A method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range
By preparing Ni-Mn-MN alloy micron particles through atomization and then subjecting them to low-temperature heat treatment, the problems of narrow cooling temperature range and difficult heat conduction of Ni-Mn-X alloy bulk materials were solved, achieving a more efficient magnetic refrigeration effect, broadening the cooling temperature range, and improving the magnetocaloric performance.
Patent Information
- Application Number
- CN202410421394.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-09
AI Technical Summary
Existing Ni-Mn-X (X=Sn, In, Sb) alloy bulk materials suffer from problems such as a narrow cooling temperature range, the need to improve magnetocaloric properties, and difficulties in heat conduction and heat exchange during application.
Ni-Mn-MN (M=Sn, In, Sb; N=Co, Fe) alloy micron particles were prepared by atomization. Non-equilibrium rapid solidification and low-temperature heat treatment were used to increase the density of defects such as vacancies inside the alloy, thereby improving the driving force for heat treatment to regulate the phase transformation and magnetic properties of the alloy, thus broadening the working temperature range of magnetic refrigeration and improving heat transfer efficiency.
By preparing Ni-Mn-MN alloy micron particles and performing low-temperature heat treatment, the ferromagnetic austenitic temperature range of the alloy is significantly broadened, the magnetic entropy change and magnetocaloric effect are improved, and the refrigeration capacity is enhanced, making it suitable for household and industrial refrigeration.
Smart Images

Figure CN118287679B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of refrigerants, specifically relating to a method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range. Background Technology
[0002] With the increasing demand for green and efficient refrigeration technologies, solid-state refrigeration technology has developed rapidly in recent years. Compared with traditional vapor compression refrigeration technology, solid-state refrigeration is environmentally friendly and has high energy conversion efficiency (4 to 6 times that of traditional refrigeration technologies), meeting the urgent requirements of environmental protection and showing broad application prospects. Solid-state refrigeration mainly utilizes the magnetocaloric effect, electrothermal effect, elastothermal effect, and compressive-thermal effect of materials. Among them, magnetic refrigeration technology based on the magnetocaloric effect relies on the change of spin electron magnetic entropy under an applied magnetic field and is relatively mature in the refrigeration field. Traditional magnetic refrigeration materials, including Gd, Gd-Si-Ge, La-Fe-Si, and Mn-Fe-(P, As), exhibit good performance, but have disadvantages such as high rare earth costs or the presence of toxic P / As elements, hindering their practical application. In contrast, safe, reliable, and cost-effective Ni-Mn-X (X = Sn, In, Sb) alloys can exhibit a giant reverse magnetocaloric effect at room temperature and are expected to be widely used in household and industrial refrigeration fields.
[0003] Excellent magnetic refrigerants should possess a large magnetic entropy change, a wide operating temperature range, and excellent heat dissipation performance. Although Ni-Mn-X (X = Sn, In, Sb) alloys have great application potential, the following problems still exist: 1) Heat conduction and heat exchange during the refrigeration process: During the refrigeration cycle, the refrigerant material needs to conduct heat itself and exchange heat with the cooling liquid. Traditional bulk refrigerants have a small specific surface area and poor heat transfer efficiency; 2) Narrow refrigeration temperature range: Although the refrigeration temperature range can be adjusted by adding a fourth component, allowing the refrigerant to operate at the target temperature, how to broaden the refrigeration temperature range still needs further investigation.
[0004] In the patent “A Ni-Co-Mn-Sn magnetic refrigeration material and its preparation method” (CN 108330372 B), the prepared alloy strip has a magnetic entropy change of only ~3J / (kg·K) under a 5T magnetic field, and the magnetocaloric effect is poor, which cannot meet the application requirements.
[0005] In the patent "A Mn-Ni-Sn-Co alloy strip and its preparation method" (CN 106119661 B), the prepared alloy strip has a cooling working range of only ~3.5K under a 1T magnetic field, which is too narrow to meet the application requirements.
[0006] The literature "Influence of Heat Treatment on Phase Transition and Magnetic Properties of Ni-Co-Mn-Sn Strips" describes the preparation of Ni-Co-Mn-Sn strips with a nominal composition of Ni using a vacuum melt rapid quenching method.38 Co 12 Mn 41 The magnetic shape memory alloy ribbon of Sn9 was subsequently subjected to heat treatment at 700-900℃ for 0.5h, 5h, and 10h. The results showed that, except for a slight increase in magnetic entropy change after 700℃ / 0.5h heat treatment compared to the prepared state, the other treatments all reduced the magnetic properties of the alloy. This method for high-temperature heat treatment of Ni-Co-Mn-Sn ribbons did not broaden the cooling range of the alloy or improve its cooling capacity.
