult to separate titanium and iron. With the growing demand for vanadium and titanium resources at home and abroad, it is of great significance to increase research on the recycling technology of this type of vanadium-titanium iron ore.

[0003] At present, the existing technologies for the beneficiation process of weathered vanadium-titanium iron ore mainly include: the patent with the authorization announcement number of CN104174486B, which discloses the "weathered sand ilmenite beneficiation combined magnetic separation process", and the method process is: through pulping, screening and discarding, strong magnetic tailings, screening, fine ore first collection, coarse grain re-grinding, one fine and two scavenging, drying and beneficiation steps, titanium ore concentrate with a grade content of 46-52% and iron ore concentrate with a grade content of 40-65%. The present invention can realize the relative independence of the production of coarse ore, medium ore and concentrate, and can adjust the output and grade of titanium medium ore and titanium concentrate, and separate refined titanium and refined iron in turn. The patent with the publication number of CN108993766A discloses "a beneficiation treatment method for weathered ilmenite", which is characterized in that the steps of its beneficiation process are: A, pre-screening; B, weak magnetic separation; C, strong magnetic separation; D, pre-classification; E, flotation. The present invention is directed to a mineral processing method for weathered ilmenite, which effectively improves the recovery rate of titanium, and simultaneously obtains titanium concentrate and iron concentrate, with a simple process, easy operation of the process, and easy promotion. The Chinese invention patent document with publication number CN109847923B discloses "a recovery process for extremely poor weathered primary ilmenite", which specifically includes three steps: pre-treatment, pre-enrichment, and efficient separation. The pre-treatment is to crush the ore to a suitable particle size, and then use a gravity magnetic pull concentrator for wet tailings to obtain tailings concentrate and tailings; pre-enrichment is to finely grind the tailings concentrate, and then use a spiral chute for enrichment to obtain spiral concentrate and spiral tailings; efficient separation is to dry the spiral concentrate, and then use a combined iron-titanium separator for separation to obtain iron concentrate, titanium concentrate, and titanium tailings.

[0004] The current problem with the process is that the weathered vanadium-titanium iron ore is severely weathered and is a deeply oxidized ore. The relationship between iron minerals and titanium minerals is relatively complex. Hematite, (altered) ilmenite, and limonite minerals account for about 80% of the total amount, and the interpenetration relationship between them is very close. Even if qualified titanium concentrate products can be obtained by using traditional strong magnetic + flotation process or strong magnetic + gravity separation process, the recovery rate is very low and the ore cannot be economically utilized. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention proposes a weathering type vanadium-titanium iron ore beneficiation process, which utilizes flash roasting to reduce iron oxide and has strong operability.

[0006] The technical solution of the present invention is as follows:

[0007] A weathering vanadium-titanium iron ore beneficiation process comprises the following steps:

[0008] S1: crushing and grinding the raw ore and then performing magnetic separation to obtain a magnetic vanadium-containing iron concentrate 1 and a non-magnetic product;

[0009] S2: Use a high gradient magnetic separator to magnetically separate the non-magnetic products to obtain a mixed coarse concentrate;

[0010] S3: flash roasting the mixed coarse concentrate to obtain a magnetized roasting product;

[0011] S4: grinding the magnetized roasting product and performing magnetic separation to obtain vanadium-containing iron concentrate 2 and tailings;

[0012] S5: Send the tailings to the shaking table for re-selection to obtain titanium concentrate and shaking table tailings.

[0013] In some embodiments, in the weathered vanadium-titanium iron ore, hematite / hematite+limonite ≥ 50 wt %, and kaolin ≥ 10 wt %.

[0014] In some embodiments, the magnetic field strength of the magnetic separation in step S1 is 0.32-0.36T.

[0015] In some embodiments, the grinding fineness in step S1 is a particle diameter less than 0.1 mm.

[0016] In some embodiments, the magnetic field strength of the magnetic separation in step S2 is 0.6-0.65T.

