Electrolyte, battery and electrical device
By introducing the first and second additives into the electrolyte, a dense membrane structure and phosphorus oxide compounds are formed, which solves the problems of large gas production and capacity attenuation during high-temperature storage of the battery, and improves the high-temperature cycle performance and electrochemical stability of the battery. Extended battery life.
Patent Information
- Application Number
- CN202410846546.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing batteries produce large amounts of gas during high-temperature storage, suffer severe high-temperature cycle capacity attenuation, and have a large impedance DCR growth rate, resulting in a decline in battery performance.
The first additive and the second additive are introduced into the electrolyte. The first additive is preferentially oxidized at the positive electrode to form a dense CEI film. The second additive decomposes to generate phosphorus oxide compounds and reacts with oxygen to remove oxygen during high-temperature storage and inhibit the electrolyte. Decompose and improve the film formation uniformity and stability of SEI film and CEI film.
It effectively suppresses gas generation during high-temperature storage, improves the high-temperature cycle performance and electrochemical stability of the battery, reduces battery impedance and cycle impedance growth rate, and extends the service life of the battery.
Smart Images

Figure CN118398901B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of batteries, and in particular, relates to electrolytes, batteries and electrical devices. Background Art
[0002] With the rapid development of electronic equipment, electric vehicles, smart homes, power tools, smart transportation and other markets, the demand for batteries is also increasing. Taking lithium-ion batteries as an example, they are widely used in consumer electronics, energy storage and power batteries, smart homes and other fields because of their advantages such as high specific energy, long cycle life and low self-discharge. Usually, the battery includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The electrolyte usually includes a solvent, an electrolyte lithium salt and an electrolyte additive. The performance of the battery can be effectively improved by adding electrolyte additives to the electrolyte. However, the current electrolyte additives still have problems in actual application. Summary of the invention
[0003] The present application aims to solve one of the related technical problems to a certain extent. To this end, one purpose of the present application is to provide an electrolyte, a battery and an electrical device, wherein the electrolyte is introduced with a first additive, a second additive and a third additive that can be selectively added, which is conducive to improving the film formation uniformity and stability of the SEI film and the CEI film, improving the high temperature cycle performance and electrochemical stability of the battery, effectively inhibiting the generation of gas, and solving the problems of large gas production and severe high temperature cycle capacity attenuation during high temperature storage of the battery, and large impedance DCR growth rate.
[0004] In a first aspect, the present application provides an electrolyte, comprising: a first additive shown in formula I, a second additive shown in formula II,
[0005] , ,
[0006] Wherein, R1, R2, and R3 are independently C 1-3 Alkyl, C 1-3 Any of the halogenated alkyl groups.
[0007] The electrolyte of the present application includes a first additive shown in formula I and a second additive shown in formula II, wherein the oxidation and reduction potentials of the first additive are both higher than those of conventional electrolyte solvents. During the pre-charging process of the battery, the first additive will be oxidized at the positive electrode and reduced at the negative electrode before the solvent, and then it is easy to form a dense CEI film at the positive electrode and a dense SEI film at the negative electrode, thereby inhibiting the dissolution of transition metal elements (such as manganese) in the active material of the positive electrode plate, thereby reducing the attenuation of high-temperature cycle capacity, and as a low-impedance additive, it can also reduce the battery impedance and reduce the cycle impedance (DCR) growth rate. The first additive will produce gas due to the breakage of the S=O bond at a high temperature of 60°C, resulting in an increase in the gas production during high-temperature storage. The main component of the gas is oxygen. The second additive is used in combination with the first additive, which can not only decompose phosphorus free radicals and oxygen free radicals when heated, and then generate phosphorus oxygen compounds, which can react with oxygen to remove the oxygen generated during high-temperature storage. Moreover, the second additive also has a high antioxidant capacity, which can further inhibit the decomposition of the electrolyte, thereby reducing the generation of gas. In summary, the present application simultaneously introduces the first additive and the second additive into the electrolyte, so that the two can cooperate with each other, which is not only beneficial to improve the film formation uniformity and stability of the SEI film and the CEI film, but also can improve the high-temperature cycle performance and electrochemical stability of the battery, effectively inhibit the generation of gas, and solve the problems of large gas production during high-temperature storage of the battery, severe attenuation of high-temperature cycle capacity, and large impedance DCR growth rate.
[0008] In some embodiments, R1, R2, and R3 are independently any one of methyl and halogenated methyl. This is beneficial for the second additive to have a better coordination effect with the first additive, and is also beneficial for achieving a better effect of inhibiting gas generation based on a lower dosage of the second additive.
[0009] In some embodiments, R1, R2, and R3 are all methyl.
[0010] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the first additive in the electrolyte is 0.5% to 2%. This is not only conducive to the formation of a uniform and stable SEI film and CEI film, but also enables the electrolyte and the battery to obtain better storage stability, high temperature performance and electrochemical stability, and can reduce battery impedance and reduce the cycle impedance (DCR) growth rate.
[0011] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the second additive in the electrolyte is 0.1% to 2%. This can effectively inhibit the decomposition and gas production of the electrolyte during the battery charge and discharge cycle and high-temperature storage process, thereby reducing the gas production of the battery, and can also reduce the risk of increased battery impedance and decreased electrochemical performance due to excessive content of the second additive.
[0012] In some embodiments, the mass ratio of the first additive to the second additive is 0.25 to 20. This can provide the electrolyte and the battery with better storage stability, high temperature performance, and electrochemical stability, reduce battery impedance and gas production, and reduce the cycle impedance (DCR) growth rate.
[0013] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the second additive in the electrolyte is 0.1% to 1%.
[0014] In some embodiments, the electrolyte further comprises: a third additive represented by formula III, R4 is any one of hydrogen, a substituted or unsubstituted hydrocarbon group, and a substituted or unsubstituted aromatic group, n is a positive integer, .
[0015] In some embodiments, R4 is substituted or unsubstituted C 1-12 This is beneficial to further improve the high temperature cycle performance and electrochemical stability of the electrolyte.
[0016] In some embodiments, n≥2. This helps the third additive to achieve better acid removal and water suppression effects at a lower dosage.
[0017] In some embodiments, the third additive includes hexamethylene diisocyanate.
[0018] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the third additive in the electrolyte is 0.01% to 1%, thereby achieving a better acid removal and water suppression effect while taking into account the cost, and improving the high temperature cycle performance and electrochemical stability of the electrolyte.
[0019] In some embodiments, the mass ratio of the first additive to the third additive is 0.25 to 20. This can better balance the cost and exert a good acid removal and water suppression effect, and further, the electrolyte and the battery can obtain better high temperature cycle performance and electrochemical stability on the basis of a lower additive dosage, and reduce the gas production of the battery.
