A colloidal electrolyte for aqueous zinc-manganese batteries, its preparation method and application

By adding hydrophilic nano-silica and ferrous sulfate to the electrolyte of aqueous zinc-manganese batteries, the problem of poor irreversibility of manganese dioxide dissolution/deposition was solved, achieving efficient manganese dioxide dissolution/deposition, improving the coulombic efficiency and cycle stability of the battery, and making it suitable for industrial applications.

CN118099557BActive Publication Date: 2026-11-17CENT SOUTH UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410071609.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-17
Publication Date
2026-11-17
Estimated Expiration
2044-01-17

AI Technical Summary

Technical Problem

In existing aqueous zinc-manganese batteries, the dissolution/deposition process of manganese dioxide is poorly irreversible, leading to fluctuations in electrolyte pH, corrosion of the zinc anode, and affecting the battery's coulombic efficiency and lifespan.

Method used

Adding hydrophilic nano-silica and ferrous sulfate to the electrolyte as gelling agents and redox media promotes the dissolution/deposition of manganese dioxide. By constructing the positive electrode double layer and chemical reactions, the deposition efficiency of manganese dioxide and the cycle stability of the battery are improved.

Benefits of technology

It improves the dissolution/deposition efficiency of manganese dioxide, enhances the coulombic efficiency and cycle stability of the battery, extends its service life, and has low raw material costs, making it suitable for industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118099557B_ABST
    Figure CN118099557B_ABST
Patent Text Reader

Abstract

This invention provides a colloidal electrolyte for aqueous zinc-manganese batteries, comprising a solvent and an electrolyte. The solvent is water, and the electrolyte contains zinc salt, manganese salt, additives, and an organic / inorganic acid that provides additional protons when MnO2 dissolves. The additives include a gelling agent and ferrous sulfate. The mass of the gelling agent accounts for 5-12.5% ​​of the electrolyte mass, and the molar concentration of ferrous sulfate is 0.005-0.02 mol / L. The colloidal electrolyte for aqueous zinc-manganese batteries provided by this invention can effectively promote the dissolution / deposition efficiency of manganese dioxide during charge and discharge. Aqueous zinc-manganese batteries assembled with this colloidal electrolyte have advantages such as high voltage, high coulombic efficiency, good cycle stability, and large areal capacity. Furthermore, it is simple and efficient to prepare, and has industrial application value. This invention also provides a method for preparing the colloidal electrolyte for aqueous zinc-manganese batteries and its application in electrolytic aqueous zinc-manganese batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of secondary battery technology, specifically to the field of aqueous zinc-ion battery technology, and particularly to a colloidal electrolyte for aqueous zinc-manganese batteries, its preparation method, and its application. Background Technology

[0002] With the further depletion of fossil fuels and the urgent need for environmental governance, the demand for and exploration of clean energy has greatly increased. Lithium-ion batteries have achieved high commercialization due to their excellent performance, but because they use anhydrous organic solutions as electrolytes, they still suffer from disadvantages such as poor safety and high cost. Aqueous zinc-ion batteries, with their controllable cost, inherent safety of water, and low electrode potential (-0.762V vs SHE), are considered a promising potential competitor. However, using water as an electrolyte also brings certain challenges to aqueous zinc-ion batteries. Limited by the narrow electrochemical window (ESW) of water molecules, traditional aqueous zinc-ion batteries typically operate at voltages below 1.8V, resulting in lower energy density. Meanwhile, manganese-based (Mn) zinc-ion batteries... 2+ The positive electrode of manganese dioxide (MnO2) dissolution / deposition mechanism has advantages such as extremely high redox potential (1.23V vs SHE) and high capacity (616mAh / g) when combined with zinc negative electrode to realize high voltage and high energy density aqueous zinc-manganese battery.

[0003] Currently, the low conductivity of manganese dioxide during electrodeposition and the poor reversibility of dissolution / deposition during charge and discharge lead to the accumulation of manganese dioxide on the carbon felt and the extra protons generated by incomplete discharge. This causes significant pH fluctuations in the electrolyte during cycling, further resulting in capacity fluctuations and severe hydrogen evolution at the zinc anode. Consequently, zinc-manganese batteries suffer from unsatisfactory coulombic efficiency and short lifespan, hindering the application of aqueous zinc-manganese batteries. Lu Yijun's research group introduced iodide ions as a redox medium into zinc acetate and manganese acetate electrolytes, effectively promoting the dissolution of manganese dioxide during discharge. Simultaneously, the buffering effect of acetate ions effectively mitigated pH changes in the electrolyte. Li Xianfeng's team at the Dalian Institute of Chemical Physics, Chinese Academy of Sciences, achieved a high-voltage and high-energy-density zinc-manganese flow battery by adding bromide ions to the electrolyte. The electrolyte improvements of the two technical solutions mentioned above promote the dissolution of manganese dioxide on the solution side, but they do not solve the problem of poor reversibility during the deposition of manganese dioxide. The irreversible dissolution of manganese dioxide will lead to the accumulation of hydrogen ions, causing the pH value to drop and thus causing corrosion of the zinc negative electrode, thereby affecting the electrochemical performance and cycle life of zinc-manganese batteries.

