A ceramic particle composite alloy steel swing hammer and preparation method thereof
Through the vacuum casting method and multi-layer structure design, the problem of unstable connection and material properties change of the composite metal hammer under high impact is solved, reliable filling of liquid metal and improvement of material properties are achieved, and the wear resistance of the hammer is enhanced. and shock absorption performance.
Patent Information
- Application Number
- CN202410510949.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-04-26
AI Technical Summary
In the existing technology, composite metal hammers are prone to falling off of prefabricated parts under high impact, and the multi-layer metal connections are unreliable, resulting in changes in material properties, and it is difficult for liquid metal to fully enter the pores of the prefabricated parts, causing air leakage or insufficient filling of the pores. question.
The porous ceramic prefabricated block is prepared by vacuum casting method. Liquid alloy is poured into the pores in a vacuum environment, combined with inert gas to promote metal penetration. Low-melting point high-density manganese-copper alloy is used as a shock-absorbing alloy to form a multi-layer structure to improve connection reliability and Material properties.
It realizes that liquid metal can reliably fill the pores of prefabricated parts in a vacuum environment, avoids air leakage, improves the reliability and material performance of multi-layer metal connections, and enhances the wear resistance and shock absorption performance of the hammer.
Smart Images

Figure CN118404037B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal casting, and in particular to a ceramic particle composite alloy steel swing hammer and a preparation method thereof. Background Art
[0002] Hammer crusher is a kind of equipment that crushes materials by impact, and it is divided into single rotor and double rotor types. It is a crusher that directly crushes materials with a maximum particle size of 600-1800 mm to 25 or less mm. Hammer crusher is suitable for medium and fine crushing of materials with medium hardness, such as limestone, slag, coke, coal, etc. in cement, chemical, electric power, metallurgy and other industrial sectors.
[0003] The advantages of hammer crusher are: large crushing ratio (generally 10-25, up to 50), high production capacity, uniform product, less over-powdering, low unit product energy consumption, simple structure, light equipment weight, easy operation and maintenance, etc. Hammer crusher series products are suitable for crushing various medium hardness and brittle materials, such as limestone, coal, salt, white ore, gypsum, alum, brick, tile, coal gangue, etc. The compressive strength of the crushed material does not exceed 150 MPa. The machine is mainly used in cement, coal preparation, power generation, building materials and compound fertilizer industries. It can crush raw materials of different sizes into uniform particles to facilitate the next process. The mechanical structure is reliable, the production efficiency is high, and the applicability is good.
[0004] The hammer is the most important working part of the hammer crusher. The quality, shape and material of the hammer determine the production capacity of the hammer crusher. The kinetic energy of the hammer is proportional to its weight. The heavier the hammer, the greater the kinetic energy and the higher the crushing efficiency. The hammer is often made of high-chromium manganese steel composite casting, and its service life is several times that of ordinary hammers.
[0005] How to manufacture high-performance hammer heads has always been a key research topic in this field. The related technologies are disclosed in the prior art:
[0006] The Chinese patent with the authorization announcement number CN104692803B discloses a method for preparing a wear-resistant composite material preform; specifically disclosed are: the steps are: (1) uniformly mixing ceramic particles with a binder and a lubricant; (2) placing the mixed material into a mold of a certain shape, and warm pressing to obtain a preform body in which ceramic particles are in contact with each other; (3) placing the preform body in a vacuum sintering furnace, evacuating to 10-100 Pa, slowly heating between 100-700°C, closing the vacuum valve, transferring to a protective atmosphere furnace, and continuing to heat to 1300-1600°C for curing and forming, to obtain a ceramic preform body for composite materials. Compared with the prior art, the present invention is simple and convenient to manufacture, has high production efficiency, can make the composite material achieve the expected wear resistance, and effectively prolongs the service life of the composite material.