[0020] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the third additive in the electrolyte is 0.01% to 0.2%.
[0021] In some embodiments, the electrolyte further includes: a negative electrode film-forming additive, which is beneficial to further improve the film-forming effect of SEI and enhance the uniformity of SEI film-forming.
[0022] In some embodiments, the negative electrode film-forming additive includes at least one of vinylene carbonate, fluoroethylene carbonate, and vinyl ethylene carbonate.
[0023] In some embodiments, based on the total mass of the electrolyte, the mass proportion of the negative electrode film-forming additive in the electrolyte is 0.5% to 2.0%.
[0024] In some embodiments, the electrolyte further comprises a stabilizer, thereby improving the storage stability of the electrolyte.
[0025] In some embodiments, the stabilizer includes at least one of triphenyl phosphite, triphenyl phosphate, pentafluoroethoxyphosphazene, and biscyclohexylcarbocyanide.
[0026] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the stabilizer in the electrolyte is 0.1% to 0.5%.
[0027] In some embodiments, the electrolyte further includes: an organic solvent and a lithium salt.
[0028] In some embodiments, the organic solvent includes a carbonate solvent and / or a carboxylate solvent, or the organic solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate and butyl propionate, or the organic solvent includes ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate in a mass ratio of 1:(0.5-2):(0.5-2).
[0029] In some embodiments, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, and lithium bis(trifluoromethanesulfonyl)imide, or the lithium salt is lithium bis(fluorosulfonyl)imide.
[0030] In some embodiments, the molar concentration of the lithium salt in the electrolyte is 0.8 mol / L to 2 mol / L.
[0031] The second aspect of the present application provides a battery, comprising the electrolyte described in the first aspect. Thus, the battery has good high temperature cycle performance and good electrochemical stability, and has low gas production, low impedance growth rate during high temperature cycles, and long service life.
[0032] In some embodiments, the battery further comprises: a positive electrode active material, the battery is a lithium ion battery, and the positive electrode active material comprises: Li a Ni b Co c M1d M2 e O f R g and / or LiMn x Fe 1-x PO4, wherein 1≤a≤1.2, 0.5≤b≤1, 0≤c≤1, 0≤d≤1, 0≤e≤0.2, b+c+d+e=1, 1≤f≤2, 0≤g≤1, f+g=2; M1 includes Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and R includes at least one of N, F, S, and Cl; 0≤x≤1.
[0033] In some embodiments, the battery further comprises: a positive electrode active material, the battery is a sodium ion battery, and the positive electrode active material comprises Na α M3 β (X γ O δ ) θ (P2O7)μZ λ , wherein M3 includes a transition metal element, X includes at least one of P, S, Si, and W, Z includes at least one of N, F, S, and Cl, 1≤α≤10, 0<β≤5, 0≤γ≤10, 0≤δ≤10, 0≤θ≤5, 0≤μ≤5, and 0≤λ≤5.
[0034] The third aspect of the present application provides an electrical device, comprising the battery described in the second aspect.
[0035] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. DETAILED DESCRIPTION
[0036] The embodiments of the present application are described in detail below, which are intended to be used to explain the present application but should not be construed as limiting the present application.
[0037] The technical solution of this application is completed by the inventor based on the following findings:
[0038] Increasing the gram capacity of the positive electrode active material and the charging voltage of the battery can effectively increase the energy density of the battery. However, in actual use, it is found that when the energy density of the battery is increased by the above methods, the cycle performance and high-temperature storage performance of the battery are seriously damaged. For example, taking a lithium battery in which the positive electrode active material is lithium manganese iron phosphate and the negative electrode active material is graphite, the energy density of the battery can be significantly improved by increasing the manganese content of the positive electrode active material. However, this is accompanied by the deterioration of the structural stability of the positive electrode active material due to the increase in manganese content, and the increase in irreversible phase changes of the positive electrode active material during the charge and discharge cycle, resulting in the dissolution of transition metals and the loss of active sites in the positive electrode active material. In addition, during the cycle, Mn 2+ It will be deposited on the negative electrode graphite surface, causing the SEI (Solid Electrolyte Interface) film on the graphite surface to continuously decompose and regenerate, continuously consuming active lithium, and increasing polarization due to SEI film thickening, electrolyte consumption, and byproduct blocking of lithium insertion and extraction channels. At the same time, the positive electrode active material produces manganese-deficient phases and Mn due to manganese dissolution. 3+ The Jan-Taylor effect will cause the lattice distortion and structural stability of the positive electrode active material to decrease, hindering the diffusion of lithium ions during the subsequent charge and discharge process, increasing the polarization of the battery and increasing the high-temperature cycle capacity loss. And because the amount of active lithium embedded in the positive electrode decreases, the amount of low-lithium graphite embedded in the negative electrode increases, and the degree of disorder on the graphite surface increases, the regeneration reaction of the SEI film will also be promoted. The dissolution of Mn, the decomposition and regeneration of the SEI film will all promote the decomposition of the electrolyte, leading to problems such as high-temperature storage gas production, high-temperature cycle capacity attenuation, and a large DCR growth rate in lithium manganese iron phosphate batteries.
[0039] As an important component of lithium secondary batteries, electrolyte has an important impact on the overall performance of the battery. Additives are an important component of electrolyte, and suitable additives can significantly improve the performance of the battery, such as cycle performance, high temperature performance, etc. To this end, the inventors envision that the above problems can be improved by improving the electrolyte.
[0040] In the present application, by simultaneously introducing the first additive and the second additive into the electrolyte, the two can cooperate with each other, which is not only conducive to improving the film formation uniformity and stability of the SEI film and the CEI film, but also can improve the high temperature cycle performance and electrochemical stability of the battery, effectively inhibit the generation of gas, and solve the problems of large gas production and severe high temperature cycle capacity attenuation and large impedance DCR growth rate during high temperature storage of the battery. Furthermore, after the electrolyte is used in the battery, better high temperature storage performance, high temperature cycle performance and longer service life can be obtained.
[0041] In view of this, the first aspect of the present application provides an electrolyte, comprising: a first additive shown in formula I and a second additive shown in formula II,
[0042] , ,
[0043] Wherein, R1, R2, and R3 are independently C 1-3 Alkyl, C 1-3 Any of the halogenated alkyl groups.
