A filler for electronic packaging and preparation method thereof and application in epoxy molding compound

Through spherical alumina composite of different particle sizes and benzene-containing silane modification treatment, the thermal conductivity and fluidity of epoxy plastic sealing materials are improved, the poor thermal conductivity and warping problems in the prior art are solved, and higher electronic packaging is achieved performance.

CN118440624BActive Publication Date: 2024-11-29HUANGPU INST OF MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410581730.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-11-29
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

The existing thermally conductive epoxy plastic seals have poor thermal conductivity, fluidity, mechanical properties and temperature resistance in electronic packaging, resulting in low warpage and reliability, making it difficult to meet high performance needs.

Method used

The spherical alumina composite with different particle sizes is used to form a three-dimensional network structure with efficient heat conduction, and the benzene-containing silane with bifunctional groups is used as a modifier to improve the pore state of the spherical alumina and the compatibility of the epoxy resin and improve heat conduction. coefficients, fluidity and mechanical properties.

Benefits of technology

It significantly improves the thermal conductivity, fluidity and mechanical properties of epoxy plastic seals for electronic packaging, reduces warpage, and meets the needs of high-performance electronic packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004834234820000021
    Figure BDA0004834234820000021
  • Figure BDA0004834234820000031
    Figure BDA0004834234820000031
  • Figure BDA0004834234820000051
    Figure BDA0004834234820000051
Patent Text Reader

Abstract

The present disclosure provides a filler for electronic packaging and a preparation method thereof and its application in epoxy molding compound, belonging to the field of electronic packaging. The filler for electronic packaging disclosed in the present disclosure includes spherical alumina with different particle sizes and phenyl silane, and the spherical alumina with different particle sizes is compounded to form a three-dimensional network structure with high efficiency and heat conduction. The phenyl silane with a bifunctional group is used as a modifier to modify the spherical alumina, so that the surface of the modified spherical alumina is more compact and smooth; the compatibility of the modified spherical alumina and epoxy resin is improved, thereby improving the thermal conductivity, fluidity, and mechanical properties of the epoxy molding compound for electronic packaging and reducing the warping of the epoxy molding compound for electronic packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of electronic packaging, and in particular to a filler for electronic packaging, a preparation method thereof, and an application of the filler in an epoxy molding compound. Background Art

[0002] In modern society, as people's requirements for electronic devices are increasing, better performance, better portability, etc., the performance requirements for materials are also increasing accordingly. To meet these needs, the integration of chips has increased rapidly, which has led to a significant increase in heat generation; the internal layout of electronic products has become more dense and smaller, which makes heat dissipation more difficult. If this problem is not solved, it will cause electronic products to overheat or even fail. To solve this problem, thermally conductive packaging materials quickly transfer this part of the heat to the outside world, reduce the temperature of the product, thereby protecting the product from damage and ensuring efficient operation.

[0003] Epoxy resin compositions are widely used in the electronic packaging industry. In recent years, due to their excellent adhesion, weather resistance, high body strength, and superior construction performance, they have been increasingly used in more sophisticated component packaging, especially chip packaging. Among them, epoxy molding compound is one of the most widely used and largest types. Its components include epoxy resin, curing agent, inorganic filler, curing accelerator, and various additives. Among them, fillers account for the largest mass fraction of epoxy molding compound components, and have a greater impact on epoxy molding compound, especially thermal conductivity, which almost entirely depends on factors such as the type and amount of fillers.

[0004] In order to achieve a higher thermal conductivity, a large amount of thermal conductive filler needs to be added to meet the requirements. The most commonly used filler is spherical alumina. However, compared with traditional epoxy molding compound fillers, these powders have poor surface properties, strong hygroscopicity, and poor epoxy compatibility. As a result, high thermal conductivity epoxy molding compound products often have defects such as poor temperature resistance, poor density, low mechanical strength, poor fluidity, and low addition amount. The performance is low and it is difficult to meet the needs of customers. It is easy to cause stress cracking, warping, and poor reliability. Poor fluidity will make it difficult to implement the process, and defects such as flash and voids will appear. This is the biggest difficulty facing thermal conductive epoxy molding compounds at this stage. Summary of the invention

[0005] The purpose of the present disclosure is to overcome the deficiencies of the prior art and provide a filler for electronic packaging and a preparation method thereof and its application in epoxy molding compound. The filler for electronic packaging can significantly increase the thermal conductivity, fluidity, and mechanical properties of the epoxy molding compound for electronic packaging and reduce the warpage of the epoxy molding compound for electronic packaging.

