A dimming temperature-increasing UV-resistant anti-icing coating and a method for preparing the coating

Hydrophobic nanosilica and rare earth oxide composite materials were prepared by curved surface response method to form dimming, heat preservation, ultraviolet-resistant anti-ice coating, which solved the ice adhesion of existing coatings at high humidity or extremely low temperatures. The increased problem improves the hydrophobicity and aging resistance of the coating, and achieves high-efficiency and low-energy-consuming anti-ice effect.

CN118546608BActive Publication Date: 2024-11-29ANHUI HACHUAN NEW MATERIAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410676412.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-29
Publication Date
2024-11-29
Estimated Expiration
2044-05-29

AI Technical Summary

Technical Problem

The existing anti-ice coating has increased the adhesion of ice at high humidity or extremely low temperatures, making it difficult to remove, and has poor UV aging resistance and limited service life. The traditional deicing method has high energy consumption and high cost, and the equipment is complex.

Method used

Hydrophobic nanosilica particles with different particle sizes were prepared by curved surface response method, and combined with rare earth oxides and low-surface energy organic polymers to form a dimming, heat preservation, ultraviolet-resistant anti-ice coating, which absorbs ultraviolet through rare earth elements. Light is converted into visible light, improving the hydrophobicity and warming effect of the coating.

Benefits of technology

It significantly improves the hydrophobic angle and aging resistance of the coating, reduces the adhesion and melting time of the ice layer, enhances the anti-ice performance and service life of the coating, and reduces energy consumption and equipment complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004864216150000061
    Figure BDA0004864216150000061
  • Figure BDA0004864216150000071
    Figure BDA0004864216150000071
Patent Text Reader

Abstract

A dimming warming UV-resistant anti-icing coating and a method for preparing the coating belong to the field of anti-icing coatings. The present invention aims to solve the problem of ice layers that are still difficult to remove at high humidity or extremely low temperatures. The present invention uses a surface response method to control the particle size of synthesized nano-silica, and then builds a micro-nano structure, so that the hydrophobicity of the coating is greatly improved, and (3,3,3-trifluoropropyl) trimethoxysilane is used to hydrophobically modify the nano-silica. Lutetium, terbium, and europium rare earth elements can be used to adjust ultraviolet light and convert it into beneficial light, which greatly improves the transmittance and utilization rate of sunlight, is conducive to improving the warming effect of the coating, and reduces the adhesion of ice on the coating and the melting of ice. Using 2-fluoro-pyridine carboxylic acid as a coordination acid can not only make rare earth elements generate organic rare earth complexes, increase compatibility with silicon fluoride organic film-forming materials, but also introduce fluoride ions to increase the hydrophobic effect. The present invention is used for dimming warming UV-resistant anti-icing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of anti-icing coatings, and specifically, relates to a dimming temperature-increasing UV-resistant anti-icing coating and a preparation method thereof, and a preparation method of a dimming temperature-increasing UV-resistant anti-icing coating. Background Art

[0002] In some cold regions or when the temperature is low in winter, ice will accumulate on the surface of the transmission line, which will seriously endanger the safety of the transmission line; in the extremely low temperature environment of the polar region, the ship is seriously covered with ice, which leads to the increase of ship weight, the reduction of residual buoyancy and capsizing; the problem of ice on the surface of the aircraft is even more fatal. The accumulation of ice on the outer surface of the aircraft will cause the original aerodynamic shape of the aircraft to be destroyed, and even cause the aircraft sensor to fail. In recent years, researchers have developed a variety of ice monitoring methods and anti-icing / de-icing technologies, such as ice monitoring sensors, thermal de-icing, mechanical de-icing and liquid anti-icing, etc., but these technologies are faced with the constraints of complex equipment, environmentally unfriendly liquid recovery and treatment, low de-icing efficiency, and high energy consumption. The anti-icing surface can delay the appearance of ice or reduce the adhesion of ice by adjusting the properties of the material itself, which can solve the problems of high energy consumption, high cost or complex external equipment of traditional de-icing methods. The construction and maintenance are simple and convenient, and the efficiency is high.

[0003] CN 117903665 A Preparation method of photothermal super-hydrophobic anti-icing and deicing composite coating, discloses a preparation method of photothermal super-hydrophobic anti-icing and deicing composite coating, the prepared mesoporous silica nanospheres are modified, then compounded with photothermal materials and photosensitive materials (organic photosensitive materials such as crystal violet lactone), and then mixed with organic solvents to make coating slurry, and then add thermosetting resin (epoxy, phenolic, alkyd resin) and curing agent, and thermal spray curing (spraying temperature is 200-300℃, curing temperature is 50-150℃, curing time is 30-60min), that is, photothermal super-hydrophobic anti-icing and deicing composite coating is obtained. However, the thermosetting resin selected for the coating has poor UV aging resistance, which affects the service life of the coating; the hydrophobic effect needs to be further improved, and the construction method and curing method need to be heated, which has certain restrictions on the use conditions.