[0007] The Chinese patent with the publication number CN115815599A discloses a method for preparing a ceramic particle reinforced alloy steel matrix composite material; specifically disclosed: including surface alloying pretreatment of ceramic particles, laying matrix alloy steel powder and pretreated ceramic particles layer by layer in a mold, and then pressurizing to obtain a prefabricated block, and hot pressing and sintering the prefabricated block, the sintering temperature is 10-20°C higher than the liquidus temperature of the matrix alloy steel powder, that is, the ceramic particle reinforced alloy steel matrix composite material is obtained. The present invention adopts layer by layer laying of ceramic particles and alloy steel powder and then vibrating and compacting, so that the ceramic particles can be evenly distributed in the matrix, and can give full play to the role of composite material particle reinforcement, and adopts a hot pressing sintering furnace to heat and melt the alloy powder under pressure, so that there is enough heat to make the alloy fluid, and there is enough pressure to make the alloy liquid penetrate into the ceramic gap to wrap the ceramic particles, thereby improving the bonding strength between the matrix and the ceramic particles. .
[0008] The Chinese patent with the announcement number CN210357383U discloses a metal-ceramic composite bimetallic swing hammer, which specifically discloses: a metal-cast hammer handle and a hammer head, one end of the hammer handle is connected to the hammer head, and the other end is used to connect to the swing hammer drive shaft of the crusher, and also includes a ceramic prefabricated block arranged on the end surface of the hammer head to increase the wear resistance of the hammer head. The metal-ceramic composite bimetallic swing hammer has good wear resistance and reduces the production cost.
[0009] However, the above prior art still has the following problems:
[0010] 1. The prior art discloses a composite metal swing hammer, but the composite metal swing hammer does not provide an effective solution to the problem of how to reliably connect the composite metal material with the porous preform. The composite metal swing hammer in the prior art is prone to the problem of preform falling off due to high impact during operation.
[0011] 2. The prior art discloses technical means for preparing composite metal hammer heads using layered materials, such as CN115815599A. However, no specific research has been conducted on how to reliably connect multiple layers of metal without excessive mixing. In actual use, the layers may be delaminated due to impact due to failure to reliably connect, or the properties of the metal materials may be changed due to excessive mixing.
[0012] 3. The casting of preforms in the prior art is usually carried out in air, and the liquid metal has surface tension and is difficult to fully enter the pores of the preform; or when it is carried out in a vacuum, it is difficult to control the direction of the metal entering the pores, resulting in air leakage in the pores and failure to fully fill them. Summary of the invention
[0013] To achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: a method for preparing a ceramic particle composite alloy steel hammer, comprising the following steps:
[0014] S1, preparing a porous ceramic prefabricated block; preparing ceramic particles of predetermined specifications and mixing them with a binder, and preparing a porous ceramic prefabricated block through pre-pressing, drying and sintering; the porous ceramic prefabricated block is a rectangular hexahedron, and one of the rectangular planes of the rectangular hexahedron is a main wear-resistant plane;
[0015] S2, vacuum casting a high damping alloy; casting the liquid first alloy into the pores of the porous ceramic prefabricated block by a vacuum casting method, and solidifying to obtain a high damping ceramic-alloy prefabricated block;
[0016] S3, casting the wear-resistant base plate; fixing the high damping ceramic-alloy prefabricated block in the casting mold, pouring a predetermined amount of liquid second alloy, cooling and solidifying to obtain the wear-resistant base plate;
[0017] S4, casting a damping and vibration-slowing layer; when the wear-resistant base plate is cooled to a predetermined temperature, pouring a predetermined amount of liquid first alloy into it, cooling and solidifying it to obtain the damping and vibration-slowing layer;
[0018] S5, casting the vibration isolation layer; when the damping and vibration absorbing layer is cooled to a predetermined temperature, pouring a predetermined amount of liquid second alloy, cooling and solidifying to obtain the damping and vibration isolation layer;
[0019] S6, cyclically casting a damping and vibration-slowing layer-vibration-isolating layer composite structure; as needed, repeatedly performing steps S4 and S5 to obtain a damping and vibration-slowing layer-vibration-isolating layer composite structure;
[0020] S7, casting the hammer body; closing the upper mold of the casting mold, pouring a predetermined amount of liquid second alloy until the pouring riser overflows, and after the mold is cooled and solidified to a predetermined temperature, demolding and removing the casting flash to obtain a ceramic particle composite alloy steel hammer;
[0021] S8. Local heat treatment: quenching and low-temperature tempering treatment is performed on the wear-resistant base plate of the swing hammer and the connecting hole of the hammer head.