[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present disclosure is as follows: in a first aspect, a filler for electronic packaging is provided, including spherical alumina and phenyl-containing silane;

[0007] Based on 100 parts by mass of spherical alumina, the spherical alumina includes 0.1-50 parts of large-particle spherical alumina, 0.1-70 parts of medium-particle spherical alumina and 0.1-20 parts of small-particle spherical alumina, the average particle size of the small-particle spherical alumina is ≤1 μm, the average particle size of the medium-particle spherical alumina is 1-10 μm, and the average particle size of the large-particle spherical alumina is >10 μm;

[0008] The structural formula of the phenylsilane-containing compound is:

[0009]

[0010] Wherein, n is an integer from 0 to 16.

[0011] In the present invention, on the one hand, spherical alumina with different particle sizes are compounded to form a three-dimensional network structure with high efficiency and thermal conductivity. On the other hand, a bifunctional phenyl-containing silane is used as a modifier to modify the spherical alumina. The alkoxy groups on the phenyl-containing silane can combine with hydrogen bonds on the surface of the spherical alumina to improve the loose pore state of the spherical alumina, making the surface of the modified spherical alumina denser and smoother; the compatibility between the modified spherical alumina and epoxy resin is improved, thereby improving the thermal conductivity, fluidity, and mechanical properties of the epoxy molding compound for electronic packaging and reducing the warping of the epoxy molding compound for electronic packaging.

[0012] Specifically, as specific examples of the phenyl-containing silane, there can be mentioned 1,4-bis(triethoxysilane)benzene, 1,4-bis(tripropoxysilane)benzene, and 1,4-bis(trihexyloxysilane)benzene.

[0013] In one embodiment, the phenyl-containing silane is 1,4-bis(triethoxysilane)benzene and 1,4-bis(tripropoxysilane)benzene.

[0014] In the present disclosure, when the phenyl-containing silane is 1,4-bis(triethoxysilane)benzene and 1,4-bis(tripropoxysilane)benzene, the overall performance of the epoxy molding compound for electronic packaging can be further improved.

[0015] In one embodiment, the mass of the phenylsilane-containing material is 0.1-1% of the mass of the spherical alumina, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1%, but is not limited to the listed values, and other values ​​within this range are also applicable.

[0016] If the mass of phenylsilane is too little, the modification degree of spherical alumina is small, and the overall performance of the epoxy molding compound for electronic packaging cannot be effectively improved; if the mass of phenylsilane is too much, the overall performance of the epoxy molding compound for electronic packaging is not significantly improved.

[0017] In one embodiment, the preparation method of the phenyl-containing silane is: 1,4-bis(trichlorosilane)benzene and lithium aluminum hydride are subjected to a first reaction to obtain phenylene disilane, and then phenylene disilane and alcohol are subjected to a second reaction to obtain the phenyl-containing silane, wherein the number of carbon atoms of the alcohol is 2-17.

[0018] In the present disclosure, the reaction equation containing phenylsilane is:

[0019]

[0020] Wherein, n is an integer from 0 to 16.

[0021] Specifically, the specific preparation steps of phenylene disilane are:

[0022] At a temperature of 10-20°C, 1,4-di(trichlorosilane)benzene is added dropwise to an ether solution of lithium aluminum hydride. After the addition is completed, the reaction is refluxed at a temperature of 35-40°C for 2-3 hours. The reaction product is extracted with petroleum ether and ether in turn, and the extracted product is washed with a hydrochloric acid aqueous solution for 4-6 times to obtain terephthalene disilane.

[0023] Specifically, the specific preparation steps of phenylsilane are:

[0024] After mixing phenylene disilane and alcohol, reflux reaction is carried out at a temperature of 60-90°C and under alkaline conditions for 2-3 hours. The reaction product is washed and distilled under reduced pressure to obtain phenyl-containing silane; wherein the carbon number of the alcohol is 2-17.