[0007] The literature "Preparation and Heat Treatment Study of Ni-Mn-In-(Cu) Alloy Strips" describes the preparation of Ni-Mn-In-(Cu) alloy strips using a vacuum single-roller rapid cooling and spinning method, followed by heat treatment at 873-1173 K for 1 hour. The results show that the phase transformation temperature of the alloy increases after heat treatment. However, this method for high-temperature heat treatment of Ni-Mn-In-(Cu) alloy strips did not investigate changes in the alloy's magnetocaloric properties.
[0008] The literature "Study on Phase Transformation Regulation and Magnetothermal Effect of Ni-Mn-Sn-Fe(Co) Alloy" and the paper "Study on Aging Behavior and Magnetothermal Properties of Ni-Mn-Sn-X (X=Fe,Co) Alloy" utilizes an induction melting furnace casting machine to prepare alloy ingots, followed by heat treatment. The Ni-Mn-Sn-X (X=Fe,Co) alloys used in this method are all bulk materials. During the preparation process, slow cooling results in fewer internal defects such as vacancies, leading to a lower driving force for the ordered transformation during subsequent heat treatment, thus significantly reducing the effectiveness of the heat treatment. For example, in the study on aging behavior and magnetothermal properties of Ni-Mn-Sn-X (X=Fe,Co) alloy, after heat treatment at 573K for 20 hours, the martensitic phase transformation temperature of the Ni-Mn-Sn-Co bulk alloy only decreased by 5.27K. This method suffers from poor heat transfer efficiency in bulk materials during application, which is detrimental to practical refrigeration applications.
[0009] The literature "Preparation and Study of Elastic-Thermoelectric Effect of Directional Solidification Ni-Mn-Sn Magnetorized Shape Memory Alloys" uses directional solidification to prepare Ni-Mn-Sn series alloys. The ferromagnetic austenite temperature range is only ~16K, which cannot meet the application requirements.
[0010] Although the aforementioned literature provides improved technical solutions for magnetic refrigerants, it still does not effectively solve the technical problems mentioned above. Summary of the Invention
[0011] The purpose of this invention is to address the common problems in bulk Ni-Mn-MN (M = Sn, In, Sb; N = Co, Fe) alloys, such as narrow cooling temperature range, insufficient magnetocaloric properties, and difficulties in heat conduction and exchange during application. This invention uses an atomization method to prepare Ni-Mn-MN (M = Sn, In, Sb; N = Co, Fe) alloy micron particles. Non-equilibrium rapid solidification results in a higher density of defects such as vacancies inside the alloy, and a higher driving force for processes such as ordered transformation during subsequent low-temperature heat treatment. This greatly enhances the heat treatment effect. Low-temperature heat treatment can significantly broaden the ferromagnetic austenite temperature range of the alloy, thereby improving the alloy's magnetic properties and magnetic entropy change, and widening the magnetic refrigeration operating temperature range. Furthermore, micron particles have better heat transfer efficiency compared to bulk working fluids.
[0012] The present invention provides a method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range, the preparation method being as follows:
[0013] Step 1: Preparation of Alloy Ingots
[0014] According to the general chemical formula Ni 50-y Mn 50-x M x N y The composition is determined by weighing high-purity metals and performing vacuum melting; where x and y are atomic percentages, x = 10⁻¹², y = 0⁻⁶; M is Sn, In, or Sb; N is Co or Fe;
[0015] Step 2: Homogenization heat treatment of alloy ingots
[0016] After the alloy ingot is vacuum-melted, the surface is polished and cleaned, then placed in a quartz tube. The quartz tube is then evacuated and sealed, and then treated at a temperature of 1173-1223K for 24-36 hours.
[0017] Step 3: Preparation of atomized alloy micron-sized particles
[0018] After the alloy ingots were uniformly treated in step two, they were polished, cleaned, and then subjected to vacuum gas atomization treatment to obtain alloy micron particles.
[0019] Step 4: Low-temperature heat treatment of alloy micron-sized particles
[0020] The alloy micron particles obtained in step three are placed in a quartz tube, then high-temperature resistant asbestos is added and sealed, and then placed in another quartz tube. The quartz tube is evacuated and sealed, and then treated at a temperature of 373-773K for 20-168 hours. After that, it is taken out of the furnace and air-cooled to obtain the magnetic refrigerant with a wide ferromagnetic austenitic temperature range.
[0021] Furthermore, the vacuum melting temperature described in step one is 1273-1373K, and the vacuum degree is 5-6×10⁻⁶. -3 Pa.
[0022] The vacuum melting of the present invention can be carried out in a KZG-1 vacuum induction melting furnace.
[0023] This invention prepares ingots by melting under vacuum. To improve compositional uniformity, the ingots are remelted 3-4 times as raw materials after each melting, meaning each ingot is melted a total of 4-5 times.
