A coated and modified lithium-rich manganese-based positive electrode material and its preparation method and application

CN118507698BActive Publication Date: 2024-11-01GANZHOU NOVA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410960026.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

[0006]但是现有技术中,富锂锰基正极材料在工作过程中易与电解液发生反应,导致富锂锰基正极材料被电解液腐蚀、分解,影响材料的可逆性和电化学性能

Benefits of technology

[0027]与现有技术相比,本发明提供的一个或多个技术方案至少具备以下有益技术效果之一:

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118507698B_ABST
    Figure CN118507698B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of lithium-ion battery materials, and discloses a coated modified lithium-rich manganese-based positive electrode material and a preparation method and application thereof. The positive electrode material comprises a lithium-rich manganese-based positive electrode material matrix and a coating layer coated on at least part of the surface of the lithium-rich manganese-based positive electrode material matrix; the molecular formula of the lithium-rich manganese-based positive electrode material matrix is ​​Li 1+m Mn 1‑m‑n X n O2, m is in the range of 0.1≤m≤0.5, n is in the range of 0≤n≤0.5, when n>0, X is any one or more of Ni, Co, Fe, Al, Zn; the molecular formula of the coating material is NaMF4; wherein M is one or more of Co, Sc, Y. The NaMF4 coating can effectively protect the lithium-rich manganese-based positive electrode material from being corroded by the electrolyte, and can also inhibit the decomposition of the electrolyte, thereby improving the sustainability and electrochemical performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium-ion battery materials and relates to a positive electrode material, in particular to a coated and modified lithium-rich manganese-based positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in mobile devices, electric vehicles, energy storage systems, aerospace and other fields. They have the advantages of high energy density, no memory effect, low self-discharge rate, environmental protection, and long service life. They are currently a hot spot for research and application in the energy industry. Commonly used high-nickel ternary materials, lithium cobalt oxide materials, and lithium iron phosphate materials have low specific capacity and low operating voltage. Relatively speaking, lithium-rich manganese-based materials have higher theoretical specific capacity and high operating voltage, and have broader application prospects.

[0003] In the prior art, doping is usually used to stabilize the crystal structure of the coated modified lithium-rich manganese-based positive electrode material, inhibit the release of oxygen in the lattice, and expand the interplanar spacing in the transition metal layer.

[0004] CN116314751A dopes cation La into the cobalt-free lithium-rich manganese-based positive electrode material to inhibit the formation of spinel phase during the charge and discharge process, thereby improving the discharge specific capacity and inhibiting the voltage decay during the charge and discharge cycle.

[0005] CN105789558A uses Zr and Na as double elements for doping, and uses the more stable Zr-O bond to stabilize the transition metal layer. + Doping into the lithium layer can expand the interlayer spacing, making lithium ions easier to deintercalate.

[0006] However, in the prior art, the lithium-rich manganese-based positive electrode material is prone to react with the electrolyte during operation, causing the lithium-rich manganese-based positive electrode material to be corroded and decomposed by the electrolyte, affecting the reversibility and electrochemical properties of the material. Summary of the invention

[0007] In view of the above problems existing in the prior art, in the first aspect, the present invention provides a coated and modified lithium-rich manganese-based positive electrode material; in the second aspect, the present invention provides a method for preparing the above coated and modified lithium-rich manganese-based positive electrode material; in the third aspect, the present invention provides a battery.

[0008] In a first aspect, the invention comprises a lithium-rich manganese-based positive electrode material substrate and a coating layer at least coated on a portion of the surface of the lithium-rich manganese-based positive electrode material substrate; the molecular formula of the lithium-rich manganese-based positive electrode material substrate is Li 1+m Mn 1-m-n X nO2, the value range of m is 0.1≤m≤0.5, the value range of n is 0≤n≤0.5, when n>0, X is any one or more of Ni, Co, Fe, Al, and Zn; the molecular formula of the coating layer material is NaMF4, and M is one or more of Co, Sc, and Y.

[0009] In a second aspect, the present invention provides a method for preparing the above-mentioned coated modified lithium-rich manganese-based positive electrode material, comprising the following steps:

[0010] Step 1, mixing sodium hydroxide, unsaturated fatty acid and anhydrous ethanol to obtain solution A,

[0011] Step 2, mixing solution A, ammonium fluoride solution, and metal salt solution M and performing a hydrothermal reaction to obtain a NaMF4 coating material;

[0012] Step 3, NaMF4 coating material, Li 1+m Mn 1-m-n X n The O2 substrate material and ethanol are mixed, ball-milled, and then dried to obtain a coated and modified lithium-rich manganese-based positive electrode material.