[0025] In a second aspect, a method for preparing the filler for electronic packaging is provided, comprising the following steps:

[0026] The spherical alumina is added into a solvent and mixed evenly to obtain a spherical alumina dispersion, and then phenylsilane is added to obtain a filler for electronic packaging, wherein the mass of the phenylsilane is 0.1-1% of the mass of the spherical alumina.

[0027] Specifically, the solvent is a mixture of water and ethanol.

[0028] In the present disclosure, a wet treatment method is adopted and phenyl silane is used as a modifier to modify the spherical alumina. The alkoxy group on the phenyl silane can combine with the hydrogen bonds on the surface of the spherical alumina, thereby improving the loose pore state of the spherical alumina and making the surface of the modified spherical alumina denser and smoother; the compatibility between the modified spherical alumina and epoxy resin is improved, thereby improving the thermal conductivity, fluidity, and mechanical properties of the epoxy molding compound for electronic packaging and reducing the warping of the epoxy molding compound for electronic packaging.

[0029] In a third aspect, the invention provides application of the filler for electronic packaging in epoxy molding compound for electronic packaging.

[0030] In a fourth aspect, an epoxy molding compound for electronic packaging is provided, comprising the following components in parts by weight: 2-10 parts of epoxy resin, 2-10 parts of curing agent, 0.01-0.5 parts of curing accelerator, 1-3 parts of low stress modifier, 70-90 parts of thermal conductive filler, 0.01-1 parts of release agent, 0.01-1 parts of pigment, and 0.1-2 parts of flame retardant; the thermal conductive filler is the filler for electronic packaging.

[0031] In one embodiment, the epoxy resin contains at least two epoxy groups; specific examples of epoxy resins include: o-cresol epoxy resin, polyaromatic epoxy resin, biphenyl epoxy resin, biphenyl aralkyl type epoxy resin, dicyclopentadiene type epoxy resin, naphthalene epoxy resin, bisphenol A type epoxy resin, etc. From the perspective of general versatility, the present disclosure prefers o-cresol epoxy resin.

[0032] In one embodiment, the curing agent is a phenolic resin containing at least two phenolic hydroxyl groups; specific examples of the curing agent include: linear phenol formaldehyde resin, linear BPA formaldehyde resin, aralkylphenol resin, biphenyl aralkylphenol resin, polyaromatic cyclic phenolic resin, etc.; from the perspective of general versatility, the present disclosure prefers linear phenol formaldehyde resin.

[0033] In one embodiment, the low stress modifier is at least one of epoxy-modified silicone resin, methacrylic-containing silane, amino-containing silane, mercapto-containing silane, and carboxyl-terminated nitrile rubber.

[0034] In one embodiment, the accelerator is at least one of an amine compound, an organic phosphorus compound, and an imidazole compound; the accelerator can be activated under curing temperature conditions to promote the reaction between the epoxy resin and the curing agent. The accelerator is usually inactive or has low activity at room temperature. From the perspective of curing temperature and curing system, the present disclosure prefers organic phosphorus compounds; further, the accelerator is at least one of triphenylphosphine (TPP), tetraphenylphosphonium bromide, triphenylphosphine-1,4-benzoquinone adduct (TPP-BQ), and urotropine.

[0035] In one embodiment, the release agent is at least one of carnauba wax, polyethylene wax, oxidized polyethylene wax, Fischer-Tropsch wax, polypropylene wax, and fatty acid wax; the release agent has good heat resistance and is not easy to decompose, which is beneficial to the separation of epoxy molding compound and mold for electronic packaging. Calcium stearate is preferred in the present disclosure.

[0036] In one embodiment, the flame retardant is at least one of a halogen flame retardant, a phosphorus flame retardant, a nitrogen flame retardant, a phosphorus-halogen flame retardant, a phosphorus-nitrogen flame retardant, and a hydroxide flame retardant.

[0037] In one embodiment, the pigment can impart color to the epoxy molding compound for electronic packaging, and has good dispersibility, weather resistance, thermal stability and chemical stability; specific examples of the pigment include carbon black, titanium dioxide, chrome yellow and phthalocyanine blue. Those skilled in the art can select a suitable pigment according to actual needs.