[0024] Furthermore, in the process of weighing high-purity metal in step one, 1.5-3.0 wt.% of Mn is added to the nominal Mn element composition, and then vacuum melting is carried out.
[0025] To compensate for the loss of Mn element during the powdering process, this invention adds 1.5-3.0 wt.% Mn to the nominal Mn element composition, and the total mass of the ingot can optionally be between 200g and 1000g.
[0026] Furthermore, in steps two and four, the quartz tubes must be acid-washed and soaked in HF with a volume percentage of 5% before use, then cleaned to remove acidic substances, dried, and ready for use.
[0027] This invention utilizes HF (47% HF by volume) and deionized water to prepare a 5% HF solution. Before use, the quartz tube needs to be acid-washed and soaked in the 5% HF solution to remove organic contaminants and impurities such as metal ions. After the quartz tube is completely immersed in the 5% HF solution for two hours, it is rinsed with deionized water for 2-3 minutes to fully remove acidic substances, and then dried in a forced-air drying oven at 60-80℃ for 24-36 hours.
[0028] Furthermore, the specific procedures for evacuating the quartz tube in steps two and four are as follows: First, the vacuum level inside the quartz tube is brought to 1-1.2 Pa. Then, 5N high-purity argon gas is introduced for purging, repeated 3-4 times, until the vacuum level inside the tube drops to 0.6-0.8 Pa. Finally, liquid nitrogen is poured in and evacuation continues until the vacuum level reaches 1-1.5 × 10⁻⁶ Pa. -5 Pa.
[0029] Because the homogenization heat treatment temperature is relatively high, the alloy needs to be sealed in a quartz tube under vacuum to prevent oxidation and element loss. The quartz tube in step two is a semi-sealed type, with one end sealed and the other end open. Its outer diameter is 25-42mm, the wall thickness is 1-2mm, and the length is 200-300mm, which can be selected according to the size of the ingot.
[0030] The sealing process of this invention involves disconnecting the quartz tube from the vacuum pump, turning on the hydrogen-oxygen generator while maintaining a vacuum, heating the quartz plug with a flame gun, and simultaneously rotating the quartz tube to ensure uniform heating of the quartz tube and the quartz plug until they melt and fuse together, thus obtaining a quartz tube with high vacuum conditions.
[0031] Furthermore, Ti wires and Mn sheets are placed inside both the quartz tube in step two and the quartz tube taken separately in step four.
[0032] In order to reduce oxidation and loss of Mn element with low saturated vapor pressure, the present invention places Ti wire and Mn sheet simultaneously inside a quartz tube.
[0033] Furthermore, the specific processes for polishing and cleaning in steps two and three are as follows:
[0034] Polish with 400# sandpaper, then completely immerse in acetone solution and ultrasonically clean in an ultrasonic cleaner with an ultrasonic vibration frequency of 20kHz-40kHz for 20-30 minutes. After removal, rinse the surface of the ingot with anhydrous ethanol for 1-2 minutes to fully remove acetone, and then place it on filter paper to air dry naturally for 0.5-1 hour.
[0035] Furthermore, the specific process of vacuum gas atomization treatment described in step three is as follows:
[0036] First, the ingot is melted and cast under vacuum conditions, with a vacuum degree of 8-9 × 10⁻⁶. -3 Pa, the temperature is set at 1273-1373K; after the ingot has melted, the molten metal is atomized into droplets by a high-pressure gas flow through a nozzle, thus completing the vacuum gas atomization treatment; wherein, the gas pressure of the high-pressure gas flow is 4-5MPa, and the gas of the high-pressure gas flow is 5N argon.
[0037] The vacuum gas atomization process of this invention can be performed using the VIGA-25 vacuum gas atomization powder maker.
[0038] Furthermore, in step two, the quartz tube containing the alloy ingot has an outer diameter of 25-42 mm, a wall thickness of 1-2 mm, and a length of 200-300 mm; in step four, the quartz tube containing the alloy micron particles has an outer diameter of 18-23 mm, a wall thickness of 1-2 mm, and a length of 120-180 mm; and in step four, another quartz tube has an outer diameter of 25-30 mm, a wall thickness of 1-2 mm, and a length of 250-300 mm.
[0039] Furthermore, before processing at a temperature of 373-773K as described in step four, the temperature is raised to 373-773K and maintained for 10-20 minutes.
[0040] Compared to the patent "A Ni-Co-Mn-Sn magnetic refrigeration material and its preparation method" (CN 108330372 B), the present invention, after heat treatment at 473K for 7 days, achieves a magnetic entropy change of 23.40 J / (kg·K) in the Ni-Mn-Sn-Co alloy under a 5T magnetic field, which greatly enhances the magnetocaloric effect of the alloy.