[0004] CN 117264493 A Anti-icing coating with photothermal effect and fan blade, discloses a preparation method of an anti-icing coating with photothermal effect, a surface layer formed by a hydrogel component, a hydrophobic polymer component and photothermal micro-nano particles, the photothermal micro-nano particles are composite particles of ferroferric oxide particles and nano-silicon dioxide particles, and the nano-silicon dioxide particles are coated on the surface of the ferroferric oxide particles. However, the zwitterionic hydrogel contains more hydrophilic sites, so that the water resistance of the coating is poor, and it is not suitable for applications with high requirements for corrosion resistance.

[0005] CN 115160857 A A kind of passive photothermal deicing super-hydrophobic anti-icing coating and its preparation method and application, disclose a kind of passive photothermal deicing super-hydrophobic anti-icing coating and its preparation method, use ethyl cellulose, hollow porous carbon fiber derived from ZIF-8 and sodium chloride and anhydrous ethanol as the bottom layer, fluorinated silicon dioxide and ethyl acetate as the surface layer, wait for natural drying and curing to obtain the passive photothermal deicing super-hydrophobic anti-icing coating. Sodium chloride can reduce the freezing point of water droplets, increase the contact angle of the coating, thereby improving the anti-icing performance of the coating surface, and the hollow porous carbon fiber derived from ZIF-8 has excellent photothermal conversion performance, can accelerate the temperature rise of the coating surface, and then accelerate the deicing of the coating. However, although sodium chloride can reduce the freezing point of water droplets in the bottom layer, it will corrode the metal substrate; although fluorinated silicon dioxide and ethyl acetate can be used as the surface layer to achieve a super-hydrophobic effect, the corrosion resistance and long-term effect of the coating cannot be guaranteed.

[0006] Although super-hydrophobic surfaces have a good anti-icing effect within a certain temperature range, at high humidity or extremely low temperatures, the air in the microstructure of the super-hydrophobic coating surface is replaced by tiny ice crystals, which causes a sharp increase in ice adhesion, making the ice layer still difficult to remove. At present, the research direction of anti-icing coatings is mainly focused on using polymers and fillers to construct super-hydrophobic surfaces. The anti-icing principle is single, the long-term effect is poor, the deicing rate is not high, and ice layers that are difficult to remove are still produced at high humidity or extremely low temperatures. Summary of the invention

[0007] The present invention improves the super-hydrophobic property of the coating as much as possible and introduces rare earth elements to achieve selective transmission of light, fully utilize solar energy, and achieve good warming and heat preservation effects; the rare earth can also absorb ultraviolet light and convert it into visible light, thereby increasing light transmittance and achieving good warming effects.

[0008] The method of the present invention uses organic carboxylic acid as a ligand to react with a rare earth compound to synthesize a rare earth complex; the complex is hydrophobically modified; hydrophobic nano-silica with different particle sizes is prepared by a surface response method; two functional fillers are compounded with a low surface energy organic polymer to prepare an anti-icing coating with dimming, heat preservation, UV resistance and super hydrophobicity.

[0009] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0010] The object of the present invention is to provide a method for preparing a dimming temperature-increasing UV-resistant anti-icing coating, comprising the following steps:

[0011] Step 1, based on the surface response method, hydrophobic nano-SiO2 particles with particle sizes of 100 nm, 400 nm, and 700 nm were prepared respectively with optimal parameters, and then all of them were modified with (3,3,3-trifluoropropyl)trimethoxysilane;

[0012] Step 2: Dissolve the rare earth oxide Re2O3 in hydrochloric acid and stir magnetically for at least 30 minutes to obtain a salt solution of the rare earth element. At the same time, react 2-fluoro-pyridinecarboxylic acid with sodium bicarbonate to generate L 2+ Ionic solution, the above two solutions are reacted at 50°C with magnetic stirring for at least 1h, then separated by high-speed centrifugal filtration, washed with anhydrous ethanol for several times, and dried to obtain Re2L3;

[0013] Step 3, take fluorinated silicone resin and butyl acetate, disperse at high speed for 5 minutes, then add BYK163 dispersant, disperse for 5 minutes, then add 100nm, 400nm and 700nm hydrophobic nano-SiO2 particles, disperse at high speed for 20 minutes, then add Re2L3, titanium dioxide, barium sulfate, aluminum oxide, BYK066 defoamer and silane coupling agent, disperse at high speed for 40 minutes, filter, and obtain a dimming temperature-increasing UV-resistant anti-icing coating;

[0014] Wherein, the Re in step 2 is lutetium, terbium or europium.

[0015] It is further defined that 100nm, 400nm and 700nm hydrophobic nano-SiO2 particles can be mixed in proportion and added in batches, one particle size can be added before another particle size, different particle sizes can be added in any order, and each particle size can be added multiple times.