[0004] The paper "Unraveling deposition / dissolution chemistry of MnO2 for high-energy aqueous batteries" (Energy & Environmental Science, Jiafeng Lei, Yanxin Yao, Zengyue Wang and Yi-Chun Lu, 2021.7) explores the introduction of ferrous sulfate as a redox medium into the electrolyte to achieve reversible dissolution and deposition of manganese dioxide under strongly acidic conditions, thus achieving efficient cycling with a low areal capacity. However, this technical solution only promotes the efficient conversion of manganese dioxide from the dissolution side, neglecting the impact of the deposition side on electrochemical performance.

[0005] Therefore, improving the dissolution / deposition of manganese dioxide is of great significance for enhancing the coulombic efficiency and lifespan of aqueous zinc-manganese batteries. Summary of the Invention

[0006] The purpose of this invention is to provide a colloidal electrolyte for aqueous zinc-manganese batteries, its preparation method, and its application. This electrolyte can effectively promote the dissolution / deposition efficiency of manganese dioxide during the charging and discharging process. Aqueous zinc-manganese batteries assembled with this colloidal electrolyte have advantages such as high voltage, high coulombic efficiency, good cycle stability, and large areal capacity. Moreover, it is simple and efficient to prepare and has industrial application value.

[0007] The first aspect of the present invention is to provide a colloidal electrolyte for an aqueous zinc-manganese battery, comprising a solvent and an electrolyte, wherein the solvent is water, the electrolyte comprises a zinc salt, a manganese salt, additives, and an organic / inorganic acid that provides additional protons when MnO2 dissolves, wherein the additives comprise a gelling agent and ferrous sulfate, the mass of the gelling agent being 5-12.5% ​​of the mass of the electrolyte, and the molar concentration of ferrous sulfate being 0.005-0.02 mol / L;

[0008] The amount of gelling agent added is 5%, 7.5%, 10%, or 12.5% ​​of the electrolyte mass, or other values ​​within this range; the concentration of ferrous sulfate is 0.005 mol / L, 0.01 mol / L, or 0.02 mol / L, or other values ​​within this range.

[0009] Furthermore, the gelling agent is any one or a composite of several of hydrophilic nano-silica, reduced graphene oxide, graphene oxide, starch, and montmorillonite.

[0010] Furthermore, the gelling agent is hydrophilic nano-silica.

[0011] Preferably, the hydrophilic nano-silica accounts for 7.5% of the mass of the electrolyte.

[0012] Preferably, the concentration of ferrous sulfate is 0.02 mol / L.

[0013] Furthermore, the concentration of zinc salt in the electrolyte is 1-2 mol / L, and the concentration of manganese salt is 1-2 mol / L.

[0014] Furthermore, the zinc salt is zinc sulfate, and the manganese salt is manganese sulfate.

[0015] Furthermore, the molar concentration of the organic acid / inorganic acid is 0.1 mol / L-0.2 mol / L. The organic acid can be one of acetic acid, formic acid, citric acid, or methanesulfonic acid, and the inorganic acid can be sulfuric acid or hydrochloric acid.

[0016] The second aspect of this invention provides a method for preparing a colloidal electrolyte for aqueous zinc-manganese batteries. This method is simple, efficient, and allows for mass production at low cost, effectively improving production efficiency and reducing production costs. The specific preparation method includes the following steps:

[0017] Step S1: Prepare zinc sulfate solution and manganese sulfate solution, and mix the zinc sulfate solution and manganese sulfate solution thoroughly;

[0018] Step S2: Weigh an appropriate amount of ferrous sulfate, gelling agent, and organic / inorganic acid, add them to the mixed solution from step S1, and shake until completely dissolved to obtain the aqueous zinc-manganese battery colloidal electrolyte.

[0019] A third aspect of the present invention is to provide an application of a colloidal electrolyte for aqueous zinc-manganese batteries in electrolytic aqueous zinc-manganese batteries.

[0020] An electrolytic aqueous zinc-manganese battery includes a positive electrode, a negative electrode, and an electrolyte, wherein the electrolyte is the colloidal electrolyte for aqueous zinc-manganese batteries described in the first aspect. This electrolyte has the advantages of improving the dissolution / deposition efficiency of manganese dioxide at the positive electrode and improving the cycle stability of the battery. The positive electrode is manganese dioxide, and the negative electrode is a zinc negative electrode, which can be a paste electrode, a foam electrode, or a sheet electrode. The positive electrode current collector is a solid network with high electronic conductivity, selected from one or more composites of carbon felt, carbon paper, carbon cloth, graphite felt, graphene film, graphene mesh, carbon nanotube film, carbon nanotube paper, conductive activated carbon film, mesoporous carbon film, conductive graphite plate, and conductive graphite mesh.