[0041] Compared to the patent "A Mn-Ni-Sn-Co alloy thin strip and its preparation method" (CN 106119661 B), the present invention, after heat treatment at 473K for 7 days, allows the Ni-Mn-Sn-Co alloy to reach a cooling operating temperature range of 12.6K under a 1T magnetic field, which greatly enhances the magnetocaloric effect of the alloy.
[0042] Compared to the literature "Preparation and Elastothermic Effect Study of Directional Solidification Ni-Mn-Sn Magnetorized Shape Memory Alloy", this invention achieves a ferromagnetic austenitic temperature range of 69.91K for Ni-Mn-Sn alloy and 134.26K for Ni-Mn-Sn-Co alloy after heat treatment at 473K for 7 days, greatly enhancing the magnetothermic effect of the alloy.
[0043] Compared to the literature "Study on Phase Transformation Regulation and Magnetothermal Effect of Ni-Mn-Sn-Fe(Co) Alloy" and the paper "Study on Aging Behavior and Magnetothermal Properties of Ni-Mn-Sn-X (X=Fe,Co) Alloy", the present invention reduces the martensitic phase transformation temperature of the alloy by 8.76K after heat treatment at 573K / 20 hours. Due to the rapid cooling during the powder sample preparation process, the powder has a large density of defects such as vacancies, which greatly enhances the effect of low-temperature heat treatment and effectively expands the ferromagnetic austenite range of the alloy.
[0044] The present invention has the following beneficial effects:
[0045] This invention aims to solve the aforementioned problems by preparing Ni-Mn-MN (M = Sn, In, Sb; N = Co, Fe) alloy micron particles and subjecting them to subsequent low-temperature heat treatment. Regarding problem 1) in the background art, compared to bulk alloys, the alloy exists in the form of micron particles, possessing a larger specific surface area. The increased contact area with the heat transfer medium allows for more efficient heat dissipation, thereby improving refrigeration efficiency. Regarding problem 2), the preparation of alloy micron particles through rapid non-equilibrium solidification results in a larger density of defects such as vacancies within the alloy. This increases the driving force for heat treatment to regulate the alloy's phase transformation and magnetic properties, making it more conducive to improving alloy performance through lower-temperature heat treatment. This expands the alloy's refrigeration operating range, increases magnetic entropy change, and thus enhances the alloy's magnetocaloric effect, making it more promising as a magnetic refrigerant for household and industrial refrigeration applications. Attached Figure Description
[0046] Figure 1 The image shows the secondary electron microstructure of micron-sized Ni-Mn-Sn-Co atomized alloy particles.
[0047] Figure 2 The images show the room temperature XRD patterns of Ni-Mn-Sn-Co alloy micron particles before and after heat treatment at 473K for 7 days.
[0048] Figure 3 DSC images of micron-sized particles in Ni-Mn-Sn-Co alloy before and after heat treatment at 473K / 7 days;
[0049] Figure 4 MT image of untreated Ni-Mn-Sn-Co alloy micron-sized particles;
[0050] Figure 5 MT image of micron-sized particles in Ni-Mn-Sn-Co alloy after heat treatment at 473K for 7 days;
[0051] Figure 6 MH diagram of micron-sized particles in untreated Ni-Mn-Sn-Co alloy;
[0052] Figure 7 MH diagram of micron-sized particles in Ni-Mn-Sn-Co alloy heat-treated at 473K / 7 days;
[0053] Figure 8 For untreated Ni-Mn-Sn-Co alloy micron particles ΔS M -T diagram;
[0054] Figure 9 The ΔS of Ni-Mn-Sn-Co alloy micron-sized particles after heat treatment at 473K for 7 days M -T diagram;
[0055] Figure 10 DSC images of micron-sized particles in Ni-Mn-Sn-Co alloy before and after heat treatment at 373K / 7 days;
[0056] Figure 11 DSC images of micron-sized particles in Ni-Mn-Sn-Co alloy before and after heat treatment at 573K for 20 hours;
[0057] Figure 12 DSC images of micron-sized particles in Ni-Mn-Sn alloy before and after heat treatment at 473K / 7 days;
[0058] Figure 13 This is a diagram illustrating the sealing process. Detailed Implementation
[0059] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the spirit of the contents disclosed in the present invention will be described in detail below. After understanding the embodiments of the present invention, any person skilled in the art can make changes and modifications based on the technology taught in the present invention without departing from the spirit and scope of the present invention.
[0060] The illustrative embodiments and descriptions of the present invention are used to explain the present invention, but are not intended to limit the present invention.
[0061] Example 1
[0062] The invention's effects are illustrated using Ni-Mn-Sn-Co alloy micron-sized particles as an example.
