A plugging and anti-collapse agent for drilling fluid based on asphalt and its production method

The sulfonated asphalt is coated with rubber modified materials and combined with sodium lignosulfonate and xanthan gum modified materials to form a high-strength cured film, which solves the problem of flow deformation of sulfonated asphalt under high temperature and high pressure conditions and significantly improves sealing efficiency. The stability and blocking effect of the plugging and anti-collapse agent enhance the strength and anti-collapse performance of the clay.

CN118496827BActive Publication Date: 2024-10-22KARAMAY YOULIAN IND +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410972617.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-22
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Existing sulfonated asphalt is prone to flow and deform under high temperature and high pressure conditions, causing well collapse problems and affecting the safety and efficiency of drilling operations.

Method used

The sulfonated asphalt is coated with rubber modified materials and combined with sodium lignosulfonate and xanthan gum modified materials to form a blocking and anti-collapse agent with high strength and stability, which strengthens the clay particles through electrostatic attraction and exchange. The cured film on the surface reduces moisture intrusion and improves the sealing effect.

Benefits of technology

Under high temperature conditions, the stability and blocking effect of the plugging and anti-collapse agent are significantly enhanced, water intrusion is reduced, the strength and anti-collapse performance of the clay are improved, and the service life of the drilling fluid is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118496827B_ABST
    Figure CN118496827B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of oilfield drilling, and discloses a plugging and anti-collapse agent for drilling fluid based on asphalt and a production method thereof. The plugging and anti-collapse agent is formed by mixing sulfonated asphalt powder as a main raw material, and rubber modified material, sodium lignin sulfonate and xanthan gum modified material as auxiliary materials. The sulfonated asphalt is coated with the rubber modified material, and a large amount of quaternary ammonium nitrogen cations in the structure of the rubber modified material are used to exchange ions with clay particles, so that the plugging and anti-collapse agent can be stably adsorbed on the surface of the clay particles to form a solidified film, thereby enhancing the strength of the mud shale. In addition, the rigid heteroazosilicon tricyclic ring can make the solidified film stronger and more stable, thereby improving the high temperature resistance of the plugging and anti-collapse agent. The addition of the xanthan gum modified material can inhibit the collapse of shale and reduce the hydration of clay, thereby synergistically enhancing the effect of the plugging and anti-collapse agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oilfield drilling, and in particular to a plugging and anti-collapse agent for drilling fluid based on asphalt and a production method thereof. Background Art

[0002] In oil drilling projects, the performance of drilling fluid is directly related to the safety and efficiency of drilling. As an important component of drilling fluid, plugging and anti-collapse agents play a vital role in preventing well wall collapse and improving drilling efficiency. Among them, asphalt can play a role through its good adhesion and film-forming properties. During the drilling process, asphalt can quickly form a dense film on the well wall, effectively preventing groundwater and other fluids from eroding the well wall and enhancing the stability of the well wall. At the same time, asphalt can also fill the tiny cracks and pores on the well wall, reduce the filtration loss of drilling fluid, and improve the plugging effect of drilling fluid. Therefore, asphalt is increasingly used in drilling fluid. However, asphalt is easy to soften and deform at high temperatures, causing the formed film to lose its original plugging effect. This phenomenon is particularly obvious in deep drilling or geothermal drilling, which seriously affects the safety and efficiency of drilling operations. Therefore, asphalt needs to be modified.

[0003] At present, sulfonated asphalt is prepared by sulfonating asphalt with sulfur trioxide, fuming sulfuric acid, concentrated sulfuric acid or chlorosulfonic acid, and has been widely used in major oil fields. However, the rheological properties of sulfonated asphalt cause it to flow and deform under high temperature and high pressure conditions, which in turn causes well collapse problems. There are obvious defects in practical applications.

[0004] Therefore, the development of drilling fluid plugging and anti-collapse agents with functional properties such as high temperature resistance is of great significance to the further development of the oil drilling industry. Summary of the invention

[0005] In order to solve the problems mentioned in the background technology, the object of the present invention is to provide a plugging and anti-collapse agent for drilling fluid based on asphalt and a production method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A plugging and anti-collapse agent for drilling fluid based on asphalt, comprising the following raw materials in parts by mass:

[0008] 45-55 parts of sulfonated asphalt powder;

[0009] 15-30 parts of rubber modified material;

[0010] Sodium lignin sulfonate 5-15 parts;

[0011] 2-6 parts of xanthan gum modified material;

[0012] The rubber modified material is a natural rubber derivative containing quaternary ammonium nitrogen cations in its structure.