[0013] Preferably, in step 1, the unsaturated fatty acid is one or more of oleic acid, erucic acid, ricinoleic acid and trans-oleic acid.

[0014] Preferably, in step 1, the molar ratio of sodium hydroxide to unsaturated fatty acid is 1:1.1-1.5.

[0015] Preferably, in step 2, the metal salt of M is one or more of cobalt nitrate, cobalt acetate, scandium nitrate and yttrium nitrate.

[0016] Preferably, in step 2, the molar ratio of sodium hydroxide, unsaturated fatty acid, ammonium fluoride and metal salt of M participating in the hydrothermal reaction is 1:1.1-1.5:4:1.

[0017] More preferably, the concentration of sodium hydroxide in the solution A is 1-4 mol / L; the concentration of the ammonium fluoride solution is 0.5-1 mol / L; and the concentration of the metal salt solution M is 0.5-3 mol / L.

[0018] Preferably, in step 2, the hydrothermal reaction temperature is 160-200° C.; and the hydrothermal reaction time is 12-30 h.

[0019] Preferably, in step 4, NaMF4 coating material, Li 1+m Mn 1-m-n X n The mass ratio of the O2 substrate material is 1:20-50.

[0020] Further preferably, in step 4, the mass ratio of NaMF4 coating material to ethanol is 1:200-500.

[0021] Preferably, in step 3, the ball milling time is 0.5-5h.

[0022] Preferably, Li is prepared by the following method: 1+m Mn 1-m-n X n O2 substrate material: Lithium source, manganese source, and doped metal X source are mixed according to the stoichiometric ratio and sintered at high temperature to obtain Li 1+m Mn 1-m-n X n O2 base material.

[0023] Further preferably, the preparation of Li 1+m Mn 1-m-n X n When the substrate material is O2, the lithium source is one or more of lithium nitrate, lithium acetate and lithium hydroxide; the manganese source is one or more of manganese nitrate and manganese acetate; the doped metal X source is one or more of nitrates or acetates containing X.

[0024] Further preferably, the preparation of Li 1+m Mn 1-m-n X n When the substrate material is O2, the molar ratio of lithium, manganese and X element in the lithium source, manganese source and doped metal X source is 1.14-1.56: 0.5-0.9: 0-0.5.

[0025] Further preferably, the preparation of Li 1+m Mn 1-m-n X n When O2 substrate material is used, the sintering temperature is 800-1100℃; the sintering time is 12-30h.

[0026] In a third aspect, the present invention provides a battery, comprising the above-mentioned coated and modified lithium-rich manganese-based positive electrode material or the coated and modified lithium-rich manganese-based positive electrode material prepared by the above-mentioned preparation method.

[0027] Compared with the prior art, one or more technical solutions provided by the present invention have at least one of the following beneficial technical effects:

[0028] (1) The coated modified lithium-rich manganese-based positive electrode material provided by the present invention can effectively protect the lithium-rich manganese-based positive electrode material through the NaMF4 coating layer, so that it is not corroded by the electrolyte, and at the same time, it can inhibit the decomposition of the electrolyte, thereby improving the sustainability and electrochemical performance of the battery. 1+m Mn 1-m-n X nThe Li in the O2-based material forms a stronger Li-F bond, which can effectively improve the structural stability of the lithium-rich manganese-based material.

[0029] (2) The preparation process provided by the present invention synthesizes the NaMF4 coating material through a one-step hydrothermal method, and then coats it on the surface of the lithium-rich manganese-based positive electrode material through a liquid phase coating method. The preparation process is simple and easy to achieve large-scale production. The raw materials are easily available, which is conducive to promotion and marketization. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 HRTEM image of the NaCoF4 coating material obtained in step 2 of Example 1 of the present invention;

[0031] Figure 2 NaCoF4@Li prepared in Example 1 of the present invention 1.2 Mn 0.58 Ni 0.22 SEM image of O2-coated modified lithium-rich manganese-based cathode material;

[0032] Figure 3 NaCoF4@Li prepared in Example 1 of the present invention 1.2 Mn 0.58 Ni 0.22 TEM image of O2-coated modified lithium-rich manganese-based cathode material;

[0033] Figure 4 Li prepared in Comparative Example 1 of the present invention 1.2 Mn 0.58 Ni 0.22 TEM image of O2 lithium-rich manganese-based cathode material;

[0034] Figure 5 A schematic diagram of a cycle performance test of a battery assembled from positive electrode materials prepared in Examples 1-4 and Comparative Example 1 of the present invention;

[0035] Figure 6 This is a SEM image of the positive electrode material prepared in Example 1 of the present invention after working for a certain period of time. DETAILED DESCRIPTION

[0036] The present invention provides the following specific technical solutions.