[0021] Combination Figure 1 As shown, the main electrode reactions of this battery are as follows:

[0022] Charging process:

[0023] Positive electrode: Fe 2+ →Fe 3+ +e -

[0024] Mn 2+ +2H₂O→MnO₂+4H₂O+2e -

[0025] Negative electrode: Zn 2+ +2e - →Zn

[0026] Discharge process:

[0027] Positive electrode: MnO2 + 4H + +2e - →Mn 2+ +3H2O

[0028] Fe 3+ +e - →Fe 2+

[0029] 2Fe 2+ +MnO2+4H + →2Fe 3+ +Mn 2+ +2H2O

[0030] Negative electrode: Zn → Zn 2+ +2e -

[0031] Compared with the prior art, the aqueous zinc-manganese battery colloidal electrolyte, its preparation method, and its application provided by this invention have the following advantages:

[0032] The aqueous zinc-manganese battery colloidal electrolyte provided by this invention incorporates hydrophilic nano-silica and other gelling agents as colloidal components. Since the negative potential on the surface of the colloidal hydrophilic nano-silica participates in the construction of the positive electrode double layer, it effectively enhances the nucleation of manganese dioxide on the electrode surface during charging, thereby effectively inhibiting the diffusion of manganese in the electrolyte, improving manganese dioxide deposition efficiency, and increasing the coulombic efficiency of the battery.

[0033] II. The aqueous zinc-manganese battery colloidal electrolyte provided by this invention uses ferrous sulfate as an electrolyte additive. Through its redox chemical reaction with manganese dioxide, it effectively promotes the dissolution of manganese dioxide positive electrode during discharge, avoids the accumulation of manganese dioxide on the surface of the positive electrode current collector, and improves the effective reaction area of ​​the battery.

[0034] Third, the aqueous zinc-manganese battery colloidal electrolyte provided by this invention uses both the colloidal component and ferrous sulfate as electrolyte additives. Due to the extremely high specific surface area of ​​the selected colloidal component, more reaction sites are provided for the reaction between ferrous ions and manganese dioxide. The two synergistically promote the dissolution / deposition of manganese dioxide, improving the cycle stability of the battery.

[0035] IV. Compared with existing battery systems, the electrolytic aqueous zinc-manganese battery provided by this invention uses inexpensive raw materials, is simple to prepare, and does not involve harmful elements such as lead (Pb), cadmium (Cd), and vanadium (V). Furthermore, due to the addition of hydrophilic nano-silica and ferrous ions in the electrolyte, the dissolution / deposition reaction is sufficient during each charge-discharge cycle, resulting in thorough electrode regeneration and exhibiting a longer cycle life and cycle stability. This demonstrates significant application prospects and research value in the field of aqueous zinc-manganese batteries. Attached Figure Description

[0036] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0037] Figure 1 A schematic diagram illustrating the working principle of a zinc-manganese battery assembled using a colloidal electrolyte with ferrous sulfate and hydrophilic nano-silica as additives.

[0038] Figure 2 This is a schematic diagram of different electrolytes used in Example 1;

[0039] Figure 3 Cyclic voltammetry curves were obtained using colloidal electrolytes containing ferrous sulfate, ferrous sulfate, and manganese sulfate as described in Example 2.

[0040] Figure 4 SEM images of carbon felt after 25 cycles of the electrolyte solution used in Example 3 with added ferrous sulfate and hydrophilic nano silica gel and the electrolyte solution of the control group;

[0041] Figure 5 Electrochemical performance test graphs of static batteries assembled using different electrolytes in Example 4;

[0042] Figure 6 The cycling performance of the homemade battery using the colloidal electrolyte containing ferrous sulfate and hydrophilic nano-silica from Example 5 is shown in the graph.

[0043] Figure 7 The cycling performance graphs are shown for the electrolyte of Example 6 with added ferrous sulfate and hydrophilic nano silica gel and the electrolyte of the control group after 25 cycles.

[0044] Figure 8 The graph shows the electrochemical performance test results of static batteries assembled using different mass fractions of colloidal electrolyte from Example 7.

[0045] Figure 9The graph shows the electrochemical performance test results of the static batteries assembled using colloidal electrolytes with different concentrations of ferrous sulfate additives from Example 8.

[0046] Figure 10 The graph shows the electrochemical performance test results of static batteries assembled using different types of colloidal electrolytes from Example 9. Detailed Implementation

[0047] To enable those skilled in the art to better understand the technical solutions in the embodiments of the present invention, and to make the above-mentioned objectives, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be further described below.