[0013] As a further solution of the present invention, the preparation method of the rubber modified material is as follows:

[0014] Step S1, dissolving the epoxidized natural rubber in toluene, stirring until dissolved, adding a tertiary amine crosslinking agent to the formed reaction solution, gradually raising the temperature to 60-70° C. after the addition, and maintaining the temperature for 3-6 hours, then adjusting the pH value with glacial acetic acid, continuing to keep the temperature and stirring for 4-6 hours, then evaporating under reduced pressure, collecting the product, and obtaining a rubber intermediate;

[0015] In the above technical solution, the epoxidized natural rubber structure contains a large number of epoxy groups, which can undergo a quaternary ammonium ring-opening reaction with the tertiary amine groups in the tertiary amine crosslinking agent structure to obtain a rubber intermediate with a branched structure;

[0016] Step S2, mixing the rubber intermediate with N,N-dimethylformamide, mechanically stirring and mixing, then adding a bridging agent, stirring at room temperature for 1-2 hours, then adding silazotricycloethylene glycol and a phase transfer catalyst, and under nitrogen protection, gradually raising the temperature to 90-100° C., maintaining the temperature for 4-8 hours under continuous stirring, and collecting the product under reduced pressure evaporation to obtain a rubber modified material.

[0017] Since active hydroxyl groups are generated during the quaternization ring-opening reaction, the rubber intermediate can undergo ring-opening esterification with the bridging agent to form an intermediate product. Then, under the action of a phase transfer catalyst, the intermediate product further condenses with the carboxyl group in the silatricycloethylene glycol structure to form a silatricyclo-natural rubber derivative bridged by a bridging agent, namely a rubber modified material.

[0018] As a further embodiment of the present invention, in step S1, the tertiary amine cross-linking agent is selected from N,N,N',N'-tetramethyl-1,4-butanediamine or N,N,N',N'-tetramethyl-1,6-hexanediamine.

[0019] As a further solution of the present invention, in step S1, the pH value is 6-7.

[0020] As a further embodiment of the present invention, in step S2, the bridging agent is selected from maleic anhydride, succinic anhydride or glutaric anhydride.

[0021] As a further embodiment of the present invention, in step S2, the phase transfer catalyst is p-toluenesulfonic acid.

[0022] As a further embodiment of the present invention, the preparation method of the xanthan gum modified material is as follows:

[0023] Mix humic acid and dimethyl sulfoxide, stir evenly, add accelerator and condensing agent to the formed homogeneous solution, stir at room temperature for 1-3 hours, then add xanthan gum to the homogeneous solution, continue to mechanically stir at room temperature for 3-6 hours, evaporate the solvent, cool and discharge the material to obtain xanthan gum modified material.

[0024] In the above scheme, the condensation agent and the promoter are first used to activate the substituted carboxyl groups in the humic acid structure, and then condense the substituted carboxyl groups with the hydroxyl groups in the xanthan gum structure to obtain the xanthan gum modified material.

[0025] As a further embodiment of the present invention, the accelerator is selected from 4-dimethylaminopyridine or N-hydroxysuccinimide.

[0026] As a further embodiment of the present invention, the condensing agent is selected from N,N'-dicyclohexylcarbodiimide or 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride.

[0027] A method for producing a plugging and anti-collapse agent for drilling fluid based on asphalt, comprising the following steps:

[0028] The first step is to add the sulfonated asphalt powder to 60-70% ethanol by volume, stir and mix, and then add the rubber modified material to the formed suspension. After the addition, the temperature is increased to 60-70°C, and after stirring and mixing for 1-2 hours, the solvent is evaporated to form an anti-collapse agent precursor;

[0029] The second step is to mix the anti-collapse agent precursor, sodium lignin sulfonate and xanthan gum modified material, and stir them at a temperature of 140-150°C for 1-2 hours, discharge the material, and undergo drying and grinding processes to obtain the anti-collapse agent.

[0030] Since the sulfonated asphalt powder can ionize to produce sulfonate groups, it will generate electrostatic attraction with the quaternary ammonium nitrogen cations in the rubber modified material structure, so that the rubber modified material with a highly branched structure can be coated on the surface of the sulfonated asphalt powder to form an anti-collapse agent precursor. Then, under high temperature conditions, the anti-collapse agent precursor is mixed with sodium lignin sulfonate and xanthan gum modified material to obtain a plugging anti-collapse agent.