[0038] In a fifth aspect, a method for preparing the epoxy molding compound for electronic packaging is provided, comprising the following steps: after uniformly mixing the components in proportion, adding the obtained premix into a screw extruder, melt-extruding, and crushing to obtain the epoxy molding compound for electronic packaging.

[0039] In one embodiment, the melt extrusion temperature is 80-100°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, but is not limited to the listed values, and other values ​​within the range are also applicable.

[0040] Compared with the prior art, the beneficial effects of the present invention are as follows: in the present invention, on the one hand, spherical alumina with different particle sizes are compounded to form a three-dimensional network structure with high efficiency in thermal conductivity; on the other hand, a bifunctional phenyl-containing silane is used as a modifier to modify the spherical alumina, and the alkoxy groups on the phenyl-containing silane can be combined with hydrogen bonds on the surface of the spherical alumina to improve the loose pore state of the spherical alumina, so that the surface of the modified spherical alumina is denser and smoother; the compatibility between the modified spherical alumina and epoxy resin is improved, thereby improving the thermal conductivity, fluidity, and mechanical properties of the epoxy molding compound for electronic packaging and reducing the warping of the epoxy molding compound for electronic packaging. DETAILED DESCRIPTION

[0041] In order to better illustrate the purpose, technical scheme and advantages of the present disclosure, the present disclosure will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present disclosure in detail, rather than to limit the present disclosure. All other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure. The experimental reagents and instruments involved in the implementation of the present disclosure are all commonly used ordinary reagents and instruments unless otherwise specified.

[0042] The raw materials used in the embodiments and comparative examples are described below, but are not limited to these materials:

[0043] Table 1

[0044]

[0045]

[0046] The terephthaloylsilane was prepared in-house, and its preparation method was as follows: 5 g of lithium aluminum hydride was added to 500 mL of ether to obtain an ether solution of lithium aluminum hydride; then, 121 g of 1,4-di(trichlorosilane)benzene was added dropwise to the ether solution of lithium aluminum hydride at a temperature of 15°C, and after the addition was completed, the reaction was refluxed at a temperature of 40°C for 2 hours, and the reaction product was extracted with petroleum ether and ether in turn, and the extracted product was washed 5 times with aqueous hydrochloric acid to obtain terephthaloylsilane.

[0047] 1,4-bis(triethoxysilane)benzene was prepared in-house. The preparation method was as follows: 50 g of p-phenylene disilane and 150 g of ethanol were mixed, and the mixture was refluxed for 2 h at pH = 5 and a temperature of 60°C. The product obtained by the reaction was washed and distilled under reduced pressure to obtain 1,4-bis(triethoxysilane)benzene, which was named KM-1.

[0048] 1,4-bis(tripropoxysilane)benzene was prepared in-house. The preparation method was as follows: 50 g of p-phenylene disilane and 180 g of n-propanol were mixed, and the mixture was refluxed for 2 h at pH = 5 and 80 ° C. The product obtained by the reaction was washed and distilled under reduced pressure to obtain 1,4-bis(tripropoxysilane)benzene, which was named KM-2.

[0049] 1,4-bis(trihexyloxysilane)benzene was prepared in-house. The preparation method was as follows: 50 g of p-phenylene disilane and 200 g of n-hexanol were mixed, and the mixture was refluxed for 2 h at pH = 5 and 90 ° C. The product obtained by the reaction was washed and distilled under reduced pressure to obtain 1,4-bis(trihexyloxysilane)benzene, which was named KM-3.

[0050] Examples 1-10 and Comparative Examples 1-4

[0051] The components and weight proportions of the fillers for electronic packaging of Examples 1-10 and Comparative Examples 1-4 are shown in Table 2. The preparation methods of the fillers for electronic packaging of Examples 1-10 and Comparative Examples 1-4 include the following steps:

[0052] (1) Weigh each component according to the ratio;

[0053] (2) mixing the filler, water and ethanol mixed solution in step (1) to obtain a filler dispersion; wherein the mass ratio of the filler to the mixed solution is 1:10;

[0054] (3) Add the modifier to the filler dispersion, stir evenly, and react at 60° C. for 5 h. Filter, dry, and crush the reaction product to obtain a filler for electronic packaging.