[0022] Furthermore, step S1 specifically includes:
[0023] S11, preparing porous ceramic prefabricated block aggregate; preparing ceramic particles of predetermined specifications and a certain proportion of a binder, rotating and stirring to mix them evenly, to obtain porous ceramic prefabricated block aggregate; the binder is sodium silicate and industrial syrup;
[0024] S12, preparing a porous ceramic prefabricated block blank by molding; pouring the porous ceramic prefabricated block aggregate into a prefabricated block mold, applying a predetermined pressure to the upper cover of the prefabricated block mold by a hydraulic press, and after a predetermined holding time, releasing the pressure and demolding to obtain a pre-tightened porous ceramic prefabricated block blank;
[0025] S13, drying and sintering; placing the pre-tightened porous ceramic prefabricated block blank into a sintering furnace for drying and sintering to obtain a porous ceramic prefabricated block.
[0026] Furthermore, in step S2, the first alloy is a manganese-copper alloy, which, based on the total mass percentage being 100%, includes the following components in mass percentage: Cu: 15-35%; Cr: 2-6%; Ni: 2-5%; C: ≤0.02%; Si: ≤0.04%; S: ≤0.05%; P: ≤0.008%; and the remainder is manganese and unavoidable impurities.
[0027] Furthermore, step S2 specifically includes:
[0028] The porous ceramic prefabricated block is placed in a vacuum casting mold, a predetermined amount of liquid first alloy is poured into it, and after vibrating and exhausting the air and evacuating the air again, an inert gas is introduced into the vacuum casting mold, so that the liquid first alloy is filled into the pores of the porous ceramic prefabricated block under the action of external air pressure, and the following conditions are met:
[0029] V2>V1·ρ·K
[0030] Wherein, V2 represents the volume of the poured liquid first metal; V1 represents the volume of the circumscribed rectangle of the porous ceramic preform; ρ represents the porosity of the porous ceramic preform; K represents the filling rate of the first alloy to the pores of the porous ceramic preform, 0 <K<80%。
[0031] Furthermore, in step S2, the vacuum casting mold is a rectangular hexahedron, and the rectangle of the vacuum casting mold horizontally projected downward is similar to the rectangle of the porous ceramic prefabricated block horizontally projected downward, satisfying:
[0032] L1:L2=l1:l2
[0033] L1 / l1=L2 / l2=c
[0034] Among them, L1 and L2 are the length and width of the rectangle of the downward horizontal projection of the vacuum casting mold; l1 and l2 are the length and width of the rectangle of the downward horizontal projection of the porous ceramic prefabricated block; c is a small constant greater than 1 to ensure that the porous ceramic prefabricated block can be placed in the vacuum casting mold without shaking.
[0035] Furthermore, in step S2, after pouring the liquid second alloy and before introducing the inert gas, the liquid second alloy infiltrates downward into the pores of the porous ceramic prefabricated block by gravity; the inert gas is introduced from above the liquid surface of the liquid second alloy, and a downward gas pressure is applied to cause the liquid second alloy to infiltrate the pores of the porous ceramic prefabricated block, and after the infiltration is completed, the upper surface of the porous ceramic prefabricated block is higher than the upper surface of the second alloy, satisfying:
[0036] (V2-V1·ρ·K) / (L1·L2-l1·l2) <h
[0037] Wherein, h is the height of the porous ceramic prefabricated block with the main wear-resistant plane as the bottom.
[0038] Furthermore, the second alloy is nickel-free alloy steel 40CrMnSiMoV, or alloy steel 50Cr, or alloy steel 35CrMo, or alloy steel NM360, or alloy steel NM400, or alloy steel NM450, or alloy steel NM500, or alloy steel NM550, or alloy steel NM600.
[0039] Furthermore, the second alloy is a nickel-free alloy steel 40CrMnSiMoV, satisfying the following weight percentages: C: 0.36-0.40%; Si: 1.20-1.60%; Mn: 0.80-1.20%; S: ≤0.020%; P: ≤0.020%; Cr: 1.20-1.50%; V: 0.07-0.12%; Mo: 0.45-0.60%, and the rest is Fe.