[0037] In a first aspect, the present invention provides a coated modified lithium-rich manganese-based positive electrode material, comprising a lithium-rich manganese-based positive electrode material substrate and a coating layer coated on at least a portion of the surface of the lithium-rich manganese-based positive electrode material substrate; the molecular formula of the lithium-rich manganese-based positive electrode material substrate is Li 1+m Mn 1-m-n X nO2, the value range of m is 0.1≤m≤0.5, the value range of n is 0≤n≤0.5, when n>0, X is any one or more of Ni, Co, Fe, Al, and Zn; the molecular formula of the coating layer material is NaMF4, and M is one or more of Co, Sc, and Y.

[0038] In the prior art, the coated modified lithium-rich manganese-based positive electrode material is easily corroded by the electrolyte, which affects the reversibility and electrochemical performance of the material. Studies have found that coating the lithium-rich manganese-based substrate material with NaMF4 material can effectively protect the coated modified lithium-rich manganese-based positive electrode material from being corroded by the electrolyte. At the same time, the structure of the NaMF4 material contains the same Li-F bond as that in the electrolyte, which increases the concentration of Li-F bonds in the electrolyte, inhibits the decomposition of the electrolyte, and improves the sustainability of the electrolyte. In addition, the F in the NaMF4 coating layer is highly reactive with the substrate material Li 1+m Mn 1-m-n X n The Li in O2 forms a stronger Li-F bond, which can effectively improve the structural stability of lithium-rich manganese-based materials.

[0039] In a second aspect, the present invention provides a method for preparing the above-mentioned coated modified lithium-rich manganese-based positive electrode material, comprising the following steps:

[0040] Step 1, mixing sodium hydroxide, unsaturated fatty acid and anhydrous ethanol to obtain solution A,

[0041] Step 2, mixing solution A, ammonium fluoride solution, and metal salt solution M and performing a hydrothermal reaction to obtain a NaMF4 coating material;

[0042] Step 3, NaMF4 coating material, Li 1+m Mn 1-m-n X n The O2 substrate material and ethanol are mixed, ball-milled, and then dried to obtain a coated and modified lithium-rich manganese-based positive electrode material.

[0043] Research has found that the NaMF4 coating material is synthesized by a one-step hydrothermal method and then coated on the surface of the lithium-rich manganese-based positive electrode material by a liquid phase coating method. The preparation process is simple, easy to achieve large-scale production, and the raw materials are easily available, which is conducive to promotion and commercialization.

[0044] Preferably, in step 1, the unsaturated fatty acid is one or more of oleic acid, erucic acid, ricinoleic acid and trans-oleic acid.

[0045] Preferably, in step 1, the molar ratio of sodium hydroxide to unsaturated fatty acid is 1:1.1-1.5.

[0046] Preferably, in step 2, the metal salt of M is one or more of cobalt nitrate, cobalt acetate, scandium nitrate and yttrium nitrate.

[0047] Preferably, in step 2, the molar ratio of sodium hydroxide, unsaturated fatty acid, ammonium fluoride and metal salt of M participating in the hydrothermal reaction is 1:1.1-1.5:4:1.

[0048] More preferably, the concentration of sodium hydroxide in the solution A is 1-4 mol / L; the concentration of the ammonium fluoride solution is 0.5-1 mol / L; and the concentration of the metal salt solution M is 0.5-3 mol / L.