[0055] Table 2

[0056]

[0057]

[0058] Application Examples 1-10 and Comparative Application Examples 1-4

[0059] The components and weight proportions of the epoxy molding compound for electronic packaging of application examples 1-10 and application comparison examples 1-4 are shown in Table 3, wherein the preparation method of the epoxy molding compound for electronic packaging of application examples 1-10 and application comparison examples 1-4 comprises the following steps:

[0060] (1) Weigh each component according to the ratio;

[0061] (2) adding the solid components into a high-speed mixer and mixing at a speed of 2000 rpm for 30 min to obtain a premix;

[0062] (3) adding the premix obtained in step (2) to the main feeding system of a twin-screw extruder, adding the liquid component to the side feeding system of the twin-screw extruder, mixing and extruding at 80-100° C., and crushing to obtain an epoxy molding compound for electronic packaging.

[0063] Table 3

[0064]

[0065]

[0066] Performance Testing

[0067] The performance of the epoxy molding compound for electronic packaging obtained from the application example and the comparative example was tested, and the test method is as follows:

[0068] (1) Gel time: Take 1.0g of epoxy molding compound powder and place it on a heating plate at 175±1℃. Start timing when the sample melts and press it continuously with a flat spatula. Stop timing when it turns into a gel state.

[0069] (2) Spiral flow length: At 175°C, the transfer pressure is set to 6.9 MPa. The epoxy molding compound powder is injected into the spiral flow length test mold preheated to the same temperature through a transfer molding press, and the length of the longest continuous point is read.

[0070] (3) Thermal conductivity: The steady-state heat flow method of ASTM D 5470 was used, and a thermal conductivity meter produced by Xiangtan Xiangke DRL was used. The hot plate temperature was 50°C, and the thickness of the epoxy molding compound sample after curing was 2 mm.

[0071] (4) Linear expansion coefficient, glass transition temperature: ASTM E831-19, probe method, TA TMAQ400 static thermomechanical analyzer, compression mode test of cured epoxy molding compound, heating rate set to 10°C / min.

[0072] (5) Bending strength: GB / T9341 is used, and the load application speed is 2 mm / min. The load value is read until the cured epoxy molding compound sample breaks.

[0073] (6) Flexural modulus: The test was conducted using a TA DMA850 dynamic thermal mechanical analyzer in a three-point bending mode with fixed amplitude oscillation, a preload of 0.5 N, a heating rate of 3 °C / min, and a temperature range of 25-280 °C. The sample size was 3*15*50 mm. The modulus data were read at 25 °C and 260 °C.

[0074] In the above performance test, the preparation method of the cured epoxy molding compound is: injecting the epoxy molding compound into molds of shapes recorded in different standards, and curing it at 175° C. for 6 hours to obtain the obtained epoxy molding compound.

[0075] The test results are shown in Tables 4 and 5.

[0076] Table 4

[0077]

[0078] Table 5

[0079]

[0080] From the test data in Table 4 and Table 5, it can be seen that the filler for electronic packaging disclosed in the present invention can significantly improve the overall performance of epoxy molding compound, and the thermal conductivity of epoxy molding compound for electronic packaging can reach above 3W / m·K, and some can reach above 4.0W / m·K, which exceeds most similar products on the market and is better than the thermal conductivity of Comparative Examples 1-2. At the same time, its fluidity can reach above 120cm, the linear expansion coefficient is lower than 15 in the first stage, and the bending strength is greater than 150MPa, which has achieved excellent performance for the requirements of chip packaging application scenarios.

[0081] From comparative examples 1-3, it can be seen that when the phenyl-containing silane is 1,4-bis(triethoxysilane)benzene and 1,4-bis(tripropoxysilane)benzene, the obtained epoxy molding compound for electronic packaging has better overall performance, among which when the phenyl-containing silane is 1,4-bis(triethoxysilane)benzene and 1,4-bis(trihexyloxysilane)benzene, the obtained epoxy molding compound for electronic packaging has a higher spiral flow length, indicating that its fluidity is better, which may be due to the fact that 1,4-bis(trihexyloxysilane)benzene has a longer fatty chain and the spherical alumina has a stronger connection performance.