[0040] Furthermore, the melting point of the first alloy is lower than that of the second alloy, and when the liquid second alloy contacts the solid first alloy, the solid first alloy is at least partially melted to form a non-planar interface fusion region with the second alloy; and the density of the first alloy is higher than that of the second alloy, and at least the partially melted first alloy is located below the liquid second alloy without being completely mixed.
[0041] The present invention also discloses a ceramic particle composite alloy steel hammer, which includes: a high-damping ceramic-alloy prefabricated block; the high-damping ceramic-alloy prefabricated block includes a porous ceramic prefabricated block and a first alloy cast into the pores of the porous ceramic prefabricated block; the porous ceramic prefabricated block is a rectangular hexahedron, and one of the rectangular planes of the porous ceramic prefabricated block is a main wear-resistant plane; a wear-resistant base plate; the wear-resistant base plate is cast from a second alloy; a damping and vibration-absorbing layer; the damping and vibration-absorbing layer is cast from a first alloy; a vibration isolation layer; the vibration isolation layer is cast from a second alloy; a hammer body; the hammer body is cast from the second alloy.
[0042] Furthermore, the first alloy is a manganese-copper alloy, which, based on the total mass percentage being 100%, satisfies the following mass percentage components: Cu: 15-35%; Cr: 2-6%; Ni: 2-5%; C: ≤0.02%; Si: ≤0.04%; S: ≤0.05%; P: ≤0.008%; and the remainder is manganese and unavoidable impurities.
[0043] Furthermore, the second alloy is nickel-free alloy steel 40CrMnSiMoV, or alloy steel 50Cr, or alloy steel 35CrMo, or alloy steel NM360, or alloy steel NM400, or alloy steel NM450, or alloy steel NM500, or alloy steel NM550, or alloy steel NM600.
[0044] Further, the second alloy is a nickel-free alloy steel 40CrMnSiMoV, satisfying the following weight percentages: C: 0.36-0.40%; Si: 1.20-1.60%; Mn: 0.80-1.20%; S: ≤0.020%; P: ≤0.020%; Cr: 1.20-1.50%; V: 0.07-0.12%; Mo: 0.45-0.60%, and the rest is Fe.
[0045] The beneficial effects of the present invention are:
[0046] 1. The present invention utilizes a vacuum casting method to place the liquid damping alloy on the upper part of the preform under a vacuum environment. After the inert gas is introduced, the liquid metal is squeezed downward into the pores of the preform, thereby avoiding the problem of air leakage of the preform.
[0047] 2. The present invention utilizes a vacuum casting method and adopts a casting mold slightly larger than the preform, so that the cast metal is mainly distributed in and above the pores of the preform, with only a small amount of shock-absorbing alloy around it, and the melting point of the shock-absorbing alloy is lower than that of the wear-resistant alloy. When casting the wear-resistant alloy, the shock-absorbing alloy around it can be melted in a small amount to form a fusion transition layer with the liquid wear-resistant alloy, thereby improving the connection reliability; at the same time, since the preform blocks heat transfer, the amount of shock-absorbing alloy melted inside the preform is small, and the shock-absorbing alloy around it will not be too much and mixed with the wear-resistant alloy, thereby affecting the material properties of the wear-resistant alloy.
[0048] 3. The present invention adopts a low-melting-point, high-density manganese-copper alloy as a shock-absorbing alloy. After it solidifies, a high-melting-point, low-density alloy steel is poured in. Even if the manganese-copper alloy melts, it will sink to the lower layer of the liquid alloy steel and will not undergo convection fusion due to gravity. When the alloy steel is slightly cooled and solidified, the next layer of manganese-copper alloy is cast. Since the melting point of the manganese-copper alloy is lower, the alloy steel layer will not be over-melted and excessive convection fusion will not occur. In the case of a small amount of fusion and no excessive fusion, the connection reliability is guaranteed and the material properties are avoided from being affected.
[0049] 4. The present invention adopts a manganese-copper alloy with good shock absorption as the damping layer, and uses a highly rigid alloy steel as the raft layer, forming a structure similar to a rigid plate "floating" above the damping layer, so that after the shock wave is weakened in the damping layer, when it "collides" with the raft layer, it is not easy to penetrate and is rebounded and dissipated. Compared with the solution of using a single damping alloy with the same total volume, it has better shock absorption performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 It is a schematic diagram of the overall method flow of the present invention.