[0049] In actual situations, the contents of sodium hydroxide, unsaturated fatty acids, ammonium fluoride, and metal salts of M involved in the hydrothermal reaction, as well as the concentrations of solution A, ammonium fluoride solution, and metal salt solution of M can be adjusted according to actual needs. The molar ratio of sodium hydroxide, unsaturated fatty acids, ammonium fluoride, and metal salts of M involved in the hydrothermal reaction is 1:1.1-1.5:4:1, the concentration of sodium hydroxide in solution A is 1-4 mol / L, the concentration of ammonium fluoride solution is 0.5-1 mol / L, and the concentration of metal salt solution of M is 0.5-3 mol / L, which are only the preferred ranges proposed by the inventors after multiple experiments.

[0050] Preferably, in step 2, the hydrothermal reaction temperature is 160-200° C.; and the hydrothermal reaction time is 12-30 h.

[0051] Research has found that if the hydrothermal reaction temperature is too high / the time is too long, the unsaturated fatty acids will undergo high-temperature carbonization, thereby producing impurities and affecting the purity of the product; if the hydrothermal reaction temperature is too low / the time is too short, the reaction will be incomplete, the yield will be low, and the product will contain unreacted raw materials, which will also affect the purity of the product.

[0052] Preferably, in step 4, NaMF4 coating material, Li 1+m Mn 1-m-n X n The mass ratio of the O2 substrate material is 1:20-50.

[0053] Research has found that if there is too much NaMF4 coating material when preparing the positive electrode material and the corresponding base material is too little, it will directly affect the specific capacity of the positive electrode material; if there is too little coating material, it will easily lead to uneven coating, affecting the performance of the positive electrode material.

[0054] Further preferably, in step 4, the mass ratio of NaMF4 coating material to ethanol is 1:200-500.

[0055] In practical applications, the amount of solvent (ethanol) added when mixing the coating material and the base material can be adjusted according to actual conditions. The mass ratio of NaMF4 coating material to ethanol of 1:200-500 is only a preferred range proposed by the inventor.

[0056] Preferably, in step 4, the ball milling time is 0.5-5h.

[0057] In an embodiment of the present invention, Li 1+m Mn 1-m-n X n The O2 substrate material can be purchased from other manufacturers or prepared by yourself.

[0058] The present invention provides the following preparation method of Li 1+m Mn 1-m-n X n Preparation method of O2 substrate material: Lithium source, manganese source and doped metal X source are mixed according to the stoichiometric ratio and sintered at high temperature to obtain Li 1+m Mn 1-m-n X n O2 base material.

[0059] Further preferably, the preparation of Li 1+m Mn 1-m-n X n When the substrate material is O2, the lithium source is one or more of lithium nitrate, lithium acetate and lithium hydroxide; the manganese source is one or more of manganese nitrate and manganese acetate; the doped metal X source is one or more of nitrates or acetates containing X.

[0060] Further preferably, the preparation of Li 1+m Mn 1-m-n X n When the substrate material is O2, the molar ratio of lithium, manganese and X element in the lithium source, manganese source and doped metal X source is 1.14-1.56: 0.5-0.9: 0-0.5.

[0061] In practical applications, the addition amounts of the lithium source, the manganese source, and the doped metal X source can be adjusted according to actual needs, and whether to dope the X element can be selected according to actual needs.

[0062] Further preferably, the preparation of Li 1+m Mn 1-m-n X n When O2 substrate material is used, the sintering temperature is 800-1100℃; the sintering time is 12-30h.

[0063] Research has found that if the sintering temperature is too high, the product is easy to harden, resulting in larger and uneven particle sizes; if the sintering temperature is too low, it is easy to cause incomplete reaction, and some oxide impurities will appear in the product. If the sintering time is too long, a large number of primary particles of the product will aggregate during the sintering process, affecting the particle size of the product; if the sintering time is too short, the reaction is incomplete, which is easy to cause uneven particle distribution, and the product contains a large number of fine impurity particles.

[0064] The present invention provides a battery, comprising the above-mentioned coated modified lithium-rich manganese-based positive electrode material or the coated modified lithium-rich manganese-based positive electrode material prepared by the above-mentioned preparation method.

[0065] In order to make the technical problems to be solved, technical solutions and technical advantages of the present invention more clear, they will be described in detail below with reference to specific examples, but the protection scope of the present invention is not limited to the following specific embodiments.