[0031] Beneficial effects of the present invention:

[0032] (1) The present invention uses rubber modifiers to coat sulfonated asphalt, so that when the plugging and anti-collapse agent is used, it can use the large amount of quaternary ammonium nitrogen cations in the rubber modifier structure to exchange ions with clay particles, and at the same time, it can also generate electrostatic effects, so that the plugging and anti-collapse agent can be stably adsorbed on the surface of clay particles, and form an interwoven, criss-crossed solidified film, so that the strength of the mudstone is effectively enhanced, and the branched natural rubber can extend to the gaps between the clay particles, thereby playing a role in plugging microcracks, which can reduce the intrusion of water and produce a strong inhibitory effect when the clay is hydrated and expanded, thereby playing a good role in plugging and anti-collapse. In addition, because the rubber modifier molecular chain contains rigid heteroazosilicon tricyclic rings, the solidified film can have higher strength and stability, which can improve the use effect of the plugging and anti-collapse agent under high temperature conditions.

[0033] (2) The present invention prepares xanthan gum modified material as an additive and utilizes the colloidal components of xanthan gum itself. During the use of the plugging and anti-collapse agent, the formed filter cake can be made denser and have a lower permeability. At the same time, the humic acid in the structure can inhibit shale collapse and reduce clay hydration, thereby synergistically enhancing the effect of the plugging and anti-collapse agent. In addition, since the sulfonated asphalt has a poor dispersion effect in the water phase after being coated with the rubber molecular chain, sodium lignin sulfonate is added to improve the dispersion effect of the asphalt in the water phase, so that it can effectively play its own plugging and anti-collapse effect.

[0034] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0036] Figure 1 This is the infrared analysis test chart of rubber modified materials. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0038] A plugging and anti-collapse agent for drilling fluid based on asphalt, comprising the following raw materials in parts by mass:

[0039] 45 parts of sulfonated asphalt powder;

[0040] 15 parts of rubber modified material;

[0041] 5 parts of sodium lignin sulfonate;

[0042] 2 parts of xanthan gum modified material;

[0043] The preparation method of the plugging and anti-collapse agent comprises the following steps:

[0044] The first step is to add the sulfonated asphalt powder to 60% ethanol by volume, stir and mix, and then add the rubber modified material to the formed suspension. After the addition is completed, the temperature is increased to 60°C, and after stirring and mixing for 2 hours, the solvent is evaporated to form an anti-collapse agent precursor;

[0045] In the second step, the anti-collapse agent precursor, sodium lignin sulfonate and xanthan gum modified material are mixed and stirred at 140°C for 1 hour. The material is discharged and subjected to drying and grinding processes to obtain the anti-collapse agent. Example 2

[0046] A plugging and anti-collapse agent for drilling fluid based on asphalt, comprising the following raw materials in parts by mass:

[0047] 50 parts of sulfonated asphalt powder;

[0048] 25 parts of rubber modified material;

[0049] Sodium lignin sulfonate 12 parts;

[0050] 5 parts of xanthan gum modified material;

[0051] The preparation method of the plugging and anti-collapse agent comprises the following steps:

[0052] The first step is to add the sulfonated asphalt powder to 70% ethanol by volume, stir and mix, and then add the rubber modified material to the formed suspension. After the addition is completed, the temperature is increased to 65°C, and after stirring and mixing for 2 hours, the solvent is evaporated to form an anti-collapse agent precursor;

[0053] The second step is to mix the anti-collapse agent precursor, sodium lignin sulfonate and xanthan gum modified material, and stir them at 150°C for 1 hour. After the material is discharged, it is dried and ground to obtain the anti-collapse agent. Example 3

[0054] A plugging and anti-collapse agent for drilling fluid based on asphalt, comprising the following raw materials in parts by mass:

[0055] 55 parts of sulfonated asphalt powder;

[0056] 30 parts of rubber modified material;

[0057] 15 parts of sodium lignin sulfonate;

[0058] 6 parts of xanthan gum modified material;

[0059] The preparation method of the plugging and anti-collapse agent comprises the following steps:

[0060] The first step is to add the sulfonated asphalt powder into 70% ethanol by volume, stir and mix, and then add the rubber modified material to the formed suspension. After the addition, the temperature is raised to 70°C, and after stirring and mixing for 1 hour, the solvent is evaporated to form an anti-collapse agent precursor;

[0061] The second step is to mix the anti-collapse agent precursor, sodium lignin sulfonate and xanthan gum modified material, and stir them at 150°C for 1 hour. After the material is discharged, it is dried and ground to obtain the anti-collapse agent.