[0051] Figure 2 It is a schematic diagram of the structure of the ceramic particle composite alloy steel swing hammer of the present invention. DETAILED DESCRIPTION
[0052] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0053] Embodiment 1
[0054] According to the attached picture Figure 1 As shown, a method for preparing a ceramic particle composite alloy steel hammer comprises the following steps:
[0055] S1, preparing a porous ceramic prefabricated block; preparing ceramic particles of predetermined specifications and mixing them with a binder, and preparing a porous ceramic prefabricated block through pre-pressing, drying and sintering; the porous ceramic prefabricated block is a rectangular hexahedron, and one of the rectangular planes of the rectangular hexahedron is a main wear-resistant plane;
[0056] S2, vacuum casting a high damping alloy; casting the liquid first alloy into the pores of the porous ceramic prefabricated block by a vacuum casting method, and solidifying to obtain a high damping ceramic-alloy prefabricated block;
[0057] S3, casting the wear-resistant base plate; fixing the high damping ceramic-alloy prefabricated block in the casting mold, pouring a predetermined amount of liquid second alloy, cooling and solidifying to obtain the wear-resistant base plate;
[0058] S4, casting a damping and vibration-slowing layer; when the wear-resistant base plate is cooled to a predetermined temperature, pouring a predetermined amount of liquid first alloy into it, cooling and solidifying it to obtain the damping and vibration-slowing layer;
[0059] S5, casting the vibration isolation layer; when the damping and vibration absorbing layer is cooled to a predetermined temperature, pouring a predetermined amount of liquid second alloy, cooling and solidifying to obtain the damping and vibration isolation layer;
[0060] S6, cyclically casting a damping and vibration-slowing layer-vibration-isolating layer composite structure; as needed, repeatedly performing steps S4 and S5 to obtain a damping and vibration-slowing layer-vibration-isolating layer composite structure;
[0061] S7, casting the hammer body; closing the upper mold of the casting mold, pouring a predetermined amount of liquid second alloy until the pouring riser overflows, and after the mold is cooled and solidified to a predetermined temperature, demolding and removing the casting flash to obtain a ceramic particle composite alloy steel hammer;
[0062] S8. Local heat treatment: quenching and low-temperature tempering treatment is performed on the wear-resistant base plate of the swing hammer and the connecting hole of the hammer head.
[0063] Further, step S1 specifically includes: S11, preparing porous ceramic prefabricated block aggregate; preparing ceramic particles of predetermined specifications and a certain proportion of a binder, and rotating and stirring to mix them evenly to obtain porous ceramic prefabricated block aggregate; the binder is sodium silicate and industrial syrup;
[0064] S12, preparing a porous ceramic prefabricated block blank by molding; pouring the porous ceramic prefabricated block aggregate into a prefabricated block mold, applying a predetermined pressure to the upper cover of the prefabricated block mold by a hydraulic press, and after a predetermined holding time, releasing the pressure and demolding to obtain a pre-tightened porous ceramic prefabricated block blank;
[0065] S13, drying and sintering; placing the pre-tightened porous ceramic prefabricated block blank into a sintering furnace for drying and sintering to obtain a porous ceramic prefabricated block.
[0066] Furthermore, in step S2, the first alloy is a manganese-copper alloy, which, based on the total mass percentage being 100%, includes the following components in mass percentage: Cu: 15-35%; Cr: 2-6%; Ni: 2-5%; C: ≤0.02%; Si: ≤0.04%; S: ≤0.05%; P: ≤0.008%; and the remainder is manganese and unavoidable impurities.