[0048] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0049] Example 1

[0050] Dissolve 0.1g of manganese dioxide in 5ml of deionized water, and simultaneously add hydrophilic nano-silica to a final concentration of 7.5% (w / w) to prepare a suspended manganese dioxide solution. Figure 2 As shown in (a);

[0051] Dissolve 0.1 g of ferrous sulfate in 5 ml of deionized water, then add sulfuric acid and hydrophilic nano-silica (final concentration of nano-silica: 7.5 wt%) to the solution to prepare a 0.1 mol / L ferrous sulfate colloidal solution. Figure 2 As shown in (b);

[0052] Dissolve 0.1 g of manganese dioxide and 0.1 g of ferrous sulfate in 5 ml of deionized water. Then add sulfuric acid and hydrophilic nano-silica (final concentration of nano-silica: 7.5 wt%) to this solution to prepare a 0.1 mol / L ferrous sulfate colloidal solution. Figure 2 As shown in (c).

[0053] like Figure 2 As shown in (a), the suspension of manganese dioxide is black, which can be attributed to the uniform suspension of black manganese dioxide in the solution; as Figure 2 As shown in (b), the prepared ferrous sulfate colloidal solution is milky white, mainly due to the milky white appearance of the hydrophilic nano-silica colloidal solution in water; Figure 2As shown in (c), when manganese dioxide and ferrous sulfate are mixed in an acidic solution, the colloid rapidly turns reddish-brown. This is because manganese dioxide and ferrous sulfate react rapidly, producing ferric ions, which are reddish-brown in color. These phenomena indicate that ferrous sulfate can directly react with manganese dioxide. Furthermore, adding ferrous sulfate to the electrolyte can dissolve some of the manganese dioxide that cannot be dissolved through electrochemical processes. Simultaneously, the generated ferric ions can be converted into ferrous sulfate through discharge on the carbon felt, further dissolving manganese dioxide.

[0054] Example 2

[0055] Prepare 20 ml of 0.01 mol / L ferrous sulfate solution and add hydrophilic nano silica gel with a final concentration of 7.5% by mass.

[0056] Prepare a 20 ml mixed solution of 0.01 mol / L ferrous sulfate and 1 mol / L manganese sulfate, and add hydrophilic nano silica with a final concentration of 7.5% by mass.

[0057] A static cell was assembled using a zinc sheet as the negative electrode and a carbon felt as the positive electrode current collector. The resulting cell was subjected to cyclic voltammetry testing using a 660E electrochemical workstation. The test results are as follows: Figure 3 As shown. Figure 3 As shown, Fe 2+ / Fe 3+ Working mechanism of redox couple and Fe 2+ / Fe 3+ and Mn 2+ The voltage of / MnO2. For colloidal electrolytes containing ferrous sulfate and manganese sulfate, it shows two redox processes. Compared to colloidal electrolytes without manganese sulfate, the first oxidation peak (approximately 1.65 V) corresponds to Fe. 2+ To Fe 3+ The conversion of Mn showed the same peak value in both colloidal electrolytes. The second oxidation peak (approximately 2.10 V) corresponds to Mn. 2+ MnO2, which only appears in electrolytes containing manganese ions. During reduction, MnO2 dissolves (approximately 1.82V) and Fe... 3+ The reduction (approximately 1.15V) occurs sequentially. Figure 3 The CV curves demonstrate the feasibility of chemical-electrochemical discharge in the battery system of this invention. In a solution containing only ferrous sulfate, only one redox peak appears, where the oxidation peak (approximately 1.65 V) corresponds to Fe. 2+ To Fe 3+ The transformation, the reduction peak corresponds to Fe 3+ The reduction (approximately 1.15 V). This CV result indicates that Fe... 2+ / Fe 3+Its redox potential is slightly lower than that of Mn. 2+ / MnO2, and also exhibits electrochemical reversibility. Results show that during the electrochemical process, Fe... 2+ Preferentially oxidized to Fe 3+ Subsequently Mn 2+ It undergoes oxidation to become MnO2, but during the discharge process, MnO2 first dissolves into Mn. 2+ However, due to poor electrochemical reversibility, some MnO2 remains, followed by Fe... 3+ Discharge transforms into Fe 2+ The Fe produced 2+ Oxidized to Fe by residual MnO2 3+ This eliminates dead manganese and achieves superior electrochemical reversibility and stability.

[0058] Example 3

[0059] A gel electrolyte for aqueous zinc-manganese batteries is prepared by the following method:

[0060] Prepare a mixed solution of 1 mol / L zinc sulfate and 1 mol / L manganese sulfate, then add hydrophilic nano silica to make its mass fraction 5%, add ferrous sulfate to make its concentration 0.01 mol / L, and add sulfuric acid with a final concentration of 0.1 mol / L. Stir for 10 min to make it uniformly dispersed to obtain the electrolyte.