[0017] In some embodiments, the flash roasting operation steps in step S3 are as follows: the mixed coarse concentrate and blast furnace gas are sprayed into the reaction tower through a nozzle, and the material falls from the upper end to the lower end of the reaction tower in a highly dispersed floating state. During this process, the iron oxide in the material is reduced to ferroferric oxide by carbon monoxide.

[0018] In some embodiments, the volume fraction of carbon monoxide in blast furnace gas is 25.3-26.2%, and the temperature of the reaction tower is 815-817°C.

[0019] In some embodiments, the magnetic field strength of the magnetic separation in step S4 is 0.32-0.35T.

[0020] In some embodiments, in step S4, the proportion of ore particles with a diameter less than 0.075 mm is ≥ 83%.

[0021] In some embodiments, the magnetic separation in step S4 includes a rough separation and a fine separation.

[0022] Beneficial effects:

[0023] (1) The present invention adopts a magnetic separation pre-enrichment process flow, the pre-selection effect is very significant, the selected grade is also greatly improved, and the reduction cost and total cost are greatly reduced.

[0024] (2) The flash magnetization roasting method used in the present invention avoids the high energy consumption and high cost of carbon reduction, and achieves high efficiency and high magnetic properties of the reduction product, which is conducive to the subsequent magnetic separation of titanium ore and iron ore.

[0025] (3) The present invention adopts the ore dressing pre-enrichment flash magnetization roasting magnetic separation enrichment shaking table re-selection smelting process, and the vanadium-containing iron concentrate TFe≥61wt%, the recovery rate≥75%, V 2 O 5 ≥1wt%, recovery rate ≥77%, titanium concentrate TiO 2 ≥50wt%, titanium recovery rate ≥53%, realizing the comprehensive recovery of vanadium, titanium and iron in the difficult-to-select weathered vanadium-titanium iron ore, with low ore dressing cost and convenient for large-scale promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the process of weathering vanadium-titanium iron ore beneficiation of the present invention. DETAILED DESCRIPTION

[0027] The present invention will be further described in detail below in conjunction with the accompanying drawings. The embodiments described with reference to the accompanying drawings are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.

[0028] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or system. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or system including the element.

[0029] like Figure 1 As shown, a weathering type vanadium-titanium iron ore beneficiation process comprises the following steps:

[0030] S1: After the raw ore is crushed and ground to a particle diameter of less than 0.1 mm, it is sent to a barrel magnetic separator for magnetic separation to obtain a magnetic vanadium-containing iron concentrate 1 and a non-magnetic product. The magnetic field strength of the magnetic separation is 0.32-0.36 T;

[0031] S2: Use a high gradient magnetic separator to perform high gradient magnetic separation on the non-magnetic product to obtain a mixed coarse concentrate with a magnetic separation intensity of 0.6 to 0.65T;

[0032] S3: flash roasting the mixed coarse concentrate to obtain a magnetized roasting product, wherein the flash roasting operation steps are as follows: the mixed coarse concentrate and blast furnace gas are sprayed into a reaction tower at a temperature of 815-817° C. through a nozzle, and the material falls from the upper end to the lower end of the reaction tower in a highly dispersed floating state. During this process, the iron oxide in the material is reduced to ferroferric oxide by carbon monoxide, and the volume fraction of carbon monoxide in the blast furnace gas is 25.3-26.2%;

[0033] S4: Grinding the magnetized roasted product, the proportion of ore particles with a particle diameter less than 0.075 mm is ≥83%, and then the product is sent to a barrel magnetic separator for primary concentration and primary magnetic separation, the magnetic field strength of the magnetic separation is 0.32-0.35T, and vanadium-containing iron concentrate 2 is obtained after magnetic separation, and the roughing and concentrating tailings are combined;

[0034] S5: Send the tailings to the shaking table for re-selection to obtain titanium concentrate and shaking table tailings.

[0035] The serial numbers of the following embodiments of the present invention are for description only and do not represent the advantages or disadvantages of the embodiments.