[0067] Further, step S2 specifically includes: placing the porous ceramic prefabricated block into a vacuum casting mold, pouring a predetermined amount of liquid first alloy, vibrating and exhausting and evacuating again, and then introducing inert gas into the vacuum casting mold, so that the liquid first alloy is filled into the pores of the porous ceramic prefabricated block under the action of external air pressure, and satisfying:
[0068] V2>V1·ρ·K
[0069] Wherein, V2 represents the volume of the poured liquid first metal; V1 represents the volume of the circumscribed rectangle of the porous ceramic preform; ρ represents the porosity of the porous ceramic preform; K represents the filling rate of the first alloy to the pores of the porous ceramic preform, 0 <K<80%。
[0070] Furthermore, in step S2, the vacuum casting mold is a rectangular hexahedron, and the rectangle of the vacuum casting mold horizontally projected downward is similar to the rectangle of the porous ceramic prefabricated block horizontally projected downward, satisfying:
[0071] L1:L2=l1:l2
[0072] L1 / l1=L2 / l2=c
[0073] Among them, L1 and L2 are the length and width of the rectangle of the downward horizontal projection of the vacuum casting mold; l1 and l2 are the length and width of the rectangle of the downward horizontal projection of the porous ceramic prefabricated block; c is a small constant greater than 1 to ensure that the porous ceramic prefabricated block can be placed in the vacuum casting mold without shaking.
[0074] Furthermore, in step S2, after pouring the liquid second alloy and before introducing the inert gas, the liquid second alloy infiltrates downward into the pores of the porous ceramic prefabricated block by gravity; the inert gas is introduced from above the liquid surface of the liquid second alloy, and a downward gas pressure is applied to cause the liquid second alloy to infiltrate the pores of the porous ceramic prefabricated block, and after the infiltration is completed, the upper surface of the porous ceramic prefabricated block is higher than the upper surface of the second alloy, satisfying:
[0075] (V2-V1·ρ·K) / (L1·L2-l1·l2) <h
[0076] Wherein, h is the height of the porous ceramic prefabricated block with the main wear-resistant plane as the bottom.
[0077] Furthermore, the second alloy is nickel-free alloy steel 40CrMnSiMoV, or alloy steel 50Cr, or alloy steel 35CrMo, or alloy steel NM360, or alloy steel NM400, or alloy steel NM450, or alloy steel NM500, or alloy steel NM550, or alloy steel NM600.
[0078] Furthermore, the second alloy is a nickel-free alloy steel 40CrMnSiMoV, satisfying the following weight percentages: C: 0.36-0.40%; Si: 1.20-1.60%; Mn: 0.80-1.20%; S: ≤0.020%; P: ≤0.020%; Cr: 1.20-1.50%; V: 0.07-0.12%; Mo: 0.45-0.60%, and the rest is Fe.
[0079] Furthermore, the melting point of the first alloy is lower than that of the second alloy, and when the liquid second alloy contacts the solid first alloy, the solid first alloy is at least partially melted to form a non-planar interface fusion region with the second alloy; and the density of the first alloy is higher than that of the second alloy, and at least the partially melted first alloy is located below the liquid second alloy without being completely mixed.
[0080] Embodiment 2
[0081] According to the attached picture Figure 2 As shown, the present invention discloses a ceramic particle composite alloy steel hammer, which includes: a high-damping ceramic-alloy prefabricated block; the high-damping ceramic-alloy prefabricated block includes a porous ceramic prefabricated block and a first alloy cast into the pores of the porous ceramic prefabricated block; the porous ceramic prefabricated block is a rectangular hexahedron, and one of the rectangular planes of the porous ceramic prefabricated block is a main wear-resistant plane; a wear-resistant bottom plate; the wear-resistant bottom plate is cast by a second alloy; a damping and vibration-absorbing layer; the damping and vibration-absorbing layer is cast by a first alloy; a vibration isolation layer; the vibration isolation layer is cast by a second alloy; a hammer body; the hammer body is cast by the second alloy.
[0082] Furthermore, the first alloy is a manganese-copper alloy, which, based on the total mass percentage being 100%, satisfies the following mass percentage components: Cu: 15-35%; Cr: 2-6%; Ni: 2-5%; C: ≤0.02%; Si: ≤0.04%; S: ≤0.05%; P: ≤0.008%; and the remainder is manganese and unavoidable impurities.
[0083] Furthermore, the second alloy is nickel-free alloy steel 40CrMnSiMoV, or alloy steel 50Cr, or alloy steel 35CrMo, or alloy steel NM360, or alloy steel NM400, or alloy steel NM450, or alloy steel NM500, or alloy steel NM550, or alloy steel NM600.