[0061] In this embodiment, a zinc sheet is used as the negative electrode, and a carbon felt is used as the positive electrode current collector. The positive and negative electrodes are fixed on both sides of the electrolytic cell by platinum sheet electrodes, with a spacing of 1 cm. 20 ml of electrolyte is added to the electrolytic cell to assemble a static battery. An electrolyte without the addition of hydrophilic nano-silica and ferrous sulfate is used as a control group, and a static battery is assembled under the same conditions. The obtained battery is then subjected to electrochemical testing using the Xinwei electrochemical testing system, with a cycling condition of a current density of 8 mA / cm². 2 The circulating surface capacity is 5mAh / cm². 2 The process involved 25 cycles, and the deposition morphology of the carbon felt cathode with hydrophilic nano-silica and ferrous sulfate additives was observed after the cycles were completed.

[0062] The positive electrode of the static battery from the electrolyzer after cycling was disassembled and subjected to SEM testing. The results are as follows: Figure 4 As shown, where Figure 4 (a) Corresponds to a colloidal electrolyte containing hydrophilic nano-silica and ferrous sulfate; Figure 4 (b) Corresponds to the electrolyte without the addition of hydrophilic nano-silica and ferrous sulfate. Figure 4It can be seen that after adding hydrophilic nano-silica and ferrous sulfate additives, there is basically no manganese dioxide residue on the surface of the carbon felt, indicating that ferrous sulfate significantly promotes the dissolution of manganese dioxide.

[0063] Example 4

[0064] Prepare a 20 ml mixed solution of 0.02 mol / L ferrous sulfate, 1 mol / L manganese sulfate and 1 mol / L zinc sulfate, and simultaneously add sulfuric acid with a final concentration of 0.1 mol / L. Stir for 10 min to ensure uniform dispersion to obtain the ferrous sulfate electrolyte.

[0065] Prepare a 20 ml mixed solution of 1 mol / L manganese sulfate and 1 mol / L zinc sulfate, add hydrophilic nano silica with a final concentration of 7.5% by mass, then add ferrous sulfate with a final concentration of 0.01 mol / L, and finally add sulfuric acid with a final concentration of 0.1 mol / L. Stir for 10 min to disperse the solution evenly to obtain a ferrous sulfate colloidal electrolyte.

[0066] Prepare a 20 ml mixed solution of 1 mol / L manganese sulfate and 1 mol / L zinc sulfate, then add hydrophilic nano silica with a final concentration of 7.5% by mass and sulfuric acid with a final concentration of 0.1 mol / L, and stir for 10 min to disperse it evenly to obtain a colloidal electrolyte.

[0067] In this embodiment, the electrolyte without the addition of hydrophilic nano-silica or ferrous sulfate was used as a control group, and static batteries were assembled under the same conditions. A zinc sheet was used as the negative electrode, and a carbon felt was used as the positive electrode current collector. The positive and negative electrodes were fixed to both sides of the electrolytic cell with a 1cm gap via platinum electrodes. 20ml of electrolyte was added to the electrolytic cell, and a static battery was assembled. The obtained battery was then electrochemically tested using a Xinwei electrochemical testing system. Cycling conditions: Charging conditions: Current density 15mA / cm². 2 The charging surface capacity is 10mAh / cm². 2 Discharge conditions: current density 15 mA / cm² 2 The cutoff voltage is 0.8V. The results are as follows: Figure 5 As shown, the colloidal electrolyte containing ferrous sulfate exhibits excellent electrochemical performance, with a first-cycle coulombic efficiency of 93%. This is attributed to the synergistic effect of the ferrous sulfate medium and colloidal particles promoting the growth of Mn. 2+ / MnO2 dissolution / deposition. Compared to electrolytes containing only ferrous sulfate, the former exhibits a superior discharge plateau at high voltages (approximately 1.96V), attributed to the hydrophilic nano-silica acting as a nucleating agent, significantly promoting MnO2 dissolution / deposition. 3+The spontaneous disproportionation process promotes the deposition process, resulting in more manganese dioxide deposition. Compared to electrolytes containing only hydrophilic nano-silica gel, the former exhibits a second voltage plateau (approximately 1.44V) in its charge-discharge curve due to the presence of ferrous sulfate mediator. This significantly removes dead manganese on the current collector, improving battery stability. This demonstrates that the synergistic effect of ferrous sulfate mediator and colloidal particles not only promotes the deposition of manganese dioxide but also enhances the deposition of more manganese dioxide. 2+ The dissolution and deposition of MnO2 can also improve the electrochemical performance of the battery.

[0068] Example 5

[0069] Prepare a 50 ml mixed solution of 0.02 mol / L ferrous sulfate, 1 mol / L manganese sulfate and 1 mol / L zinc sulfate. Add hydrophilic nano silica with a final concentration of 7.5% by mass and sulfuric acid with a final concentration of 0.2 mol / L. Stir for 10 min to disperse the solution evenly to obtain the electrolyte.