[0063] The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range in this embodiment is as follows:
[0064] (1) Alloy ingot preparation: according to Ni 42 Mn 42 Sn 10 The composition of Co6 was determined by weighing out 99.995% high-purity Ni particles, 99.95% high-purity Mn flakes, 99.99+% Sn flakes, and 99.95% high-purity Co particles. To compensate for the loss of Mn during the powdering process, 2 wt.% Mn was added to this nominal Mn composition. The total mass of the ingot was 500g. Induction melting was used, employing a KZG-1 vacuum induction melting furnace, with the temperature set at 1373K and the vacuum degree at 6×10⁻⁶. -3 Pa. Ingots are prepared by melting under vacuum. To improve compositional uniformity, the ingots are remelted four times as raw materials after each melting, meaning each ingot is melted a total of five times.
[0065] (2) Homogenization heat treatment of alloy ingots: Homogenization heat treatment helps reduce segregation and makes the alloy composition more uniform. The surface of the obtained alloy ingot was polished with 400# sandpaper, and then completely immersed in acetone solution. It was then ultrasonically cleaned in an ultrasonic cleaner to remove impurities such as debris and sand particles from the surface of the ingot. The ultrasonic vibration frequency was 40kHz and the cleaning time was 30 minutes. After ultrasonic cleaning, the surface of the ingot was rinsed with anhydrous ethanol for 2 minutes to fully remove acetone, and then placed on filter paper to air dry naturally for 1 hour. Due to the high temperature of homogenization heat treatment, in order to prevent alloy oxidation and element loss, the alloy needs to be sealed in a quartz tube under vacuum. The quartz tube is semi-sealed, with one end sealed and the other end open. The outer diameter is 42mm, the wall thickness is 2mm, and the length is 250mm. A 5% HF solution was prepared using 47% HF and deionized water. The quartz tube needs to be acid-washed and soaked in 5% HF before use to remove organic contaminants and metal ions. The quartz tube was completely immersed in 5% HF for two hours, then rinsed with deionized water for 2-3 minutes to thoroughly remove acidic substances, and then dried in an 80℃ forced-air drying oven for 24 hours. To reduce oxidation and loss of Mn element with low saturated vapor pressure, Ti wires and Mn sheets were placed inside the quartz tube simultaneously. The open end of the quartz tube was connected to a vacuum pump to first achieve a vacuum of 1 Pa. Then, 5N high-purity argon gas was introduced for purging, repeated 3-4 times until the vacuum decreased to 0.6 Pa. Finally, liquid nitrogen was poured in and evacuated until the vacuum reached 1×10⁻⁶ Pa. -5 Disconnect the quartz tube from the vacuum pump. While maintaining a vacuum, turn on the oxyhydrogen generator and heat the quartz stopper using a flame torch. Simultaneously rotate the quartz tube to ensure uniform heating of both the tube and the stopper until they melt and fuse, resulting in a quartz tube with high vacuum conditions. Heat the high-temperature heat treatment box furnace to 1173K and stabilize it for 10 minutes after reaching this temperature. Place the quartz tube containing the alloy ingot into the heat treatment box furnace. Once the furnace temperature reaches the set temperature, start timing and hold for 24 hours. Then remove and air-cool.
[0066] (3) Preparation of atomized alloy micronized particles. The homogenized alloy ingot surface was polished with 400# sandpaper, then completely immersed in acetone solution and ultrasonically cleaned in an ultrasonic cleaner to remove debris, sand particles, and other impurities from the ingot surface. The ultrasonic vibration frequency was 40kHz, and the cleaning time was 30 minutes. After removal, the ingot surface was rinsed with anhydrous ethanol for 1-2 minutes, then placed on filter paper and air-dried naturally for 0.5-1 hour. The cleaned ingot was then placed in a VIGA-25 vacuum gas atomizing powder generator, with an ingot mass of 500g. First, the ingot was melted under vacuum conditions, with a vacuum degree of 8×10⁻⁶. -3The pressure is set at 1373 K. After the ingot has melted completely, the molten metal flows out through the insulated crucible and the guide nozzle. Through the nozzle, a high-pressure gas stream (5N argon) atomizes and breaks the molten metal into numerous tiny droplets, which solidify into micron-sized particles during flight. The gas pressure is 4 MPa.