[0084] Furthermore, the second alloy is a nickel-free alloy steel 40CrMnSiMoV, satisfying the following weight percentages: C: 0.36-0.40%; Si: 1.20-1.60%; Mn: 0.80-1.20%; S: ≤0.020%; P: ≤0.020%; Cr: 1.20-1.50%; V: 0.07-0.12%; Mo: 0.45-0.60%, and the rest is Fe.
[0085] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a ceramic particle composite alloy steel swing hammer, characterized in that: The following steps are involved: S1, preparing a porous ceramic prefabricated block; preparing ceramic particles of predetermined specifications and mixing them with a binder, and preparing a porous ceramic prefabricated block through pre-pressing, drying and sintering; the porous ceramic prefabricated block is a rectangular hexahedron, and one of the rectangular planes of the rectangular hexahedron is a main wear-resistant plane; S2, vacuum casting a high damping alloy; casting the liquid first alloy into the pores of the porous ceramic prefabricated block by a vacuum casting method, and solidifying to obtain a high damping ceramic-alloy prefabricated block; S3, casting the wear-resistant base plate; fixing the high damping ceramic-alloy prefabricated block in the casting mold, pouring a predetermined amount of liquid second alloy, cooling and solidifying to obtain the wear-resistant base plate; S4, casting a damping and vibration-slowing layer; when the wear-resistant base plate is cooled to a predetermined temperature, pouring a predetermined amount of liquid first alloy into it, cooling and solidifying it to obtain the damping and vibration-slowing layer; S5, casting the vibration isolation layer; when the damping and vibration absorbing layer is cooled to a predetermined temperature, pouring a predetermined amount of liquid second alloy, cooling and solidifying to obtain the damping and vibration isolation layer; S6, cyclically casting a damping and vibration-slowing layer-vibration-isolating layer composite structure; as needed, repeatedly performing steps S4 and S5 to obtain a damping and vibration-slowing layer-vibration-isolating layer composite structure; S7, casting the hammer body; closing the upper mold of the casting mold, pouring a predetermined amount of liquid second alloy until the pouring riser overflows, and after the mold is cooled and solidified to a predetermined temperature, demolding and removing the casting flash to obtain a ceramic particle composite alloy steel hammer; S8. Local heat treatment: quenching and low-temperature tempering treatment is performed on the wear-resistant base plate of the swing hammer and the connecting hole of the hammer head.
2. The method for preparing a ceramic particle composite alloy steel swing hammer according to claim 1, characterized in that: Step S1 specifically includes: S11, preparing porous ceramic prefabricated block aggregate; preparing ceramic particles of predetermined specifications and a certain proportion of a binder, rotating and stirring to mix them evenly, to obtain porous ceramic prefabricated block aggregate; the binder is sodium silicate and industrial syrup; S12, preparing a porous ceramic prefabricated block blank by molding; pouring the porous ceramic prefabricated block aggregate into a prefabricated block mold, applying a predetermined pressure to the upper cover of the prefabricated block mold by a hydraulic press, and after a predetermined holding time, releasing the pressure and demolding to obtain a pre-tightened porous ceramic prefabricated block blank; S13, drying and sintering; placing the pre-tightened porous ceramic prefabricated block blank into a sintering furnace for drying and sintering to obtain a porous ceramic prefabricated block.
3. The method for preparing a ceramic particle composite alloy steel swing hammer according to claim 1, characterized in that: In step S2, the first alloy is a manganese-copper alloy, which, based on the total mass percentage being 100%, includes the following components in mass percentage: Cu: 15-35%; Cr: 2-6%; Ni: 2-5%; C: ≤0.02%; Si: ≤0.04%; S: ≤0.05%; P: ≤0.008%; the remainder being manganese and unavoidable impurities.