[0070] A 7cm x 7cm zinc sheet was used as the negative electrode. A 6.5mm thick 7cm x 7cm carbon felt was used as the positive electrode current collector, with 2cm x 2cm tabs left at the top of both the positive and negative electrodes. 50ml of electrolyte and the positive and negative electrodes were added to a self-made battery mold (2cm x 7cm x 10cm) to assemble the battery. The resulting battery was then subjected to electrochemical testing using a Newway electrochemical testing system. Cycling conditions: charging current density 200mA / cm². 2 The discharge current density is 100 mA / cm². 2 The circulating surface capacity is 300mAh / cm². 2 .

[0071] The homemade battery assembled with a colloidal electrolyte containing ferrous sulfate exhibited excellent cycle stability under long-term cycling, as shown in the following results. Figure 6 As shown. By Figure 6 It can be seen that the colloidal electrolyte with ferrous sulfate as an additive has a significantly improved coulombic efficiency compared with the conventional liquid electrolyte, and its cycle stability is far superior to that of the conventional electrolyte. Even under a large capacity of 300mAh and a large current of 100mA, it can still cycle stably for 100 cycles (more than 600h).

[0072] Example 6

[0073] In this embodiment, the preparation method of the gel electrolyte for aqueous zinc-manganese batteries is as follows:

[0074] Prepare a 20 ml mixed solution of 1 mol / L zinc sulfate and 1 mol / L manganese sulfate, then add hydrophilic nano silica to make its mass fraction 7.5%, then add ferrous sulfate to make its concentration 0.01 mol / L, and finally add sulfuric acid with a final concentration of 0.1 mol / L. Stir for 10 min to make it uniformly dispersed to obtain the electrolyte.

[0075] The electrolyte from Example 6 was also applied to an aqueous zinc-manganese battery. The cycling conditions in this example were: current density 15 mA / cm². 2 The circulating surface capacity is 10mAh / cm². 2 .

[0076] The cycling stability of zinc-manganese full cells with ferrous sulfate as an additive in colloidal electrolyte under long-term cycling was observed, and the results are as follows: Figure 7 As shown. By Figure 7 It can be seen that, compared with conventional liquid electrolytes (which do not contain ferrous sulfate and gelling agents, but whose other components are the same as in this example), the colloidal electrolyte with added ferrous sulfate as an additive has a significantly improved coulombic efficiency, and its cycle stability is far superior to that of conventional electrolytes, even at 15 mA / cm². 2 The battery can still cycle stably for more than 500 cycles under high current density, while the control sample shows rapid capacity fluctuations, indicating that the accumulation of manganese dioxide in the positive electrode leads to battery instability.

[0077] Example 7

[0078] This embodiment analyzes the impact of different contents of nano-silica on battery performance, as detailed below:

[0079] (1) Prepare a 20 ml mixed solution of 1 mol / L manganese sulfate and 1 mol / L zinc sulfate, then add 5% hydrophilic nano silica, 0.01 mol / L ferrous sulfate, and 0.1 mol / L sulfuric acid, and stir for 10 min to disperse it evenly to obtain a colloidal electrolyte.

[0080] (2) Prepare a 20 ml mixed solution of 1 mol / L manganese sulfate and 1 mol / L zinc sulfate, then add hydrophilic nano silica with a final concentration of 7.5% by mass, ferrous sulfate with a final concentration of 0.01 mol / L, and sulfuric acid with a final concentration of 0.1 mol / L, and stir for 10 min to disperse it evenly to obtain a colloidal electrolyte.

[0081] (3) Prepare a 20ml mixed solution of 1mol / L manganese sulfate and 1mol / L zinc sulfate, then add hydrophilic nano silica with a final concentration of 12.5% ​​by mass, ferrous sulfate with a final concentration of 0.01mol / L, and sulfuric acid with a final concentration of 0.1mol / L, and stir for 10min to disperse it evenly to obtain a colloidal electrolyte.

[0082] In this embodiment, the three electrolytes are identical in composition and concentration except for the mass fraction of colloidal particles. Static batteries are assembled under the same conditions. A zinc sheet is used as the negative electrode, and a carbon felt is used as the positive electrode current collector. The positive and negative electrodes are fixed to opposite sides of the electrolytic cell via platinum electrodes, with a 1cm gap. 20ml of electrolyte is added to the electrolytic cell, and a static battery is assembled. The obtained battery is then subjected to electrochemical testing using a Xinwei electrochemical testing system under the following cycling conditions:

[0083] Charging conditions: current density 15 mA / cm² 2 The charging surface capacity is 10mAh / cm². 2 The discharge conditions are: current density 15 mA / cm². 2 The cutoff voltage is 0.8V.