[0036] Iron minerals are mainly hematite (titanium) iron ore, limonite and a small amount of magnetite. Vanadium is mainly found in iron minerals. Titanium minerals are mainly ilmenite and altered ilmenite. Gangue minerals are mainly clay minerals, mainly kaolin. Most iron minerals contain ilmenite lamellae or inclusions, which form a complex and difficult-to-dissociate intergrowth relationship between ilmenite minerals. Hematite and ilmenite are intergrowth, and hematite contains fine-grained ilmenite and ilmenite lamellae, showing irregular ilmenite, altered ilmenite and limonite closely intergrowth. Kaolin, the main gangue mineral in the ore, is a loose aggregate, and most kaolin is non-magnetic or weakly magnetic.

[0037] Embodiment 1:

[0038] A weathered vanadium-titanium iron ore sample comes from a foreign vanadium-titanium iron ore deposit. The main element analysis results of the ore are: TFe43.72wt%, V 2 O 5 0.72wt%TiO 2 13.56wt%Al 2 O 3 8.36wt%SiO 2 9.24wt%.

[0039] To achieve this, follow these steps:

[0040] S1: After the raw ore is crushed and ground to less than 0.1 mm, it is sent to a barrel magnetic separator for magnetic separation to obtain magnetic vanadium-containing iron concentrate 1 and non-magnetic products. The magnetic field intensity of the magnetic separation is 0.33T;

[0041] S2: The non-magnetic product of the previous step is subjected to high gradient magnetic separation using a high gradient magnetic separator with a magnetic field strength of 0.6 T to obtain a mixed coarse concentrate;

[0042] S3: The mixed coarse concentrate and blast furnace gas with a carbon monoxide volume fraction of 25.7% are sprayed into a reaction tower with a height of 3 meters and a temperature of 815°C through a nozzle. The materials float from the upper end of the reaction tower to the lower end in a highly dispersed floating state, and are reduced to obtain a magnetized roasted product;

[0043] S4: Grind the product of the previous step of magnetization roasting, and then send it to a barrel magnetic separator for a roughing separation and a fine separation, with a magnetic field strength of 0.35T, to obtain vanadium-containing iron concentrate 2, and combine the roughing and fine separation tailings for standby use;

[0044] S5: Send the tailings from the previous step to the shaking table for re-selection to obtain titanium concentrate and shaking table tailings.

[0045] In this example, vanadium-containing iron concentrate TFe 61.42wt%, recovery rate 76.27%, V 2 O 5 1.15wt%, recovery rate 78.28%, titanium concentrate TiO 2 The recovery rate of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore was 50.13wt% and the titanium recovery rate was 53.31%, realizing the comprehensive recovery of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore.

[0046] Example 2

[0047] A weathered vanadium-titanium iron ore sample comes from a vanadium-titanium iron ore deposit in Australia. The main element analysis results of the ore are: TFe42.36wt%, V 2 O 5 0.69wt%TiO 2 14.37wt%Al 2 O 3 8.41wt%SiO 2 9.27wt%.

[0048] To achieve this, follow these steps:

[0049] S1: After the raw ore is crushed and ground to less than 0.1 mm, it is sent to a barrel magnetic separator for magnetic separation to obtain magnetic vanadium-containing iron concentrate 1 and non-magnetic products. The magnetic field intensity of the magnetic separation is 0.36T;

[0050] S2: The non-magnetic product of the previous step is subjected to high gradient magnetic separation using a high gradient magnetic separator with a magnetic field strength of 0.6 T to obtain a mixed coarse concentrate;

[0051] S3: The mixed coarse concentrate and blast furnace gas with a carbon monoxide volume fraction of 26.2% are sprayed into a reaction tower with a height of 3 meters and a temperature of 817°C through a nozzle. The materials float from the upper end of the reaction tower to the lower end in a highly dispersed floating state, and are reduced to obtain a magnetized roasting product;

[0052] S4: Grind the product of the previous step of magnetization roasting, and then send it to a barrel magnetic separator for a roughing separation and a fine separation, with a magnetic field strength of 0.35T, to obtain vanadium-containing iron concentrate 2, and combine the roughing and fine separation tailings for standby use;

[0053] S5: Send the tailings from the previous step to the shaking table for re-selection to obtain titanium concentrate and shaking table tailings.