4. The method for preparing a ceramic particle composite alloy steel swing hammer according to claim 3, characterized in that: Step S2 specifically includes: The porous ceramic prefabricated block is placed in a vacuum casting mold, a predetermined amount of liquid first alloy is poured into it, and after vibrating and exhausting the air and evacuating the air again, an inert gas is introduced into the vacuum casting mold, so that the liquid first alloy is filled into the pores of the porous ceramic prefabricated block under the action of external air pressure, and the following conditions are met: V2>V1·ρ·K Wherein, V2 represents the volume of the poured liquid first metal; V1 represents the volume of the circumscribed rectangle of the porous ceramic preform; ρ represents the porosity of the porous ceramic preform; K represents the filling rate of the first alloy to the pores of the porous ceramic preform, 0 <K<80%。 5. The method for preparing a ceramic particle composite alloy steel swing hammer according to claim 4, characterized in that: In step S2, the vacuum casting mold is a rectangular hexahedron, and the rectangle of the vacuum casting mold horizontally projected downward is similar to the rectangle of the porous ceramic prefabricated block horizontally projected downward, satisfying: L1:L2=l1:l2 L1 / l1=L2 / l2=c Among them, L1 and L2 are the length and width of the rectangle of the downward horizontal projection of the vacuum casting mold; l1 and l2 are the length and width of the rectangle of the downward horizontal projection of the porous ceramic prefabricated block; c is a small constant greater than 1 to ensure that the porous ceramic prefabricated block can be placed in the vacuum casting mold without shaking.
6. The method for preparing a ceramic particle composite alloy steel swing hammer according to claim 5, characterized in that: In step S2, after pouring the liquid second alloy and before introducing the inert gas, the liquid second alloy infiltrates downward into the pores of the porous ceramic prefabricated block by gravity; the inert gas is introduced from above the liquid surface of the liquid second alloy, and the downward gas pressure is applied to cause the liquid second alloy to infiltrate the pores of the porous ceramic prefabricated block, and after the infiltration is completed, the upper surface of the porous ceramic prefabricated block is higher than the upper surface of the second alloy, satisfying: (V2-V1·ρ·K) / (L1·L2-l1·l2) <h Wherein, h is the height of the porous ceramic prefabricated block with the main wear-resistant plane as the bottom.
7. The method for preparing a ceramic particle composite alloy steel swing hammer according to claim 5, characterized in that: The second alloy is nickel-free alloy steel 40CrMnSiMoV, or alloy steel 50Cr, or alloy steel 35CrMo, or alloy steel NM360, or alloy steel NM400, or alloy steel NM450, or alloy steel NM500, or alloy steel NM550, or alloy steel NM600.
8. The method for preparing a ceramic particle composite alloy steel swing hammer according to claim 7, characterized in that: The melting point of the first alloy is lower than that of the second alloy. When the liquid second alloy contacts the solid first alloy, the solid first alloy is at least partially melted to form a non-planar interface fusion region with the second alloy. The density of the first alloy is higher than that of the second alloy. The at least partially melted first alloy is located below the liquid second alloy without being completely mixed.
9. A ceramic particle composite alloy steel swing hammer, characterized in that: The ceramic particle composite alloy steel swing hammer comprises: A high damping ceramic-alloy prefabricated block; the high damping ceramic-alloy prefabricated block comprises a porous ceramic prefabricated block and a first alloy cast into the pores of the porous ceramic prefabricated block; the porous ceramic prefabricated block is a rectangular hexahedron, and one of the rectangular planes of the porous ceramic prefabricated block is a main wear-resistant plane; Wear-resistant base plate; the wear-resistant base plate is cast from the second alloy; Damping and vibration absorbing layer; the damping and vibration absorbing layer is cast by the first alloy; A vibration isolation layer; the vibration isolation layer is cast from the second alloy; The swing hammer body is cast from the second alloy.
10. The ceramic particle composite alloy steel swing hammer according to claim 9, characterized in that: The first alloy is a manganese-copper alloy, which satisfies the following mass percentages based on the total mass percentage of 100%: Cu: 15-35%; Cr: 2-6%; Ni: 2-5%; C: ≤0.02%; Si: ≤0.04%; S: ≤0.05%; P: ≤0.008%; the remainder is manganese and unavoidable impurities; The second alloy is nickel-free alloy steel 40CrMnSiMoV, or alloy steel 50Cr, or alloy steel 35CrMo, or alloy steel NM360, or alloy steel NM400, or alloy steel NM450, or alloy steel NM500, or alloy steel NM550, or alloy steel NM600.