[0066] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0067] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0068] Embodiment 1:

[0069] A method for preparing a coated and modified lithium-rich manganese-based positive electrode material comprises the following steps:

[0070] Step 1, dissolving 0.01 mol sodium hydroxide and 0.014 mol oleic acid in 3.5 mL anhydrous ethanol to form solution A;

[0071] Step 2, mixing solution A obtained in step 1, 50 mL of 0.8 mol / L ammonium fluoride solution and 10 mL of 1 mol / L cobalt nitrate solution, stirring evenly to obtain solution B; transferring solution B into a polytetrafluoroethylene liner, hydrothermally reacting at 200° C. for 24 hours, and then washing with water and alcohol to obtain a NaCoF4 coating material;

[0072] Step 3: After solid phase mixing of 0.125 mol lithium hydroxide, 0.058 mol manganese acetate and 0.022 mol nickel acetate, the mixture was placed in a muffle furnace for sintering at 950° C. for 18 h to obtain Li 1.2 Mn 0.58 Ni 0.22 O2 base material.

[0073] Step 4, take 5gLi 1.2 Mn 0.58Ni 0.22 The O2 substrate material was dispersed in 80 mL of ethanol, 0.175 g of NaCoF4 coating material was added, ball milled and mixed for 4 h, and dried to obtain NaCoF4@Li 1.2 Mn 0.58 Ni 0.22 O2-coated modified lithium-rich manganese-based positive electrode material.

[0074] Figure 1 HRTEM image of the NaCoF4 coated material obtained in step 2 of Example 1, measured Figure 1 The lattice fringes in the figure indicate that the material obtained in step 2 of Example 1 is NaCoF4.

[0075] Figure 2 The coated and modified lithium-rich manganese-based positive electrode material NaCoF4@Li prepared in Example 1 1.2 Mn 0.58 Ni 0.22 SEM image of O2, Figure 2 It can be seen intuitively that the positive electrode material prepared in Example 1 is in the form of micron blocks, the particles have no agglomeration phenomenon, the particle size distribution is uniform, and the material surface is smooth, indicating that the preparation process provided by the present invention has uniform coating and good coating effect.

[0076] Comparative Example 1:

[0077] 0.125 mol lithium hydroxide, 0.058 mol manganese acetate, and 0.022 mol nickel acetate were mixed in a solid phase and placed in a muffle furnace for sintering at 950 ° C for 18 h to obtain Li 1.2 Mn 0.58 Ni 0.22 O2 material is a lithium-rich manganese-based positive electrode material.

[0078] Figure 3 NaCoF4@Li prepared in Example 1 1.2 Mn 0.58 Ni 0.22 TEM image of O2-coated modified lithium-rich manganese-based cathode material. Figure 4 Li prepared in Comparative Example 1 1.2 Mn 0.58 Ni 0.22 TEM image of O2 lithium-rich manganese-based cathode material, combined with Figure 3 and Figure 4 It can be seen that the NaCoF4 coating material is uniformly coated on the Li 1.2 Mn 0.58 Ni 0.22 O2 substrate material.

[0079] Embodiment 2:

[0080] A method for preparing a coated and modified lithium-rich manganese-based positive electrode material comprises the following steps:

[0081] Step 1, 0.01 mol sodium hydroxide and 0.011 mol erucic acid are dissolved in 10 mL anhydrous ethanol to form solution A;

[0082] Step 2, mixing solution A obtained in step 1, 80 mL of 0.5 mol / L ammonium fluoride solution and 20 mL of 0.5 mol / L scandium nitrate solution, stirring evenly to obtain solution B; transferring solution B into a polytetrafluoroethylene liner, hydrothermally reacting at 160° C. for 30 hours, and then washing with water and alcohol to obtain a NaScF4 coated material;

[0083] Step 3: After solid phase mixing of 0.114 mol lithium hydroxide, 0.050 mol manganese nitrate and 0.04 mol ferrous nitrate, the mixture was placed in a muffle furnace and sintered at 800° C. for 30 h to obtain Li 1.1 Mn 0.5 Fe 0.4 O2 base material.

[0084] Step 4, take 5g Li 1.1 Mn 0.50 Fe 0.4 The O2 substrate material was dispersed in 45 mL of ethanol, 0.1 g of NaScF4 coating material was added, ball milled and mixed for 0.5 h, and dried to obtain NaScF4@Li 1.1 Mn 0.50 Fe 0.4 O2-coated modified lithium-rich manganese-based positive electrode material.