[0044] Among them, the first additive shown in Formula I has a strong polarity, a weak interaction with other non-polar molecules, less friction and collision between molecules, and has better stability compared with other sulfate compounds; in addition, compared with other sulfate compounds, the first additive shown in Formula I also has better thermal stability, not only can it be stored at room temperature without low-temperature storage, it can operate stably over a wide voltage range, and has good cycle life and capacity retention rate, and also has better high-temperature performance, and can maintain relatively stable electrochemical properties in a high-temperature environment, thereby extending the service life of the battery. Moreover, the oxidation and reduction potentials of the first additive shown in Formula I are both higher than those of conventional electrolyte solvents. During the pre-charging process of the battery, it will be oxidized at the positive electrode and reduced at the negative electrode before the solvent, and then it is easy to form a dense CEI film at the positive electrode and a dense SEI film at the negative electrode. Among them, the first additive will form a small amount of inorganic salts (Li2SO4, Li2O) in the CEI film formed by decomposition of the positive electrode, which improves the rigidity and flexibility of the positive electrode interface layer, inhibits the decomposition of the electrolyte, and improves the stability of the positive electrode interface film. In addition, the CEI film formed by the first additive can also reduce The electrochemical impedance of the positive electrode accelerates the transmission rate of lithium ions, helps form a more stable electrode-electrolyte interface, reduces the internal resistance and interface reaction of the battery, and protects the positive electrode. In addition, it can also inhibit the dissolution of transition metal elements (such as manganese) in the active materials of the positive electrode plate, thereby reducing the attenuation of high-temperature cycle capacity; lithium carbonate will be generated in the SEI film formed by the first additive, which helps to improve the film formation uniformity and stability of the SEI film; furthermore, the first additive is a low-impedance additive, which can also reduce the battery impedance and reduce the cycle impedance (DCR) growth rate.
[0045] However, the first additive will break the S=O bond and produce gas at a high temperature of 60°C, resulting in an increase in gas production during high-temperature storage. After testing the gas production components during high-temperature storage, it was found that the gas mainly contained oxygen. The second additive shown in Formula II can be preheated to easily decompose phosphorus free radicals P· and oxygen free radicals O·. P· and O· will form phosphorus oxide compounds, which can react with oxygen to remove the oxygen produced during high-temperature storage. Moreover, the second additive also has a high antioxidant capacity, which can further inhibit the decomposition of the electrolyte, thereby further reducing the generation of gas. In unsaturated phosphate esters, since the unsaturated bonds are rich in electrons and are not easy to break to form free radicals P· and O·, and the phosphorus oxygen bond and the unsaturated bond are easy to form conjugation and are not easy to break, compared with unsaturated phosphate esters, the saturated phosphate ester shown in Formula II is easier to preheat and decompose into phosphorus free radicals P· and oxygen free radicals O·.
[0046] In summary, the present application simultaneously introduces the first additive and the second additive into the electrolyte, so that the two can cooperate with each other, so that the electrolyte can be used in the battery, which is not only beneficial to improve the film formation uniformity and stability of the SEI film and the CEI film, but also can improve the high-temperature cycle performance and electrochemical stability of the battery, effectively inhibit the generation of gas, and solve the problems of large gas production during high-temperature storage of the battery, severe attenuation of high-temperature cycle capacity, and large impedance DCR growth rate.
[0047] It should be noted that in the second additive represented by Formula II of the present application, R1, R2, and R3 may be completely the same, or may be different or not completely the same. 1-3 Taking alkyl as an example, R1, R2, and R3 can be alkyl groups with the same number of carbon atoms, or alkyl groups with the same or different number of carbon atoms. In addition, in Formula II, when R1, R2, and R3 contain at least two haloalkyl groups, the number of carbon atoms of the at least two haloalkyl groups can be the same or different, and the number of halogen substitutions and the type of halogen in the at least two haloalkyl groups can be the same or different. It is understood that the halogen refers to an element of Group VIIA, such as one or more of F, Cl, Br, and I; the haloalkyl group can be an alkyl group partially or completely substituted by halogen. In addition, unless otherwise specified, in this application, the term "C 1~3 "Alkyl" is understood to mean a straight-chain or branched saturated monovalent hydrocarbon radical having 1, 2 or 3 carbon atoms.
[0048] In some specific embodiments of the present application, in the second additive shown in Formula II, R1, R2, and R3 can be independently any one of a methyl group and a halogenated methyl group. Exemplarily, R1, R2, and R3 can be independently methyl or a fluoromethyl group. As a specific example, R1, R2, and R3 can all be methyl groups, that is, the second additive shown in Formula II can be trimethyl phosphate (TMP). As a result, it is not only beneficial for the second additive to have a better coordination effect with the first additive, but also beneficial for achieving a better effect of suppressing gas production on the basis of a lower dosage of the second additive.
[0049] In some specific embodiments of the present application, based on the total mass of the electrolyte, the mass percentage of the first additive in the electrolyte can be 0.5% to 2%, for example, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9% or 2.0%, etc. Properly increasing the amount of the first additive is conducive to further improving the high temperature cycle performance and electrochemical stability of the battery, while properly reducing the amount of the first additive is conducive to reducing costs and reducing the risk of increased electrolyte impedance due to the failure of the first additive to fully react. In this application, by controlling the amount of the first additive added in the electrolyte to meet the given range, it is not only conducive to forming a uniform and stable SEI film and CEI film, but also enables the electrolyte and the battery to obtain better storage stability, high temperature performance and electrochemical stability, which can reduce the battery impedance and reduce the cycle impedance (DCR) growth rate.
[0050] In some specific embodiments of the present application, based on the total mass of the electrolyte, the mass percentage of the second additive in the electrolyte can be 0.1%~2%, such as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9% or 2.0%, etc. In the present application, by controlling the amount of the second additive added in the electrolyte to meet the given range, it is possible to better inhibit the decomposition and gas production of the electrolyte during the battery charge and discharge cycle and high temperature storage process, thereby reducing the gas production of the battery, and also reduce the risk of increased battery impedance and decreased electrochemical performance due to excessive content of the second additive. Further, the mass percentage of the second additive in the electrolyte can be 0.1%~1%, thereby further reducing the risk of increased battery impedance and decreased electrochemical performance due to excessive content of the second additive on the basis of effectively reducing the gas production of the battery.
[0051] In some specific embodiments of the present application, in the electrolyte, the mass ratio of the first additive to the second additive can be 0.25-20, for example, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5, 19, 19.5 or 20, etc. Based on the amount of the first additive, increasing the amount of the second additive is beneficial to further inhibiting the decomposition and gas production of the electrolyte and the first additive during charge and discharge cycles and in high temperature environments. In the present application, by controlling the relative amounts of the second additive and the first additive to meet the given range, it is beneficial for the battery to form a uniform and stable SEI film and CEI film, reduce the internal resistance and interface reaction of the battery, and protect the positive electrode plate. It can also better inhibit the decomposition and gas production of the electrolyte during the battery charge and discharge cycle and high-temperature storage process, reduce the gas production of the battery, and reduce the risk of increased battery impedance and decreased electrochemical performance due to excessive content of the second additive. As a result, the electrolyte and the battery can obtain better storage stability, high temperature performance and electrochemical stability, can reduce the battery impedance and gas production, and reduce the cycle impedance (DCR) growth rate.