[0062] Comparative Example 1

[0063] A plugging and anti-collapse agent for drilling fluid based on asphalt, comprising the following raw materials in parts by mass:

[0064] 50 parts of sulfonated asphalt powder;

[0065] Sodium lignin sulfonate 12 parts;

[0066] 5 parts of xanthan gum modified material;

[0067] The preparation method of the plugging and anti-collapse agent is as follows:

[0068] The sulfonated asphalt powder, sodium lignin sulfonate and xanthan gum modified material are mixed and stirred at 150°C for 1 hour. The material is discharged and subjected to drying and grinding processes to obtain a plugging and anti-collapse agent.

[0069] Comparative Example 2

[0070] A plugging and anti-collapse agent for drilling fluid based on asphalt, comprising the following raw materials in parts by mass:

[0071] 50 parts of sulfonated asphalt powder;

[0072] 25 parts of rubber modified material;

[0073] Sodium lignin sulfonate 12 parts;

[0074] The preparation method of the plugging and anti-collapse agent comprises the following steps:

[0075] The first step is to add the sulfonated asphalt powder to 70% ethanol by volume, stir and mix, and then add the rubber modified material to the formed suspension. After the addition is completed, the temperature is increased to 65°C, and after stirring and mixing for 2 hours, the solvent is evaporated to form an anti-collapse agent precursor;

[0076] The second step is to mix the anti-collapse agent precursor and sodium lignin sulfonate, and stir them at a temperature of 150° C. for 1 hour. The material is discharged, and after drying and grinding processes, the anti-collapse agent can be obtained.

[0077] The rubber modified materials in the above examples and comparative examples were prepared by the following method:

[0078] Step S1, dissolving 1.2 g of epoxidized natural rubber in toluene, stirring until dissolved, adding 0.5 g of N,N,N',N'-tetramethyl-1,6-hexanediamine to the formed reaction solution, gradually raising the temperature to 65° C. after the addition, and maintaining the temperature for 4 h, then adjusting the pH value to 7 with glacial acetic acid, continuing to keep warm and stir for 5 h, then evaporating under reduced pressure, collecting the product, and obtaining a rubber intermediate;

[0079] Step S2, 1.5 g of the rubber intermediate is mixed with N,N-dimethylformamide, and the mixture is mechanically stirred and mixed. Then, 0.1 g of succinic anhydride is added, and the mixture is stirred for 1 h at room temperature. Then, 0.2 g of tricyclic silazoline glycol and 0.01 g of p-toluenesulfonic acid are added. Under nitrogen protection, the temperature is gradually increased to 100 ° C. and maintained for 6 h under continuous stirring. The product is evaporated under reduced pressure and collected to obtain a rubber modified material.

[0080] Figure 1 This is the infrared analysis test chart of the rubber modified material, where 3402cm -1 The absorption peak at 1713 cm is the characteristic absorption peak of the hydroxyl group produced by the ring-opening reaction. Obviously, the active hydroxyl group produced was not completely consumed in step S2. -1 The absorption peak at 1402 cm is the characteristic absorption peak of the ester group C=O produced by the condensation reaction. -1 The absorption peak at 1040 cm is the characteristic absorption peak of CN in quaternary ammonium nitrogen cations. -1 The absorption peak that appears at is the Si-O characteristic absorption peak.

[0081] The xanthan gum modified materials in the above examples and comparative examples were prepared by the following method:

[0082] Mix 1.8g of humic acid and dimethyl sulfoxide, stir well, add 0.3g of 4-dimethylaminopyridine and 0.8g of N,N'-dicyclohexylcarbodiimide to the formed homogeneous solution, stir at room temperature for 2h after addition, then add 3.5g of xanthan gum to the homogeneous solution, continue to mechanically stir at room temperature for 4h after addition, evaporate to remove the solvent, cool and discharge the material to obtain xanthan gum modified material.

[0083] Test Case

[0084] Configuration of base slurry:

[0085] Add 2g of anhydrous sodium carbonate to 1L of purified water, shake well, control the speed to 10000r / min, add 45g of bentonite for drilling fluid under stirring conditions, stir for 30min after adding, and cure at room temperature for 24h to form a freshwater base slurry.