[0085] Embodiment 3:

[0086] A method for preparing a coated and modified lithium-rich manganese-based positive electrode material comprises the following steps:

[0087] Step 1, 0.01 mol sodium hydroxide and 0.015 mol trans-oleic acid are dissolved in 2.5 mL anhydrous ethanol to form solution A;

[0088] Step 2, mixing solution A obtained in step 1, 40 mL of 1 mol / L ammonium fluoride solution and 3.33 mL of 3 mol / L yttrium nitrate solution, stirring evenly to obtain solution B; transferring solution B into a polytetrafluoroethylene liner, hydrothermally reacting at 200° C. for 12 h, and then washing with water and alcohol to obtain a NaYF4 coating material;

[0089] Step 3: After solid phase mixing of 0.156 mol lithium hydroxide and 0.05 mol manganese acetate, the mixture was placed in a muffle furnace for sintering at 1100° C. for 12 h to obtain Li 1.5 Mn 0.5O2 base material.

[0090] Step 4, take 5gLi 1.5 Mn 0.5 The O2 substrate material was dispersed in 80 mL of ethanol, 0.25 g of NaYF4 coating material was added, ball milled and mixed for 5 h, and dried to obtain NaYF4@Li 1.5 Mn 0.5 O2-coated modified lithium-rich manganese-based positive electrode material.

[0091] Embodiment 4:

[0092] A method for preparing a coated and modified lithium-rich manganese-based positive electrode material comprises the following steps:

[0093] Step 1, 0.01 mol sodium hydroxide and 0.014 mol oleic acid are dissolved in 4 mL anhydrous ethanol to form solution A;

[0094] Step 2, mixing solution A obtained in step 1, 44.4 mL of 0.9 mol / L ammonium fluoride solution and 5 mL of 2 mol / L cobalt nitrate solution, stirring evenly to obtain solution B; transferring solution B into a polytetrafluoroethylene liner, hydrothermally reacting at 190° C. for 20 h, and then washing with water and alcohol to obtain a NaCoF4 coating material;

[0095] Step 3: After solid phase mixing of 0.125 mol lithium hydroxide, 0.063 mol manganese acetate and 0.017 mol zinc nitrate, the mixture was placed in a muffle furnace and sintered at 1000° C. for 16 h to obtain Li 1.2 Mn 0.63 Zn 0.17 O2 base material.

[0096] Step 4, take 5gLi 1.2 Mn 0.63 Zn 0.17 The O2 substrate material was dispersed in 125 mL of ethanol, 0.2 g of NaCoF4 coating material was added, ball milled and mixed for 3 h, and dried to obtain NaCoF4@Li 1.2 Mn 0.63 Zn 0.17 O2-coated modified lithium-rich manganese-based positive electrode material.

[0097] The positive electrode materials prepared in Examples 1-4 and Comparative Example 1 are assembled into batteries, and the assembly method is as follows:

[0098] The lithium-rich manganese-based material prepared in Examples 1-4 and Comparative Example 1 was used as the positive electrode material, mixed with the conductive agent acetylene black (AB) and the binder polyvinylidene fluoride (PVDF) at a mass ratio of 8:1:1, and N-methylpyrrolidone (NMP) was used as the solvent. The mixture was placed in a small beaker and stirred at a speed of 800 r / min for 2 hours to obtain a slurry. The slurry was coated on the current collector aluminum foil using an automatic coating machine, placed flat on tempered glass and transferred to a vacuum drying oven at 85°C for 4 hours, punched into a pole piece with a diameter of 12 mm, and then dried at 105°C in a vacuum drying oven for 4 hours. The pole piece was placed in a glove box filled with argon atmosphere with a water content and oxygen content of less than 0.1 ppm for 4 hours to reduce the moisture adsorbed by the pole piece during the transfer process, and then assembled into a CR2032 button battery in the glove box. The battery uses a pure metal lithium sheet with a diameter of 16 mm and a thickness of 0.5 mm as the negative electrode, and a porous polyethylene membrane of model Celgard2300 with a diameter of 18 mm as the separator.

[0099] After the battery was assembled and aged for 12 hours, it was activated at a voltage of 2-4.6V and a current density of 0.1C for 3 cycles, and then cycled at a current density of 1C for 100 cycles. The discharge specific capacity results are shown in Table 1.