[0052] In some specific embodiments of the present application, the electrolyte may further include: a third additive shown in Formula III, whose general formula is: , R4 is any one of hydrogen, substituted or unsubstituted hydrocarbon group, substituted or unsubstituted aromatic group, and n is a positive integer. Among them, the trace amount of water in the electrolyte may cause the electrolyte salt to hydrolyze to produce acidic impurities (such as LiPF6 will hydrolyze to produce HF), and the main component of the CEI film formed by the first additive at the positive electrode includes lithium carbonate. When the lithium carbonate content is high, it is easy to react with the negative electrode active material, such as graphite, to produce gas and destroy the SEI film on the surface of the negative electrode active material, and it is easy to be corroded by acidic impurities (such as HF, PF5, etc.), thereby causing the dissolution of transition metal elements (such as manganese) in the positive electrode active material; at the same time, when the lithium carbonate content is too high, it may also cause the SEI film to become thicker and reduce the electrochemical performance. By further introducing a third additive into the electrolyte, the effect of removing acid and inhibiting water can be achieved. The isocyanate group (-N=C=O) contained in the third additive can react with water and acidic impurities in the electrolyte to generate a polymer product, and the generated polymer can participate in promoting the formation of the SEI film and inhibit the deposition of transition metal elements dissolved from the positive electrode at the negative electrode, thereby further improving the high-temperature cycle performance and electrochemical stability of the electrolyte. The improvement of the high-temperature cycle performance and electrochemical stability of the electrolyte is conducive to further reducing the gas production of the battery.
[0053] In the embodiments of the present application, the term "hydrocarbon group" may be a hydrocarbon group including one or more carbon atoms, and the carbon chain formed by the multiple carbon atoms may include at least one of a carbon-carbon single bond, a carbon-carbon double bond and a carbon-carbon triple bond; in the term "unsubstituted or substituted by any group", the "substituted by any group" means that at least one hydrogen atom bound to the carbon atom is replaced by any group other than hydrogen, for example, it may be substituted by a halogen (such as fluorine), by a hydrocarbonoxy group, by a hydroxyl group, etc. Taking "a hydrocarbon group unsubstituted or substituted by any group" as an example, it should be understood that the hydrocarbon group may not be substituted, or may be substituted by one or more (such as 1, 2, 3, 4) substituents at any position. When there are two or more substituents, the multiple substituents may be the same or different, and may be located at the same position or at different positions. In the "substituted by any group" mentioned in the present application, the arbitrary group includes but is not limited to halogen, hydrocarbon, hydrocarbonoxy, cyano, amino, etc., wherein the hydrocarbon or hydrocarbonoxy included in the arbitrary group may be chain or cyclic, and the term "hydrocarbonoxy" should be understood as -O-hydrocarbon, indicating that the hydrocarbon group is connected to the rest of the molecule through an oxygen atom.
[0054] In some specific embodiments of the present application, in the third additive shown in Formula III, R4 can be substituted or unsubstituted C 1-12 The term "C 1-12 "Alkyl" should be understood to mean a straight-chain or branched saturated monovalent hydrocarbon group having 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12 carbon atoms. As a result, the third additive can achieve a better effect of removing acid and inhibiting water on the basis of a lower addition amount, thereby further improving the high temperature cycle performance and electrochemical stability of the electrolyte and reducing the gas production of the battery.
[0055] In some specific embodiments of the present application, the third additive shown in Formula III may include a monoisocyanate (n=1) compound or a polyisocyanate (n≥2, exemplary, n may be 2, 3, 4, 5, 6, 7, 8, 9 or 10, etc.) compound. In some specific embodiments, in the third additive shown in Formula III, n may be ≥2, exemplary, n may be 2, 3, 4, 5, 6, 7, 8, 9 or 10, etc., and the increase in the number of isocyanate groups in the third additive is conducive to better acid removal and water inhibition effects. Therefore, the selection of isocyanate compounds with n≥2 is conducive to further achieving better acid removal and water inhibition effects on the basis of a lower addition amount, thereby further improving the high temperature cycle performance and electrochemical stability of the electrolyte and reducing the gas production of the battery.
[0056] In some specific embodiments of the present application, the third additive may be hexamethylene diisocyanate (HDI). HDI contains two isocyanate groups, which not only has better acid removal and water inhibition effects, but also has better stability and relatively low production costs. It can improve the high-temperature cycle performance and electrochemical stability of the electrolyte at a lower dosage (such as a mass share of 0.01%-0.2% in the electrolyte) and reduce the gas production of the battery.
[0057] In some specific examples of the present application, in the second additive shown in Formula II, R1, R2, and R3 may all be methyl groups, and the third additive shown in Formula III may include hexamethylene diisocyanate (HDI). The combination of trimethyl phosphate and hexamethylene diisocyanate with the first additive shown in Formula I can achieve a good coordination effect, significantly improve the high-temperature cycle performance and electrochemical stability of the battery, effectively inhibit the generation of gas, and solve the problems of large gas production and severe high-temperature cycle capacity attenuation during high-temperature storage of the battery, and large impedance DCR growth rate.
[0058] In some specific embodiments of the present application, based on the total mass of the electrolyte, the mass percentage of the third additive in the electrolyte can be 0.01% to 1%, for example, it can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, etc. By controlling the amount of the third additive added to the electrolyte to meet the given range, it can achieve a better acid removal and water suppression effect on the basis of taking into account the cost, thereby further inhibiting the deposition of transition metal elements dissolved from the positive electrode at the negative electrode, improving the high temperature cycle performance and electrochemical stability of the electrolyte, and reducing the decomposition and gas production of the electrolyte during the battery charge and discharge cycle. Furthermore, the mass percentage of the third additive in the electrolyte can be 0.01%-0.2%, which can further take into account the cost and exert a better acid removal and water inhibition effect, and then can better improve the high temperature cycle performance and electrochemical stability of the electrolyte on the basis of a lower dosage, and reduce the gas production of the battery.