[0067] (4) Low-temperature heat treatment of alloy micron particles. In order to further broaden the cooling working range of the alloy and improve its magnetic cooling capacity, the alloy micron particles were heat-treated. To prevent the micron particles from being lifted or lost during the sealing process, the specific operation for sealing the alloy micron particles was as follows: Take 60g of alloy micron particles, take a No. 1 semi-sealed quartz tube with an outer diameter of 25mm, a wall thickness of 2mm, and a length of 250mm, and a No. 2 semi-sealed quartz tube with an outer diameter of 18mm, a wall thickness of 2mm, and a length of 120mm. The pretreatment of the quartz tubes was the same as in step (2). To avoid the alloy micron particles being drawn into the vacuum pump, the sealing was done in the form of a sleeve. That is, the sample was placed in the No. 2 quartz tube, the open end was sealed with high-temperature resistant asbestos, and then the No. 2 tube was placed in the No. 1 tube for vacuuming. Repeat the sealing operation in step (2) to obtain a quartz tube with high vacuum conditions. The medium-temperature heat treatment box furnace was heated to 473K and stabilized for 10 minutes after reaching the temperature. A quartz tube containing alloy micron-sized particles is placed inside a furnace. Once the furnace temperature reaches the set temperature, timing begins, and the tube is held at that temperature for 168 hours. Afterward, it is removed and air-cooled. The specific temperature and time can be selected according to the expected performance targets.
[0068] like Figure 1 The image shown is a secondary electron microstructure of the Ni-Mn-Sn-Co atomized alloy micron particles in this embodiment.
[0069] The selected low-temperature heat treatment temperature is 473K, and the treatment time is 7 days. Figure 2 The XRD patterns of Ni-Mn-Sn-Co alloy micron particles before and after heat treatment at 473K for 7 days show that both types of micron particles exhibit a coexistence of L21 austenite and 5M martensite at room temperature. The intensity ratio of diffraction peaks (111) and (220), i.e., I(111) / I(220), can characterize the degree of ordering of the austenite phase. After heat treatment at 473K for 7 days, the value of I(111) / I(220) increased from 0.0307 to 0.0563, indicating that the degree of ordering of the alloy micron particles was significantly improved. Figure 3 The differential scanning calorimetry (DSC) images of the Ni-Mn-Sn-Co alloy micron-sized particles before and after heat treatment at 473 K / 7 days are shown in Table 1. Specific phase transformation parameters are also shown. It can be seen that the martensitic phase transformation temperature M of the alloy after heat treatment is... s The temperature decreases by approximately 17 K, while the ferromagnetic-paramagnetic transition temperature T of austenite decreases by approximately 17 K. cThe temperature was increased by approximately 8K. This demonstrates that heat treatment significantly broadens the ferromagnetic austenitic temperature range of the alloy, helping it to exhibit its optimal magnetic properties.
[0070] Table 1. DSC phase transformation parameters of Ni-Mn-Sn-Co alloy micron particles before and after 473K / 7-day heat treatment
[0071] sample <![CDATA[M f DSC (K)]]> <![CDATA[M s DSC (K)]]> <![CDATA[A s DSC (K)]]> <![CDATA[A f DSC (K)]]> <![CDATA[ΔT hys (K)]]> <![CDATA[T C DSC (K)]]> Untreated 264.69 295.29 296.62 313.15 24.90 404.80 473K / 7 days 247.29 278.24 282.55 301.37 29.20 412.50
[0072] The phase transformation characteristics of Ni-Mn-Sn-Co alloy micron particles under magnetic field before and after heat treatment at 473K / 7 days were measured using a vibrating magnetometer (VSM). The magnetization-temperature (MT) curves under different magnetic fields are shown below. Figure 4 and Figure 5 As shown in Table 2, the phase transformation parameters are similar to those obtained by DSC. After heat treatment, the phase transformation temperature of the alloy microparticles at 50 Oe decreased by approximately 16 K. The increase in ΔM after heat treatment (an increase of approximately 14%) also indicates a significant improvement in the magnetic properties of the alloy microparticles compared to before heat treatment. ΔT B The increase in / ΔH indicates that the alloy microparticles can undergo magnetoinduced reverse martensitic phase transformation and drive a large magnetocaloric effect under a lower magnetic field, which means that Ni-Mn-Sn-Co alloy microparticles are more likely to be widely used in the field of refrigeration.
[0073] Table 2. VSM phase transformation parameters of Ni-Mn-Sn-Co alloy micron particles before and after 473K / 7-day heat treatment
[0074]
[0075]
[0076] To further characterize the magnetocaloric properties of the alloy, the magnetization-magnetic field (MH) curve of the alloy was measured, such as... Figure 6 and Figure 7 As shown, a complete magnetostrictive inverse martensite transformation occurs at 298 K before low-temperature heat treatment, while the temperature decreases to 284 K after treatment. Furthermore, the austenite saturation magnetization is significantly improved after low-temperature heat treatment, indicating that the magnetic properties of the alloy are well optimized. In addition, the curve after low-temperature heat treatment shows a steeper slope, meaning that martensite can be magnetized under a smaller magnetic field. This phenomenon is consistent with the above description.