[0082] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present disclosure rather than to limit the protection scope of the present disclosure. Although the present disclosure has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present disclosure can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present disclosure.

Claims

1. A filler for electronic packaging, characterized in that: including spherical alumina and phenyl-containing silane; Based on 100 parts by mass of spherical alumina, the spherical alumina includes 0.1-50 parts of large-particle spherical alumina, 0.1-70 parts of medium-particle spherical alumina and 0.1-20 parts of small-particle spherical alumina, the average particle size of the small-particle spherical alumina is ≤1 μm, the average particle size of the medium-particle spherical alumina is 1-10 μm, and the average particle size of the large-particle spherical alumina is >10 μm; The structural formula of the phenylsilane-containing compound is: Wherein, n is an integer from 0 to 16.

2. The filler for electronic packaging according to claim 1, characterized in that: The benzene-containing silanes are 1,4-bis(triethoxysilane)benzene and 1,4-bis(tripropoxysilane)benzene.

3. The filler for electronic packaging according to claim 1, characterized in that: The mass of the phenylsilane is 0.1-1% of the mass of the spherical alumina.

4. The electronic packaging filler according to claim 1, characterized in that: The preparation method of the phenyl-containing silane comprises: subjecting 1,4-di(trichlorosilane)benzene and lithium aluminum hydride to a first reaction to obtain p-phenylene disilane, and then subjecting p-phenylene disilane to a second reaction with alcohol to obtain the phenyl-containing silane, wherein the number of carbon atoms of the alcohol is 2-17.

5. A method for preparing a filler for electronic packaging as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: The spherical alumina is added into a solvent and mixed evenly to obtain a spherical alumina dispersion, and then phenylsilane is added to obtain a filler for electronic packaging, wherein the mass of the phenylsilane is 0.1-1% of the mass of the spherical alumina.

6. Use of the filler for electronic packaging as claimed in any one of claims 1 to 4 in epoxy molding compound for electronic packaging.

7. An epoxy molding compound for electronic packaging, characterized in that: The invention comprises the following components in parts by weight: 2-10 parts of epoxy resin, 2-10 parts of curing agent, 0.01-0.5 parts of curing accelerator, 1-3 parts of low stress modifier, 70-95 parts of thermal conductive filler, 0-1 parts of release agent, 0.01-1 parts of pigment and 0.1-2 parts of flame retardant; the thermal conductive filler is the filler for electronic packaging as described in any one of claims 1 to 4.

8. The epoxy molding compound for electronic packaging as claimed in claim 7, characterized in that: The epoxy resin contains at least two epoxy groups; And / or, the curing agent is a phenolic resin containing at least two phenolic hydroxyl groups; And / or, the low stress modifier is at least one of epoxy-modified silicone resin, methacrylic-containing silane, amino-containing silane, mercapto-containing silane, and carboxyl-terminated nitrile rubber; And / or, the accelerator is at least one of an amine compound, an organic phosphorus compound, and an imidazole compound; And / or, the release agent is at least one of carnauba wax, polyethylene wax, oxidized polyethylene wax, Fischer-Tropsch wax, polypropylene wax, and fatty acid wax; And / or, the flame retardant is at least one of a halogen flame retardant, a phosphorus flame retardant, a nitrogen flame retardant, a phosphorus-halogen flame retardant, a phosphorus-nitrogen flame retardant, and a hydroxide flame retardant.

9. A method for preparing an epoxy molding compound for electronic packaging as claimed in claim 7 or 8, characterized in that: The following steps are involved: After the components are uniformly mixed according to proportion, the obtained premix is ​​added into a screw extruder, melt-extruded, and crushed to obtain the epoxy molding compound for electronic packaging.

10. The preparation method according to claim 9, characterized in that: The temperature of the melt extrusion is 80-100°C.

Citation Information

Patent Citations

  • Super heat resistance and high heat conduction epoxy molding compound used for semiconductor packaging

    CN109467881A

  • High-thermal-conductivity and low-stress epoxy molding compound for semiconductor packaging

    CN111073217A