[0059] In some specific embodiments of the present application, in the electrolyte, the mass ratio of the first additive to the third additive can be 0.25~20, for example, it can be 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5, 19, 19.5 or 20, etc. Taking the dosage of the first additive as a benchmark, increasing the dosage of the third additive is beneficial to further improve the acid removal and water suppression effect, improve the stability of the SEI film and the CEI film, inhibit the dissolution of transition metal elements in the active material of the positive electrode plate and the deposition of transition metal elements dissolved from the positive electrode on the surface of the negative electrode plate, improve the high temperature cycle performance and electrochemical stability of the electrolyte, and reduce the decomposition and gas production of the electrolyte during the battery charge and discharge cycle. In this application, by controlling the relative dosage of the third additive and the first additive to meet the given range, it is possible to better balance the cost and exert a better acid removal and water suppression effect, and then the electrolyte and the battery can obtain better high temperature cycle performance and electrochemical stability on the basis of a lower dosage of additives, and reduce the gas production of the battery.
[0060] In some specific embodiments of the present application, the electrolyte may further include: a negative electrode film-forming additive. The addition of the negative electrode film-forming additive is conducive to further improving the film-forming effect of SEI and improving the uniformity of SEI film-forming.
[0061] In some specific embodiments of the present application, the negative electrode film-forming additive may include at least one of vinylene carbonate, fluoroethylene carbonate, and vinyl ethylene carbonate. The given range of film-forming additives can better improve the film-forming effect of SEI and improve the uniformity of SEI film-forming.
[0062] In some specific embodiments of the present application, based on the total mass of the electrolyte, the mass proportion of the negative electrode film-forming additive in the electrolyte can be 0.5% to 2.0%, for example, 0.5%, 1.0%, 1.5%, 2.0%, etc. In this way, the uniformity of SEI film formation can be improved, and the manufacturing cost, high temperature cycle performance and electrochemical stability of the battery can be further taken into account, and the risk of increased battery impedance and decreased electrochemical performance caused by excessive use of the negative electrode film-forming additive can be reduced.
[0063] In some specific embodiments of the present application, the electrolyte may further include a stabilizer. The addition of a stabilizer can improve the storage stability of the electrolyte, help keep the electrolyte stable during storage and transportation, and reduce the risk of deterioration due to changes in the external environment.
[0064] In some specific embodiments of the present application, the stabilizer may include at least one of triphenyl phosphite, triphenyl phosphate, pentafluoroethoxyphosphazene, and dicyclohexylcarbocyanide. The stabilizer within the given range can better improve the stability of the electrolyte during storage, transportation, and use.
[0065] In some specific embodiments of the present application, based on the total mass of the electrolyte, the mass percentage of the stabilizer in the electrolyte can be 0.1%~0.5%, for example, it can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%, etc., thereby not only improving the storage stability of the electrolyte, but also helping to take into account the manufacturing cost of the electrolyte and broaden the application scenarios of the electrolyte.
[0066] In some specific embodiments of the present application, the electrolyte may further include: an organic solvent and a lithium salt. Optionally, the electrolyte may be used in a lithium battery. The organic solvent is the main component of the electrolyte and is an important carrier for ion transport, which can make the organic solvent have a higher solubility of lithium salt, so that the electrolyte has a higher ionic conductivity. After the lithium salt is dissolved in the organic solvent, lithium ions can be released, and the lithium ions and the organic solvent form a solvation structure, which is conducive to the rapid migration of lithium ions.
[0067] In some specific embodiments of the present application, the organic solvent may include a carbonate solvent and / or a carboxylate solvent, thereby improving the dispersion uniformity and ion conductivity of the electrolyte.
[0068] In some specific embodiments of the present application, the organic solvent may include at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate and butyl propionate. The organic solvent in the given range can make the electrolyte have a higher ionic conductivity after dissolving the lithium salt, which is beneficial to improve the cycle life, charge and discharge rate, high temperature performance, low temperature performance and energy density of the battery.
[0069] In some specific embodiments of the present application, the composition of the organic solvent can be flexibly adjusted according to the actual situation of the battery system, for example, as some specific examples, the organic solvent can include ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) in a mass ratio of 1: (0.5-2): (0.5-2). The organic solvent can be suitable for layered transition metal oxides as positive electrode active materials (for example, Li a Ni b Co c M1 d M2e O f R g A battery system comprising a positive electrode active material, wherein 1≤a≤1.2, 0.6≤b≤1, 0≤c≤1, 0≤d≤1, 0≤e≤0.2, b+c+d+e=1, 1≤f≤2, 0≤g≤1, f+g=2; M1 includes Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, and Nb, and R includes at least one of N, F, S, and Cl).
[0070] In some specific embodiments of the present application, the lithium salt may include at least one of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium tetrafluoroborate (LiBF4) and lithium bis(trifluoromethanesulfonyl)imide (C2F6LiNO4S2). Further, the lithium salt may be lithium bis(fluorosulfonyl)imide, which helps to reduce the generation of hydrogen fluoride in the electrolyte, and then the amount of the third additive can be reduced accordingly, thereby reducing the manufacturing cost.
[0071] In some specific embodiments of the present application, the molar concentration of the lithium salt in the electrolyte may be 0.8 mol / L to 2 mol / L, for example, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L or 2 mol / L, etc. The cost of lithium salt in the electrolyte accounts for a relatively high proportion, and controlling the concentration of lithium salt in the electrolyte to meet the given range is beneficial for fully dissolving the lithium salt in the organic solvent, and also for making the electrolyte have both high ionic conductivity and low manufacturing cost.
[0072] In some specific embodiments of the present application, the electrolyte has a wide range of applications, such as being suitable for lithium-ion batteries with relatively low operating voltages such as lithium iron manganese phosphate systems, and lithium-ion batteries with relatively high operating voltages such as nickel cobalt manganese systems. For systems with low or high operating voltages, it is beneficial to improve the high-temperature cycle performance and electrochemical stability of the battery, effectively inhibit the generation of gas, and solve the problems of large gas production during high-temperature storage of the battery, severe high-temperature cycle capacity attenuation, and large impedance DCR growth rate.
[0073] In some specific embodiments of the present application, in addition to the above components, the electrolyte may optionally include a small amount of other conventional additives or auxiliary agents that can improve certain battery properties. Those skilled in the art can choose according to actual needs, which will not be described in detail here.
[0074] The second aspect of the present application proposes a battery, which includes the electrolyte described in the first aspect. It should be noted that the characteristics and effects described for the electrolyte in the first aspect of the present application are also applicable to the battery in the second aspect of the present application, and will not be repeated here. In general, the battery has good high-temperature cycle performance and good electrochemical stability, and has low gas production and low impedance growth rate during high-temperature cycles. In addition, it should be noted that the type of the battery is not particularly limited, and those skilled in the art can flexibly choose according to actual needs, for example, it can be a secondary battery.