[0077] The magnetic entropy change (ΔS) of the alloy before and after low-temperature heat treatment was calculated using discrete Maxwell equations based on the MH curve. M )like Figure 8 and Figure 9 As shown. The maximum magnetic entropy change of the alloy (ΔS) M max ), refrigeration operating temperature range (ΔT)FWHM ), cooling capacity (RC), average hysteresis (AHL), and net cooling capacity (RC) net As shown in Table 3. It can be seen from the table that ΔS after heat treatment... M max The magnetic entropy change increased from 22.57 J / (kg·K) to 23.40 J / (kg·K), while the operating range expanded from 16.71 K to 20.00 K, a widening of nearly 20%. Due to the increase in magnetic entropy change and the expansion of the cooling range, the net cooling capacity of the alloy increased from 165.70 J / kg to 199.23 J / kg, representing a 20.24% improvement in cooling capacity.
[0078] Table 3. Magnetic refrigeration properties of Ni-Mn-Sn-Co alloy micron-sized particles before and after 473K / 7-day heat treatment
[0079]
[0080] In summary, due to the large density of vacancies and other defects in the gas-atomized Ni-Mn-Sn-Co particles, the driving force for the ordered transformation during subsequent low-temperature heat treatment is enhanced, which greatly expands the cooling operating range of the alloy and significantly improves its cooling capacity. Under a 5T magnetic field, the cooling operating range reaches 20.00K and the net cooling capacity reaches 199.23J / kg, which is expected to promote the development of magnetic refrigeration in the fields of home and industry.
[0081] Example 2
[0082] The difference between this embodiment and Embodiment 1 is that the low-temperature heat treatment temperature is 373K and the treatment time is 7 days. Everything else is the same as in Embodiment 1.
[0083] Figure 10 The table shows the differential scanning calorimetry (DSC) images of the Ni-Mn-Sn-Co alloy micron-sized particles before and after the 373K / 7-day heat treatment in this embodiment. Specific phase transformation parameters are shown in Table 4. It can be seen that the martensitic phase transformation temperature M of the alloy after heat treatment... s The temperature decreases by approximately 12K, while the ferromagnetic-paramagnetic transition temperature T of austenite decreases by approximately 12K. c The temperature increased by approximately 4K. This demonstrates that heat treatment broadens the ferromagnetic austenitic temperature range of the alloy, contributing to its optimal magnetic properties. However, because the low-temperature heat treatment temperature is below 473K, the driving force for heat treatment is lower compared to 473K, resulting in a lower performance gain from low-temperature aging compared to 473K.
[0084] Table 4. DSC phase transformation parameters of Ni-Mn-Sn-Co alloy micron particles before and after 373K / 7-day heat treatment
[0085]
[0086]
[0087] Example 3
[0088] The difference between this embodiment and Embodiment 1 is that the low-temperature heat treatment temperature is selected as 573K, and the time is 20 hours. Everything else is the same as in Embodiment 1.
[0089] Figure 11 The differential scanning calorimetry (DSC) images of the Ni-Mn-Sn-Co alloy micron-sized particles before and after the 573K / 20-hour heat treatment are shown in Table 5. Specific phase transformation parameters are also shown. It can be seen that the martensitic phase transformation temperature M0 of the alloy after heat treatment is... s The temperature decreases by approximately 9K, while the ferromagnetic-paramagnetic transition temperature T of austenite decreases by approximately 9K. c The temperature was increased by approximately 3K. This demonstrates that heat treatment broadens the ferromagnetic austenitic temperature range of the alloy, which helps the alloy exhibit its optimal magnetic properties.
[0090] Table 5. DSC phase transformation parameters of Ni-Mn-Sn-Co alloy micron particles before and after heat treatment at 573K / 20 hours.
[0091] sample <![CDATA[M f DSC (K)]]> <![CDATA[M s DSC (K)]]> <![CDATA[A s DSC (K)]]> <![CDATA[A f DSC (K)]]> <![CDATA[ΔT hys (K)]]> <![CDATA[T C DSC (K)]]> Untreated 264.69 295.29 296.62 313.15 24.90 404.80 573K / 20 hours 256.86 286.53 289.59 304.00 25.10 408.01
[0092] Example 4
[0093] The difference between this embodiment and Embodiment 1 is that the alloy composition is Ni. 48 Mn 42 Sn 10 Everything else is the same as in Example 1.
[0094] Figure 12 The differential scanning calorimetry (DSC) images of the Ni-Mn-Sn alloy micron-sized particles before and after the 473K / 7-day heat treatment are shown in Table 6. Specific phase transformation parameters are also shown. It can be seen that the martensitic phase transformation temperature M0 of the alloy after heat treatment is... s The temperature decreases by approximately 13 K, while the ferromagnetic-paramagnetic transition temperature T of austenite decreases by approximately 13 K. c It has increased by ~6K.