[0084] The results are as follows Figure 8 As shown, electrolytes with different colloidal particle mass fractions exhibit drastically different electrochemical performance. The colloidal electrolyte with 5% hydrophilic nano-silica shows similar electrochemical performance to conventional electrolytes, but with low coulombic efficiency and significant fluctuations after 80 cycles. This is attributed to the low number of colloidal particles failing to effectively form a stable colloid, thus hindering manganese dioxide deposition and resulting in unstable electrochemical performance. The 7.5% colloidal electrolyte, due to its suitable colloidal concentration, exhibits stable electrochemical performance. For the 12.5% ​​colloidal electrolyte, further increases in colloidal concentration lead to a decrease in water content and increased electrolyte viscosity. Although the coulombic efficiency is higher at this concentration, the cycling performance significantly declines, with a rapid decrease in battery performance after only 170 cycles. Therefore, a suitable colloidal concentration helps improve battery stability while achieving higher battery coulombic efficiency.

[0085] Example 8

[0086] This embodiment analyzes the effect of different concentrations of ferrous sulfate on battery performance, as detailed below:

[0087] (1) Prepare a 20ml mixed solution of 1mol / L manganese sulfate and 1mol / L zinc sulfate, then add 7.5% hydrophilic nano silica and 0.01mol / L ferrous sulfate ions, and 0.1mol / L sulfuric acid. Stir for 10min to disperse it evenly to obtain a colloidal electrolyte.

[0088] (2) Prepare a 20 ml mixed solution of 1 mol / L manganese sulfate and 1 mol / L zinc sulfate, then add 7.5% hydrophilic nano silica and 0.02 mol / L ferrous sulfate ions, and 0.1 mol / L sulfuric acid. Stir for 10 min to disperse it evenly to obtain a colloidal electrolyte.

[0089] (3) Prepare a 20ml mixed solution of 1mol / L manganese sulfate and 1mol / L zinc sulfate, then add 7.5% hydrophilic nano silica and 0.04mol / L ferrous sulfate ions, and 0.1mol / L sulfuric acid. Stir for 0min to disperse it evenly and obtain a colloidal electrolyte.

[0090] In this embodiment, the three electrolytes are identical in composition and concentration except for the ferrous sulfate ion concentration. A static battery is assembled under the same conditions. A zinc sheet is used as the negative electrode, and a carbon felt is used as the positive electrode current collector. The positive and negative electrodes are fixed to both sides of the electrolytic cell with a 1cm gap via platinum electrodes. 20ml of electrolyte is added to the electrolytic cell, and a static battery is assembled. The obtained battery is then electrochemically tested using a Xinwei electrochemical testing system under the following cycling conditions:

[0091] Charging conditions: current density 15 mA / cm² 2 The charging capacity is 10mAh / cm². 2 Discharge conditions: current density 15 mA / cm² 2 The cutoff voltage is 0.8V.

[0092] The results are as follows Figure 9As shown, different concentrations of ferrous sulfate significantly affect the coulombic efficiency and cycle life of the battery. The electrolyte with 0.01 mol / L ferrous sulfate additive exhibited significant coulombic efficiency fluctuations after 250 cycles, indicating poor cycle stability at high capacity with a smaller redox medium additive. The electrolyte with 0.02 mol / L ferrous sulfate additive showed higher coulombic efficiency (95%) and cycle stability (600 cycles). The electrolyte with 0.04 mol / L ferrous sulfate additive failed after only 70 cycles, indicating that a large amount of redox medium resulted in poor cycle performance due to severe zinc anode corrosion. Therefore, a suitable redox medium concentration significantly improves battery cycle performance while achieving higher coulombic efficiency.

[0093] Example 9

[0094] This embodiment analyzes the impact of different types of colloidal electrolytes on battery performance, as detailed below:

[0095] (1) Prepare a 20ml mixed solution of 1mol / L manganese sulfate and 1mol / L zinc sulfate, then add 7.5% hydrophilic nano silica and 0.01mol / L ferrous sulfate ions, and 0.1mol / L sulfuric acid. Stir for 10min to disperse it evenly to obtain a colloidal electrolyte.

[0096] (2) Prepare a 20 ml mixed solution of 1 mol / L manganese sulfate and 1 mol / L zinc sulfate, then add 7.5% redox graphene and 0.02 mol / L ferrous sulfate ions, and 0.1 mol / L sulfuric acid. Stir for 10 min to disperse the solution evenly and obtain a colloidal electrolyte.

[0097] (3) Prepare a mixed solution of 1 mol / L manganese sulfate and 1 mol / L zinc sulfate in 20 ml, then add soluble starch with a final concentration of 7.5% by mass, 0.04 mol / L ferrous sulfate ions, and sulfuric acid with a final concentration of 0.1 mol / L, and stir for 10 min to make it evenly dispersed to obtain a colloidal electrolyte.

[0098] In this embodiment, the three electrolytes are identical in composition and concentration except for the type of colloidal electrolyte. A static battery is assembled under the same conditions. A zinc sheet is used as the negative electrode, and a carbon felt is used as the positive electrode current collector. The positive and negative electrodes are fixed to opposite sides of the electrolytic cell via platinum electrodes, with a 1cm gap. 20ml of electrolyte is added to the electrolytic cell, and a static battery is assembled. The obtained battery is then electrochemically tested using a Xinwei electrochemical testing system under the following cycling conditions:

[0099] Charging conditions: current density 15 mA / cm² 2The charging capacity is 10mAh / cm². 2 Discharge conditions: current density 15 mA / cm² 2 The cutoff voltage is 0.8V.