[0075] According to some specific embodiments of the present application, the battery may be a lithium ion battery or a sodium ion battery.
[0076] Typically, a battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0077] In some embodiments of the present application, the positive electrode sheet may include a positive electrode current collector and a positive electrode active material layer disposed on the surface of the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material, a conductive agent and a binder, the positive electrode current collector may include a metal foil or a composite positive electrode current collector, for example, the metal foil may be aluminum foil, the composite positive electrode current collector may include a polymer material base and a metal layer formed on at least one side of the surface of the polymer material base, for example, the composite negative electrode current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.). The positive electrode active material may include the above-mentioned positive electrode active material or a commonly used positive electrode active material in the art. The conductive agent and the binder may be conventional materials in the art.
[0078] In some specific embodiments of the present application, when the battery is a lithium-ion battery, its positive electrode active material may include: Li a Ni b Co c M1 d M2 e O f R g and / or LiMn x Fe 1-xPO4, wherein 1≤a≤1.2, 0.5≤b≤1, 0≤c≤1, 0≤d≤1, 0≤e≤0.2, b+c+d+e=1, 1≤f≤2, 0≤g≤1, f+g=2; M1 may include Mn and / or Al, M2 may include at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, R may include at least one of N, F, S, Cl; 0≤x≤1. As an example, the positive active material of the lithium ion battery may include LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.7 Co 0.1 Mn 0.2 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiMn 0.6 Fe 0.4 PO4、LiMn 0.7 Fe 0.3 PO4、LiMn 0.8 Fe 0.2 PO4、LiMn 0.5 Fe 0.5 One or more of PO4.
[0079] According to some embodiments of the present application, when the battery is a sodium ion battery, its positive electrode active material may include Na α M3 β (X γ O δ ) θ (P2O7)μZ λ , wherein M3 may include a transition metal element, X may include at least one of P, S, Si, and W, Z may include at least one of N, F, S, and Cl, 1≤α≤10, 0<β≤5, 0≤γ≤10, 0≤δ≤10, 0≤θ≤5, 0≤μ≤5, and 0≤λ≤5. As an example, the positive active material of the sodium ion battery may include one or more of NaFePO4, Na2FeP2O7, Na4Fe3(PO4)2P2O7, Na3V2(PO4)3, and Na2Fe(SO4)2.
[0080] In some embodiments of the present application, the negative electrode plate may include a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector, the negative electrode active material layer may include a negative electrode active material, a conductive agent and a binder, wherein the negative electrode current collector may be a metal foil or a composite current collector, for example, the metal foil may be a copper foil, the composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate, for example, the composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.). The negative electrode active material may include a commonly used negative electrode active material in the art (such as at least one of commonly used negative electrode active materials such as graphite, silicon-carbon composite materials, silicon materials, lithium metal, lithium titanate, etc.). The conductive agent and the binder may be conventional materials in the art.
[0081] In some embodiments of the present application, the isolation membrane can adopt an isolation membrane that is well known in the art and can be used in batteries and is stable to the electrolyte used. For example, its material can include but is not limited to at least one of polyolefins, aromatic polyamides, polytetrafluoroethylene, and polyether sulfone, such as a polyethylene diaphragm, a polypropylene diaphragm, a PE ceramic coated diaphragm, etc., and the specific material can be flexibly selected according to needs.
[0082] The third aspect of the present application proposes an electrical device, which includes the battery described in the second aspect of the present application. It should be noted that the features and effects described for the battery in the second aspect of the present application are also applicable to the electrical device, and will not be repeated here. In addition, it should be noted that the specific type of the electrical device is not particularly limited, and those skilled in the art can flexibly choose according to actual needs, for example, it may include but not be limited to electronic equipment, vehicles, etc.
[0083] The embodiments of the present application are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. In addition, unless otherwise explicitly stated, all reagents used in the following embodiments are commercially available or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0084] Example 1
[0085] 1. Preparation of positive electrode sheet
[0086] The positive electrode active material (LiNi 0.8 Co 0.1 Mn 0.1 O2 and LiMn 0.6 Fe0.4 PO4 is mixed in a mass ratio of 7:3), binder polyvinylidene fluoride (PVDF), conductive agent carbon black, and conductive agent carbon nanotubes are mixed in a weight ratio of 93:2.3:2:0.7, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the coating amount is 35g / m 2 After drying at 85°C, cold pressing is performed, and trimming, cutting, and slitting are performed. After slitting, it is dried at 85°C under vacuum conditions for 4 hours, and the pole ears are welded to obtain the positive electrode sheet.
[0087] 2. Preparation of negative electrode sheet
[0088] The negative electrode active material graphite, the conductive agent carbon black, the thickener sodium carboxymethyl cellulose (CMC-Na), and the binder styrene-butadiene rubber were mixed in a weight ratio of 95:1.5:1:2.5, and deionized water was added to obtain the negative electrode slurry under the action of a vacuum mixer; the negative electrode slurry was evenly coated on the negative electrode current collector copper foil, and the coating amount was 20g / m 2 After drying at 85°C, cold pressing is performed, and edge trimming, cutting, and slitting are performed. After slitting, it is dried at 85°C under vacuum conditions for 4 hours, and the tabs are welded to obtain the negative electrode sheet.
[0089] 3. Preparation of electrolyte
[0090] In a glove box filled with argon (water content <10ppm, oxygen content <1ppm), the solvents ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate are mixed evenly in a mass ratio of 3:5:2, and fully dried lithium hexafluorophosphate is quickly added to the mixed solvent to make the molar concentration of lithium hexafluorophosphate in the electrolyte 1mol / L, and electrolyte additives are added, and the electrolyte is obtained after fully mixing. Among them, the mass percentage of the first additive in the electrolyte is 0.5%, and the mass percentage of the second additive in the electrolyte is 0.5%. Among them, the first additive is a compound shown in formula I (CAS number: 2520352-94-5), and the second additive is trimethyl phosphate (TMP, CAS number: 512-56-1).
[0091] 4. Preparation of isolation membrane
[0092] A polyethylene isolation film with a thickness of 8 μm was selected.
[0093] 5. Lithium-ion battery preparation
[0094] The positive electrode sheet, negative electrode sheet and separator prepared according to the above process were laminated to form a lithium-ion battery with a thickness of 4.7 mm, a width of 55 mm and a length of 60 mm, and vacuum-baked at 75°C for 10 hours, and the above-prepared electrolyte was injected. After standing for 24 hours, the battery was placed in an environment of 45°C, a pressure of 3 kg was applied, and it was charged to 4.0V at 0.1C (160mA), and then stood for 2 days (to fully activate the battery) to obtain a battery.