[0054] In this example, vanadium-containing iron concentrate TFe 60.73wt% and recovery rate 75.72% were obtained. 2 O 5 1.03wt%, recovery rate 77.35%, titanium concentrate TiO 2 The recovery rate of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore was 50.35wt% and the titanium recovery rate was 54.37%, realizing the comprehensive recovery of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore.

[0055] Example 3

[0056] A weathered vanadium-titanium iron ore sample comes from a vanadium-titanium iron ore deposit in New Zealand. The main element analysis results of the ore are: TFe42.89wt%, V 2 O 5 0.73wt%TiO 2 13.28wt%Al 2 O 3 8.19wt%SiO 2 9.41wt%.

[0057] To achieve this, follow these steps:

[0058] S1: After the raw ore is crushed and ground to less than 0.1 mm, it is sent to a barrel magnetic separator for magnetic separation to obtain magnetic vanadium-containing iron concentrate 1 and non-magnetic products. The magnetic field intensity of the magnetic separation is 0.35T;

[0059] S2: The non-magnetic product of the previous step is subjected to high gradient magnetic separation using a high gradient magnetic separator with a magnetic field strength of 0.6 T to obtain a mixed coarse concentrate;

[0060] S3: The mixed coarse concentrate and blast furnace gas with a carbon monoxide volume fraction of 25.3% are sprayed into a reaction tower with a height of 3 meters and a temperature of 816°C through a nozzle. The materials float from the upper end of the reaction tower to the lower end in a highly dispersed floating state, and are reduced to obtain a magnetized roasted product;

[0061] S4: Grind the product of the previous step of magnetization roasting, and then send it to a barrel magnetic separator for a roughing separation and a fine separation, with a magnetic field strength of 0.35T, to obtain vanadium-containing iron concentrate 2, and combine the roughing and fine separation tailings for standby use;

[0062] S5: Send the tailings from the previous step to the shaking table for re-selection to obtain titanium concentrate and shaking table tailings.

[0063] In this example, vanadium-containing iron concentrate TFe 60.82wt% and recovery rate 76.18% were obtained. 2 O 5 1.24wt%, recovery rate 77.42%, titanium concentrate TiO 2 The recovery rate of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore was 50.21wt% and the titanium recovery rate was 52.37%, realizing the comprehensive recovery of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore.

[0064] Example 4

[0065] A weathered vanadium-titanium iron ore sample comes from a vanadium-titanium iron ore deposit in New Zealand. The main element analysis results of the ore are: TFe42.37wt%, V 2 O 5 0.68wt%TiO 2 14.03wt%Al 2 O 3 8.39wt%,SiO 2 9.52wt%.

[0066] To achieve this, follow these steps:

[0067] S1: After the raw ore is crushed and ground to less than 0.1 mm, it is sent to a barrel magnetic separator for magnetic separation to obtain magnetic vanadium-containing iron concentrate 1 and non-magnetic products. The magnetic field intensity of the magnetic separation is 0.35T;

[0068] S2: The non-magnetic product of the previous step is subjected to high gradient magnetic separation using a high gradient magnetic separator with a magnetic field strength of 0.6 T to obtain a mixed coarse concentrate;

[0069] S3: The mixed coarse concentrate and blast furnace gas with a carbon monoxide volume fraction of 25.5% are sprayed into a reaction tower with a height of 3 meters and a temperature of 816°C through a nozzle. The materials float from the upper end of the reaction tower to the lower end in a highly dispersed floating state, and are reduced to obtain a magnetized roasting product;

[0070] S4: Grind the product of the previous step of magnetization roasting, and then send it to a barrel magnetic separator for a roughing separation and a fine separation, with a magnetic field strength of 0.35T, to obtain vanadium-containing iron concentrate 2, and combine the roughing and fine separation tailings for standby use;

[0071] S5: Send the tailings from the previous step to the shaking table for re-selection to obtain titanium concentrate and shaking table tailings.