[0100] The results are as follows Figure 10 As shown, the use of 7.5% hydrophilic nano-silica exhibited the highest average coulombic efficiency (96%) and electrochemical cycling performance (stable for 600 cycles), which is attributed to the synergistic effect of negatively charged colloidal particles and ferrous sulfate significantly improving the cycling stability of manganese dioxide dissolution / deposition. The use of 7.5% negatively charged graphene redox colloidal electrolyte also showed high coulombic efficiency (94%), but the cycle life decreased significantly (450 cycles), indicating that graphene redox accelerates zinc sheet corrosion in acidic environments, leading to poor cycling performance. The use of 7.5% neutral soluble starch colloidal electrolyte exhibited the worst coulombic efficiency (92%) and moderate cycle life (550 cycles), indicating that neutral colloidal electrolytes have a poor effect in promoting manganese dioxide dissolution / deposition.

[0101] In summary, this invention utilizes carbon felt as the positive current collector and zinc sheet as the negative electrode. A 1 mol / L zinc sulfate and manganese sulfate solution and a 0.1 mol / L sulfuric acid solution are prepared, along with a 0.02 mol / L ferrous sulfate redox medium and 7.5 wt% hydrophilic nano-silica as electrolyte additives. The assembled Zn-MnO2 battery exhibits high areal capacity, coulombic efficiency, energy density, and cycle stability. Furthermore, the colloid effectively promotes the growth of Mn. 2+ / MnO2 deposition / dissolution.

[0102] The embodiments of the present invention have been described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions, and variations made to these embodiments without departing from the principles and spirit of the present invention still fall within the protection scope of the present invention.

Claims

1. A colloidal electrolyte for aqueous zinc-manganese batteries, characterized in that, The electrolyte comprises a solvent and an electrolyte, wherein the solvent is water, and the electrolyte contains zinc salt, manganese salt, additives, and an organic / inorganic acid that provides additional protons when MnO2 dissolves. The additives include a gelling agent and ferrous sulfate, wherein the mass of the gelling agent accounts for 5-12.5% ​​of the mass of the electrolyte, and the molar concentration of ferrous sulfate is 0.02 mol / L; the concentration of zinc salt in the electrolyte is 1-2 mol / L, the concentration of manganese salt is 1-2 mol / L, and the molar concentration of organic / inorganic acid is 0.1 mol / L-0.2 mol / L. The ferrous sulfate undergoes a redox reaction with manganese dioxide, which promotes the dissolution of the manganese dioxide cathode during the discharge process. The gelling agent acts as a nucleating agent, and the negative charge on its surface participates in the construction of the positive electrode double layer, which promotes the deposition of manganese dioxide and provides reaction sites for the reaction between ferrous ions and manganese dioxide.

2. The gel electrolyte for aqueous zinc-manganese batteries according to claim 1, characterized by The gelling agent is a composite of any one or more of the following: hydrophilic nano-silica, reduced graphene oxide, graphene oxide, starch, and montmorillonite.

3. The gel electrolyte for aqueous zinc-manganese batteries according to claim 2, characterized by The gelling agent is hydrophilic nano-silica.

4. The gel electrolyte for aqueous zinc-manganese batteries according to claim 3, characterized by The hydrophilic nano-silica accounts for 7.5% of the mass of the electrolyte.

5. The gel electrolyte for aqueous zinc-manganese batteries according to claim 1, characterized in that, The zinc salt is zinc sulfate, and the manganese salt is manganese sulfate.

6. The gel electrolyte for aqueous zinc-manganese batteries according to claim 1, characterized in that, The organic acid is one of acetic acid, formic acid, citric acid or methanesulfonic acid, and the inorganic acid is sulfuric acid or hydrochloric acid.

7. A method for preparing the colloidal electrolyte for aqueous zinc-manganese batteries as described in claim 1, characterized in that, Includes the following steps: Step S1: Prepare zinc sulfate solution and manganese sulfate solution, and mix the zinc sulfate solution and manganese sulfate solution thoroughly; Step S2: Weigh an appropriate amount of ferrous sulfate, gelling agent, and organic / inorganic acid, add them to the mixed solution from step S1, and shake until completely dissolved to obtain the aqueous zinc-manganese battery colloidal electrolyte.

8. An electrolytic aqueous zinc-manganese battery, characterized in that, It includes a positive electrode, a negative electrode, and an electrolyte, wherein the electrolyte is a colloidal electrolyte for aqueous zinc-manganese batteries as described in any one of claims 1-6.

Citation Information

Patent Citations

  • Colloidal electrolyte and zinc ion battery containing same

    CN111883857A