[0095] Examples 2 to 25 and Comparative Examples 1 to 13
[0096] The differences between Examples 2 to 25 and Comparative Examples 1 to 13 and Example 1 are shown in Tables 1, 2 and 3, wherein Table 1 shows the differences and test results between Examples 1 to 19; Table 2 shows the differences and test results between Examples 20 to 21, 25 and Comparative Examples 1 to 10; Table 3 shows the differences and test results between Examples 22 to 24 and Comparative Examples 11 to 13 and Example 1. In Examples 22 to 24, the composition of the positive electrode active material used in the positive electrode sheet is different from that in Example 1, as shown in Table 3. The preparation method of the battery in Example 25 is the same as that in Example 6, except that the positive electrode active material is Na4Fe3(PO4)2(P2O7) (NFPP for short), and the electrolyte salt in the electrolyte includes 0.8 mol / L NaPF6 and 0.2 mol / L NaFSI, as shown in Table 2. Among them, in Table 1 and Table 2, the CAS number of triethyl phosphate is 78-40-0; the CAS number of propyl isocyanate is 110-78-1; the CAS number of HDI is 822-06-0; the CAS number of vinylene carbonate is 872-36-6; the CAS number of triphenyl phosphite is 101-02-0; the CAS number of tripropargyl phosphate is 1779-34-6; the CAS number of TFMP (bis(2,2,2-trifluoroethyl)methyl phosphate) is 757-95-9; the CAS number of TMSP (tri(trimethylsilyl) phosphate) is 10497-05-9.
[0097] The high temperature storage performance and high temperature cycle performance of the batteries obtained in Examples 1 to 25 and Comparative Examples 1 to 13 were tested. The test method is as follows. The test results are shown in Tables 1, 2 and 3.
[0098] (1) High temperature storage performance test: The formed battery is charged to the upper cut-off voltage (4.35V for Example 1 and 3.65V for Example 25) at room temperature with a constant current and constant voltage of 1C, the initial battery thickness is tested, and the battery is discharged to the lower cut-off voltage (2.5V for Example 1 and 2V for Example 25) at 1C, and the initial discharge capacity of the battery is measured; then, the battery is charged to the upper cut-off voltage at room temperature with a constant current and constant voltage of 1C, and then stored at 60°C for 30 days, the battery thickness after storage is tested, and then the battery is discharged to the lower cut-off voltage at 1C, and the discharge capacity of the battery after storage is measured. The high temperature storage performance calculation formula is as follows:
[0099] Battery capacity retention rate (%) = discharge capacity after storage / initial discharge capacity × 100%;
[0100] Expansion rate (%) = (battery thickness after storage - initial battery thickness) / initial battery thickness × 100%.
[0101] (2) High temperature cycle performance test: At 45°C, the formed battery is charged at a constant current and constant voltage of 1C to the upper cut-off voltage, and then discharged at a discharge rate of 1C to the lower cut-off voltage, for 500 charge and discharge cycles:
[0102] Cycle capacity retention rate (%) = (500th discharge capacity / 1st cycle discharge capacity) × 100%;
[0103] High temperature cycle DCR growth rate: (DCR value after high temperature cycle - initial DCR value) / initial DCR value × 100%.
[0104] DCR test method: Place the battery in a 25°C environment, discharge it at a constant current of 1C to the lower cut-off voltage, let it stand for 5 minutes, charge it at a constant current and constant voltage of 1C to the upper cut-off voltage, the cut-off current is 0.05C, and then discharge it at a constant current of 1C for 30 minutes. Place the battery adjusted to 50% SOC at 25°C, let it stand for 5 minutes, and discharge it at a constant current of 2C for 30 seconds. The discharge current during 2C discharge is I 2C Record the initial voltage V0 and the voltage V1 after 30s of discharge. The discharge DC internal resistance calculation formula at 50% SOC is as follows: DCR (mΩ) = (V0-V1) / I 2C ×1000.
[0105]
[0106]
[0107]
[0108] Results and Conclusions:
[0109] Combining Examples 1 to 25 and Comparative Examples 1 to 13 and Tables 1 to 3, it can be seen that after the first additive and the second additive are simultaneously introduced into the electrolyte in the above embodiments of the present application, the expansion rate and capacity attenuation of the battery after storage at high temperature are significantly reduced, and the capacity retention rate of the battery after high-temperature cycling is significantly improved, and the impedance DCR growth rate after cycling is also reduced. After the electrolyte of the above embodiments of the present application is used in the battery, the high-temperature cycle performance and storage performance of the battery are effectively improved, and the gas production after high-temperature storage is also effectively reduced. In addition, it can be seen from Examples 1, 5, and 13 that adding an appropriate amount of the third additive to the electrolyte in combination with the first additive and the second additive can further improve the high-temperature cycle performance and electrochemical stability of the battery, and improve the expansion rate and capacity attenuation of the battery after storage at high temperature. The main reason for the analysis is that the third additive contains an isocyanate group (-N=C=O), which can react with H2O and acidic impurities in the electrolyte to generate a polymer product, and the generated polymer can participate in promoting the formation of the SEI film, achieving the effect of removing acid and inhibiting water, thereby improving the high-temperature cycle and electrochemical stability of the electrolyte. Further, in combination with Examples 5, 7, 9 and Comparative Examples 3, 4, 9, and 10, it can be seen that the introduction of the first additive into the electrolyte can effectively improve the high-temperature gas production and capacity attenuation problems of the battery, reduce the high-temperature cycle DCR growth rate, and improve the high-temperature cycle performance; the high-temperature gas production in Comparative Examples 3, 4, and 9 is relatively large, and the reason for the analysis is that the second additive is not added, and the decomposition and gas production problem of the first additive at high temperature cannot be effectively alleviated. In combination with Examples 5, 6, 11, 12 and Comparative Examples 1, 2, 8, and 10, it can be seen that when an appropriate amount of the second additive is added and used in combination with other additives, the high-temperature gas production problem of the battery can be effectively improved, the expansion rate of the high-temperature storage battery is significantly reduced, and the high-temperature cycle performance of the battery is improved. The high-temperature cycle DCR growth rate is relatively large in Comparative Examples 1, 2, and 8, and the reason for the analysis is that the first additive is not added. In Example 19, by further introducing a stabilizer (triphenyl phosphite), the storage shelf life of the electrolyte is greatly improved. The electrolyte in Example 5 has a shelf life of 30 days at 0°C-10°C, and the electrolyte in Example 18 has a shelf life of 60 days at 0°C-10°C. In addition, it can be seen from Examples 5, 12 and Comparative Examples 2, 4, etc. that the combination of the first additive, the second additive and the third additive is also conducive to obtaining a better improvement effect on the basis of a lower total dosage.Combining Example 1 and Comparative Examples 5-6, it can be seen that compared with tripropargyl phosphate and TMSP (tri(trimethylsilyl) phosphate) containing unsaturated bonds, trimethyl phosphate has a better effect on improving the high-temperature gas production problem, capacity attenuation problem and high-temperature cycle DCR growth rate of the battery. The reason for this may be that the unsaturated bonds of tripropargyl phosphate are rich in electrons and are not easy to break to form phosphorus free radicals and oxygen free radicals, and the phosphorus oxygen bond and the unsaturated bond are easy to conjugate, that is, tripropargyl phosphate is not easy to break bonds to form phosphorus free radicals and oxygen free radicals to consume the gas production of the first additive, while silicon oxygen in TMSP plays a dominant role and is not easy to break bonds. It mainly plays a role in removing water and suppressing acid. Relatively speaking, saturated phosphates are more likely to break bonds to form phosphorus free radicals and oxygen free radicals. Combining Example 1, Examples 4-5 and Examples 22-24, it can be seen that among the positive active materials, LiMn. 0.6 Fe 0.4 When the mass proportion of PO4 is relatively large, the performance of the battery will decline. The reason for this may be that when the content of lithium manganese iron phosphate is relatively large, manganese dissolution is relatively serious, resulting in a decline in battery performance. Combining Example 6 and Example 25, it can be seen that the use of the additive combination in the above embodiments of the present application in sodium ion batteries can also achieve the effect of good high temperature performance and less gas production, which shows that the additive combination in the above embodiments of the present application is not only applicable to lithium ion battery systems, but also to sodium ion battery systems.