[0072] In this example, vanadium-containing iron concentrate TFe 60.36wt% and recovery rate 76.28% were obtained. 2 O 5 1.05wt%, recovery rate 76.63%, titanium concentrate TiO 2 The recovery rate of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore was 50.48wt% and the titanium recovery rate was 53.62%, realizing the comprehensive recovery of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore.

[0073] Comparative Example 1

[0074] Weathered vanadium-titanium iron ore sample is the same as Example 1

[0075] To achieve this, follow these steps:

[0076] S1: After the raw ore is crushed and ground to less than 0.1 mm, it is sent to a barrel magnetic separator for magnetic separation to obtain magnetic vanadium-containing iron concentrate 1 and non-magnetic products. The magnetic field intensity of the magnetic separation is 0.2T;

[0077] S2: The non-magnetic product of the previous step is subjected to high gradient magnetic separation using a high gradient magnetic separator with a magnetic field strength of 0.5 T to obtain a mixed coarse concentrate;

[0078] S3: The mixed coarse concentrate and air with a carbon monoxide mass percentage concentration of 0.95% are sprayed into a reaction tower with a height of 3 meters and a temperature of 816°C through a nozzle. The materials float from the upper end of the reaction tower to the lower end in a highly dispersed floating state, and are reduced to obtain a magnetized roasting product;

[0079] S4: Grind the product of the previous step of magnetization roasting, and then send it to a barrel magnetic separator for a roughing separation and a fine separation, with a magnetic field strength of 0.35T, to obtain vanadium-containing iron concentrate 2, and combine the roughing and fine separation tailings for standby use;

[0080] S5: Send the tailings from the previous step to the shaking table for re-selection to obtain titanium concentrate and shaking table tailings.

[0081] In this example, vanadium-containing iron concentrate TFe 61.36wt%, recovery rate 70.32%, V 2 O 5 1.02wt%, recovery rate 71.83%, titanium concentrate TiO 2The recovery rate of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore was 49.25wt% and the titanium recovery rate was 48.51%, realizing the comprehensive recovery of vanadium, titanium and iron in the refractory weathered vanadium-titanium iron ore.

[0082] It can be seen that the process parameters used in Comparative Example 1 are different from those in the embodiment of the present application. In the comparative example, air with a carbon monoxide mass percentage concentration of 0.95% is used for roasting, and the magnetic field strength of the magnetic separation is also different from that in the embodiment of the present application. The vanadium-containing iron concentrate, V 2 O 5 、TiO 2 The recovery rates are lower than those of other embodiments of the present application.

[0083] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A weathering vanadium-titanium iron ore beneficiation process, characterized in that: The following steps are involved: S1: After the raw ore is crushed and ground to a particle diameter of less than 0.1 mm, it is sent to a barrel magnetic separator for magnetic separation at a magnetic field strength of 0.32 to 0.36 T. After the magnetic separation is completed, a magnetic vanadium-containing iron concentrate 1 and a non-magnetic product are obtained; S2: Use a high gradient magnetic separator to magnetically separate the non-magnetic products at a magnetic field strength of 0.6 to 0.65 T to obtain a mixed coarse concentrate; S3: The mixed coarse concentrate and blast furnace gas with a carbon monoxide volume fraction of 25.3-26.2% are sprayed together through a nozzle into a reaction tower with a height of 3 meters and a temperature of 815-817°C. The materials float from the upper end of the reaction tower to the lower end in a highly dispersed floating state, and are reduced to obtain a magnetized roasting product; S4: Grinding the magnetized roasted product to a grinding fineness of ≥83% of particles with a diameter less than 0.075 mm, and feeding the ground product into a barrel magnetic separator for primary roughing and primary fine separation at a magnetic field strength of 0.32 to 0.35 T, and obtaining vanadium-containing iron concentrate 2 and tailings after magnetic separation; S5: Send the tailings to the shaking table for re-selection to obtain titanium concentrate and shaking table tailings.

2. A weathered vanadium-titanium iron ore beneficiation process according to claim 1, characterized in that: In the weathered vanadium-titanium iron ore, magnetic hematite / hematite+limonite≥50wt%, and kaolin≥10wt%.