[0095] Table 6. DSC phase transformation parameters of Ni-Mn-Sn alloy micron particles before and after 473K / 7-day heat treatment
[0096] sample <![CDATA[M f DSC (K)]]> <![CDATA[M s DSC (K)]]> <![CDATA[A s DSC (K)]]> <![CDATA[A f DSC (K)]]> <![CDATA[ΔT hys (K)]]> <![CDATA[T C DSC (K) <!-- 7 -->]]> Untreated 283.28 302.48 311.57 325.21 25.51 353.60 473K / 7 days 268.69 289.36 300.1 313.72 27.89 359.27
[0097] It is evident that heat treatment broadens the ferromagnetic austenitic temperature range of the alloy, which helps the alloy to exhibit its best magnetic properties.
Claims
1. A method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range, characterized in that... The preparation method is as follows: Step 1: Preparation of Alloy Ingots According to the chemical general formula Ni 50-y Mn 50-x M x N y The components of the chemical general formula are high-purity metals, which are vacuum melted; wherein, x, y are atomic percentage, x = 10-12, y = 0-6; M is Sn, In or Sb; N is Co or Fe. Step 2: Homogenization heat treatment of alloy ingots After the alloy ingot is vacuum-melted, the surface is polished and cleaned, then placed in a quartz tube. The quartz tube is then evacuated and sealed, and then treated at a temperature of 1173-1223K for 24-36 hours. Step 3: Preparation of atomized alloy micron-sized particles After the alloy ingots were uniformly treated in step two, they were polished, cleaned, and then subjected to vacuum gas atomization treatment to obtain alloy micron particles. Step 4: Low-temperature heat treatment of alloy micron-sized particles The alloy micron particles obtained in step three are placed in a quartz tube, then high-temperature resistant asbestos is added and sealed, and then placed in another quartz tube. The quartz tube is evacuated and sealed, and then treated at a temperature of 373-773K for 20-168 hours. After that, it is taken out of the furnace and air-cooled to obtain the magnetic refrigerant with a wide ferromagnetic austenitic temperature range.
2. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... The vacuum melting temperature described in step one is 1273-1373K, and the vacuum degree is 5-6×10⁻⁶. -3 Pa.
3. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... In step one, during the weighing of high-purity metal, 1.5-3.0 wt.% of Mn is added to the nominal Mn content, and then vacuum melting is carried out.
4. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... In steps two and four, the quartz tubes must be acid-washed and soaked in HF with a volume percentage of 5% before use, then cleaned to remove acidic substances, dried, and ready for use.
5. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... The specific procedures for evacuating the quartz tube in steps two and four are as follows: First, the vacuum level inside the quartz tube is brought to 1-1.2 Pa. Then, 5N high-purity argon gas is introduced for purging, repeated 3-4 times, until the vacuum level inside the tube drops to 0.6-0.8 Pa. Finally, liquid nitrogen is poured in and evacuation continues until the vacuum level reaches 1-1.5 × 10⁻⁶ Pa. -5 Pa.
6. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... Ti wires and Mn sheets were placed inside both the quartz tube in step two and the quartz tube taken separately in step four.
7. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... The specific processes for polishing and cleaning in steps two and three are as follows: Polish with 400# sandpaper, then completely immerse in acetone solution and ultrasonically clean in an ultrasonic cleaner with an ultrasonic vibration frequency of 20kHz-40kHz for 20-30 minutes. After removal, rinse the surface of the ingot with anhydrous ethanol for 1-2 minutes, then place it on filter paper to air dry naturally for 0.5-1 hour.
8. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... The specific process of vacuum gas atomization treatment described in step three is as follows: First, the ingot is melted and cast under vacuum conditions, with a vacuum degree of 8-9 × 10⁻⁶. -3 The temperature is set at 1273-1373K. After the ingot is melted, the molten metal is atomized into droplets by a high-pressure gas flow through a nozzle, thus completing the vacuum gas atomization process. The high-pressure gas flow has a pressure of 4-5MPa and is composed of 5N argon gas.
9. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... In step two, the quartz tube containing the alloy ingot has an outer diameter of 25-42mm, a wall thickness of 1-2mm, and a length of 200-300mm; in step four, the quartz tube containing the alloy micron particles has an outer diameter of 18-23mm, a wall thickness of 1-2mm, and a length of 120-180mm; and in step four, the additional quartz tube has an outer diameter of 25-30mm, a wall thickness of 1-2mm, and a length of 250-300mm.
10. The method for preparing a magnetic refrigerant with a wide ferromagnetic austenitic temperature range according to claim 1, characterized in that... Before processing at 373-773K as described in step four, raise the temperature to 373-773K and hold it for 10-20 minutes.
Citation Information
Patent Citations
A Mn-Ni-Sn-Co alloy thin strip and a preparation method thereof
CN106119661B
A Ni-Co-Mn-Sn magnetic refrigeration material and its preparation method
CN108330372B