[0110] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0111] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. An electrolyte, characterized in that: include: A first additive represented by formula I and a second additive represented by formula II, 、 , Wherein, R1, R2, and R3 are independently C 1-3 Alkyl, C 1-3 Any of the halogenated alkyl groups; Based on the total mass of the electrolyte, the mass percentage of the first additive in the electrolyte is 0.5% to 2%; the mass percentage of the second additive in the electrolyte is 0.1% to 2%.
2. The electrolyte according to claim 1, characterized in that R1, R2, and R3 are each independently a methyl group or a halogenated methyl group.
3. The electrolyte according to claim 1, characterized in that R1, R2 and R3 are all methyl groups.
4. The electrolyte according to any one of claims 1 to 3, characterized in that The mass ratio of the first additive to the second additive is 0.25-20.
5. The electrolyte according to claim 4, characterized in that Based on the total mass of the electrolyte, the mass percentage of the second additive in the electrolyte is 0.1% to 1%.
6. The electrolyte according to claim 1 or 5, characterized in that Also includes: a third additive shown in formula III, , R4 is any one of hydrogen, substituted or unsubstituted hydrocarbon group, and substituted or unsubstituted aromatic group, and n is a positive integer.
7. The electrolyte according to claim 6, characterized in that At least one of the following conditions is met: R4 is substituted or unsubstituted C 1-12 alkyl; n≥2。 8. The electrolyte according to claim 6, characterized in that The third additive includes hexamethylene diisocyanate.
9. The electrolyte according to claim 7 or 8, characterized in that The mass percentage of the third additive in the electrolyte is 0.01%-1%; and / or the mass ratio of the first additive to the third additive is 0.25-20.
10. The electrolyte according to claim 9, characterized in that The mass percentage of the third additive in the electrolyte is 0.01% to 0.2%.
11. The electrolyte according to claim 1 or 10, characterized in that: At least one of the following conditions is met: The electrolyte further comprises: a negative electrode film-forming additive; The electrolyte further comprises: a stabilizer; The electrolyte also includes: an organic solvent and a lithium salt.
12. The electrolyte according to claim 11, characterized in that Meet at least one of the following seven conditions: (i) the organic solvent comprises a carbonate solvent and / or a carboxylate solvent; (ii) the lithium salt comprises at least one of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate and lithium bis(trifluoromethanesulfonyl)imide; (iii) the molar concentration of the lithium salt in the electrolyte is 0.8 mol / L to 2 mol / L; (iv) the negative electrode film-forming additive includes at least one of vinylene carbonate, fluoroethylene carbonate, and vinyl ethylene carbonate; (v) based on the total mass of the electrolyte, the mass proportion of the negative electrode film-forming additive in the electrolyte is 0.5% to 2.0%; (vi) the stabilizer comprises at least one of triphenyl phosphite, triphenyl phosphate, pentafluoroethoxyphosphazene, and dicyclohexylcarbocyanide; (vii) Based on the total mass of the electrolyte, the mass percentage of the stabilizer in the electrolyte is 0.1% to 0.5%.
13. The electrolyte according to claim 12, characterized in that The organic solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate and butyl propionate.
14. The electrolyte according to claim 12, characterized in that The organic solvent comprises ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate in a mass ratio of 1:(0.5-2):(0.5-2).
15. The electrolyte according to claim 12, characterized in that The lithium salt is lithium bis(fluorosulfonyl)imide.
16. A battery, characterized in that: The invention comprises the electrolyte according to any one of claims 1 to 15.
17. The battery according to claim 16, characterized in that Also includes: Positive electrode active material, the battery is a lithium ion battery, and the positive electrode active material includes: Li a Ni b Co c M1 d M2 e O f R g and / or LiMn x Fe 1-x PO4, wherein 1≤a≤1.2, 0.5≤b≤1, 0≤c≤1, 0≤d≤1, 0≤e≤0.2, b+c+d+e=1, 1≤f≤2, 0≤g≤1, f+g=2; M1 includes Mn and / or Al, M2 includes at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, Sr, Sb, Y, W, Nb, and R includes at least one of N, F, S, and Cl; 0≤x≤1; and / or, The battery is a sodium ion battery, and the positive electrode active material includes Na α M3 β (X γ O δ ) θ (P2O7)μZ λ , wherein M3 includes a transition metal element, X includes at least one of P, S, Si, and W, Z includes at least one of N, F, S, and Cl, 1≤α≤10, 0<β≤5, 0≤γ≤10, 0≤δ≤10, 0≤θ≤5, 0≤μ≤5, and 0≤λ≤5.
18. An electrical device, characterized in that: A battery comprising the battery of claim 16 or 17.
Citation Information
Patent Citations
Lithium ion battery
CN115064770A
Secondary battery and device
CN116487706A
Electrolyte additive, electrolyte and battery
CN117577943A