[0086] The prepared base slurry was evenly divided into 5 parts, the rotation speed was controlled to be 10000r / min, and 5g of the plugging and anti-collapse agents prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2 were added to the fresh water base slurry under stirring conditions. After the addition, the filtration loss test was performed according to the standard GB / T 16783.1-2014. After the test was completed, the plugging and anti-collapse agents of Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to hot rolling aging for 18h at a temperature of 180±5°C, and then naturally cooled, and the filtration loss test was performed again. The results are recorded in the following table:

[0087]

[0088] From the analysis of the test results, it can be seen that the plugging and anti-collapse agents in Examples 1 to 3 have significantly better plugging and anti-collapse effects, and still maintain good plugging and anti-collapse effects after high-temperature treatment. In contrast, in Comparative Example 1, sulfonated asphalt that is not coated with rubber modifier is used as the main raw material of the plugging and anti-collapse agent, and the plugging effect is obviously weakened, and the plugging effect decreases significantly after high-temperature treatment. The plugging and anti-collapse agent prepared in Comparative Example 2 does not add the raw material xanthan gum modified material, which obviously has a negative impact on the plugging effect of the plugging and anti-collapse agent, but the high temperature resistance performance is better.

[0089] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A plugging and anti-collapse agent for drilling fluid based on asphalt, characterized in that: Including the following raw materials by mass: 45-55 parts of sulfonated asphalt powder; 15-30 parts of rubber modified material; Sodium lignin sulfonate 5-15 parts; 2-6 parts of xanthan gum modified material; The rubber modified material is a natural rubber derivative containing quaternary ammonium nitrogen cations in its structure; The preparation method of the rubber modified material is as follows: Step S1, dissolving the epoxidized natural rubber in toluene, stirring until dissolved, adding a tertiary amine crosslinking agent to the formed reaction solution, gradually raising the temperature to 60-70° C. after the addition, and maintaining the temperature for 3-6 hours, then adjusting the pH value with glacial acetic acid, continuing to keep the temperature and stirring for 4-6 hours, then evaporating under reduced pressure, collecting the product, and obtaining a rubber intermediate; Step S2, mixing the rubber intermediate with N,N-dimethylformamide, mechanically stirring and mixing, then adding a bridging agent, stirring at room temperature for 1-2 hours, then adding silazotricycloethylene glycol and a phase transfer catalyst, and gradually raising the temperature to 90-100° C. under nitrogen protection, maintaining the temperature for 4-8 hours under continuous stirring, and collecting the product by reduced pressure evaporation to obtain a rubber modified material; The bridging agent is selected from maleic anhydride, succinic anhydride or glutaric anhydride; The preparation method of the xanthan gum modified material is as follows: Mix humic acid and dimethyl sulfoxide, stir evenly, add an accelerator and a condensing agent to the formed homogeneous solution, stir at room temperature for 1-3 hours after the addition, then add xanthan gum to the homogeneous solution, continue to mechanically stir at room temperature for 3-6 hours after the addition, evaporate the solvent, cool and discharge the material, and obtain a xanthan gum modified material; The accelerator is selected from 4-dimethylaminopyridine or N-hydroxysuccinimide; The condensing agent is selected from N,N'-dicyclohexylcarbodiimide or 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride.

2. The asphalt-based plugging and anti-collapse agent for drilling fluid according to claim 1, characterized in that: In step S1, the tertiary amine cross-linking agent is selected from N,N,N',N'-tetramethyl-1,4-butanediamine or N,N,N',N'-tetramethyl-1,6-hexanediamine.

3. The asphalt-based plugging and anti-collapse agent for drilling fluid according to claim 1, characterized in that: In step S1, the pH value is 6-7.

4. The asphalt-based plugging and anti-collapse agent for drilling fluid according to claim 1, characterized in that: In step S2, the phase transfer catalyst is p-toluenesulfonic acid.

5. A method for producing a plugging and anti-collapse agent for drilling fluid based on asphalt as claimed in claim 1, characterized in that: The following steps are involved: The first step is to add the sulfonated asphalt powder to 60-70% ethanol by volume, stir and mix, and then add the rubber modified material to the formed suspension. After the addition, the temperature is increased to 60-70°C, and after stirring and mixing for 1-2 hours, the solvent is evaporated to form an anti-collapse agent precursor; The second step is to mix the anti-collapse agent precursor, sodium lignin sulfonate and xanthan gum modified material, and stir them at a temperature of 140-150°C for 1-2 hours, discharge the material, and undergo drying and grinding processes to obtain the anti-collapse agent.

Citation Information

Patent Citations

  • Filtrate reducer for drilling fluid and preparation method of filtrate reducer

    CN104449595A

  • High-toughness low-shrinkage epoxy resin composition, insulating part and preparation method

    CN104559063A

  • Lubrication blocking agent used for drilling fluid and preparation method thereof

    CN104962247A

  • Quaternary ammonium salt-containing raw silicone rubber and its synthesis method and use in preparation of intrinsic quaternary ammonium salt mildewproof antibacterial sealant

    CN108641086A

  • Blocking and anti-collapse agent used for drilling fluid and preparation method thereof

    CN109705824A