[0100] Table 1 - Performance test of batteries assembled from positive electrode materials prepared in Examples 1-4 and Comparative Example 1

[0101]

[0102] Figure 5 The cycle performance diagram of the battery assembled from the positive electrode materials prepared in Examples 1-4 and Comparative Example 1. Figure 5 As shown in Table 1, the specific capacity and capacity retention rate of the battery assembled with the positive electrode materials prepared in Examples 1-4 after cycling are higher than those of the battery assembled with the positive electrode materials prepared in Comparative Example 1, indicating that the electrochemical performance of the positive electrode material provided by the present invention is more excellent. Based on the capacity retention rate of the battery assembled with the positive electrode materials prepared in Comparative Example 1 after 100 cycles, the capacity retention rate of the battery assembled with the positive electrode materials prepared in Examples 1-4 is significantly improved, indicating that the capacity attenuation rate of the battery when it is recharged after discharge is less, which can reflect from the side that the NaMF4@Li 1+m Mn 1-m-n X n The reversible performance of O2 positive electrode materials has been improved, proving that coating the surface of nickel-manganese-rich based positive electrode materials with NaMF4 materials can improve their electrochemical reversibility.

[0103] The battery assembled with the positive electrode material prepared in Example 1 was disassembled after 100 cycles, and the positive electrode material obtained by disassembly was crushed and then subjected to SEM detection. Figure 6 The SEM image is shown below. Figure 6 It can be seen that after working for a certain period of time, the lithium-rich manganese-based positive electrode material is still in micron blocks, the surface of the material is smooth, and the structure is consistent with Figure 1 Similarly, this can reflect to a certain extent that the lithium-rich manganese-based material provided by the present invention has good structural stability.

[0104] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A coated and modified lithium-rich manganese-based positive electrode material, characterized in that: The invention comprises a lithium-rich manganese-based positive electrode material matrix and a coating layer at least coated on a part of the surface of the lithium-rich manganese-based positive electrode material matrix; the molecular formula of the lithium-rich manganese-based positive electrode material matrix is ​​Li 1+m Mn 1-m-n X n O2, m is in the range of 0.1≤m≤0.5, n is in the range of 0≤n≤0.5, when n>0, X is any one or more of Ni, Co, Fe, Al, Zn; the molecular formula of the coating material is NaMF4, M is one or more of Co, Sc, Y; The method for preparing the coated modified lithium-rich manganese-based positive electrode material comprises the following steps: Step 1, mixing sodium hydroxide, unsaturated fatty acid and anhydrous ethanol to obtain solution A; Step 2, mixing solution A, ammonium fluoride solution, and metal salt solution M and performing a hydrothermal reaction to obtain a NaMF4 coating material; Step 3, NaMF4 coating material, Li 1+m Mn 1-m-n X n The O2 matrix material and ethanol are mixed, ball-milled, and then dried to obtain a coated and modified lithium-rich manganese-based positive electrode material.

2. The coated and modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 1, the unsaturated fatty acid is one or more of oleic acid, erucic acid, and ricinoleic acid; and the metal salt of M is one or more of nitrate and acetate.

3. The coated and modified lithium-rich manganese-based positive electrode material according to claim 1 or 2, characterized in that: In step 1, the molar ratio of sodium hydroxide to unsaturated fatty acid is 1:1.1-1.5; in step 2, the molar ratio of sodium hydroxide, unsaturated fatty acid, ammonium fluoride and metal salt of M involved in the hydrothermal reaction is 1:1.1-1.5:4:

1.

4. The coated and modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 2, the hydrothermal reaction temperature is 160-200° C.; the hydrothermal reaction time is 12-30 h.

5. The coated modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 3, NaMF4 coating material, Li 1+m Mn 1-m-n X n The mass ratio of O2 matrix material is 1:20-50.

6. The coated and modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 3, the ball milling time is 0.5-5h.

7. The coated and modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: Li was prepared by 1+m Mn 1-m-n X n O2 matrix material: Lithium source, manganese source, and doped metal X source are mixed according to the stoichiometric ratio and sintered at high temperature to obtain Li 1+m Mn 1-m-n X n O2 matrix material.

8. The coated and modified lithium-rich manganese-based positive electrode material according to claim 7, characterized in that: The molar ratio of lithium, manganese and X element in the lithium source, manganese source and doped metal X source is 1.14-1.56: 0.5-0.9: 0-0.5; the sintering temperature is 800-1100° C.; and the sintering time is 12-30 hours.

9. A battery, characterized in that: It comprises the coated and modified lithium-rich manganese-based positive electrode material as described in any one of claims 1 to 8.