[0016] To further define, the process of step one is as follows:

[0017] After mixing anhydrous ethanol with a certain amount of NH3·H2O, the mixture was evenly mixed under magnetic stirring at 50°C; ethyl orthosilicate was slowly added dropwise, and the magnetic stirring was continued for 3 hours to obtain hydrophilic nano-SiO2 particles;

[0018] Slowly drop a certain amount of (3,3,3-trifluoropropyl)trimethoxysilane and an organic tin catalyst, continue magnetic stirring for 3 hours; centrifuge at high speed, wash with anhydrous ethanol for many times, and dry at 70°C for 24 hours to obtain nano-SiO2 particles.

[0019] Further defined, the preferred parameters for the hydrophobic nano-SiO2 particles with a particle size of 100 nm are: reaction temperature 50°C, ethanol concentration 13M, pH value 12, and ethyl orthosilicate concentration 0.4M.

[0020] Further defined, the preferred parameters for the hydrophobic nano-SiO2 particle size of 400nm are: reaction temperature 50°C, ethanol concentration 9M, pH value 12.5, and ethyl orthosilicate concentration 0.4M.

[0021] Further defined, the preferred parameters for the hydrophobic nano-SiO2 particle size of 700nm are: reaction temperature 50°C, ethanol concentration 9M, pH value 13, and ethyl orthosilicate concentration 0.7M.

[0022] Further defined, in step 2, 50 g of rare earth oxide Re2O3 is dissolved in 100 ml of hydrochloric acid with a mass percent concentration of 10%; 50 ml of 2-fluoro-pyridinecarboxylic acid is reacted with 20 g of sodium bicarbonate.

[0023] It is further defined as 40g of fluorinated silicone resin, 15g of butyl acetate, 1g of 100nm hydrophobic nano-SiO2 particles, 0.5g of 400nm hydrophobic nano-SiO2 particles, 0.8g of 700nm hydrophobic nano-SiO2 particles, 20g of Re2L3, 2g of titanium dioxide, 5g of barium sulfate, 10g of aluminum oxide, 0.5g of BYK066 defoaming agent, and 1g of silane coupling agent.

[0024] Further defined, step 2 is drying at 70° C. for 24 h.

[0025] The object of the present invention is to provide a coating prepared by any of the above methods.

[0026] The object of the present invention is to provide a dimming temperature-increasing UV-resistant anti-icing coating, characterized in that the coating is obtained by spraying a coating prepared by any of the above-mentioned methods on the surface of a substrate and standing and curing at room temperature for 30 minutes.

[0027] The present invention uses a surface response method to prepare hydrophobic nano-SiO2 particles of different sizes (100nm, 400nm and 700nm) under optimal conditions, and adds three kinds of nano-SiO2 particles in proportion to build a micro-nano structure, and the hydrophobic surface with an undulating structure is constructed, which greatly increases the amount of air pockets between particles, so that the hydrophobic angle of the coating is significantly improved. And by using the -OH on the surface of siloxane to easily condense with a large amount of -OH on the surface of the nano-SiO2 particles, the hydrophobicity of the hydrophobic nano-SiO2 particles can be achieved, and the hydrophobicity of the coating is greatly improved after the addition.

[0028] The coating prepared by adding the rare earth dimming complex in the present invention can selectively transmit light, can fully utilize the solar energy, and the coating has good warming and heat preservation effects; the rare earth dimming complex can also absorb ultraviolet light and convert ultraviolet light into visible light, and the light transmittance is increased, which not only improves the aging resistance of the coating, but also improves the warming effect of the coating.

[0029] This is because the ultraviolet light with a wavelength of 290-400nm in the sunlight reaching the ground through the atmosphere has a strong photo-oxidative damage effect on polymers. The present invention adjusts it into beneficial light of other wavelengths to improve the utilization rate of solar energy.

[0030] The three rare earth compounds of lutetium, terbium and europium have different electronic layer structures. When exposed to ultraviolet light, they produce transitions of different energy levels, and respectively stimulate blue light with a wavelength of 435-480nm, green light with a wavelength of 500-560nm, and red light with a wavelength of 610-700nm. This greatly improves the utilization rate of light, converts ultraviolet light that is harmful to the organic coating into visible light, improves the aging resistance of the coating and the warming effect of the coating, and is more conducive to reducing the adhesion and melting of ice on the coating. The addition of the rare earth organic dimming complex of the present invention allows the coating to automatically adjust solar energy, maximize the photothermal effect of sunlight, and greatly accelerate the melting and shedding process of the ice layer on the surface of the composite coating under irradiation. And the ultraviolet conversion greatly improves the aging resistance of the coating.

[0031] The present invention adopts 2-fluoro-pyridinecarboxylic acid as the coordination acid, which can not only make the rare earth element generate an organic rare earth complex to increase the compatibility with the silicon fluoride organic film-forming material, but also introduce fluorine ions to increase the hydrophobic effect.

[0032] The hydrophobic angle of the coating prepared by the method of the present invention is greatly improved (the hydrophobic angle reaches more than 160°), and the rolling angle is greatly reduced (less than 5°), that is, the hydrophobic effect of the coating is greatly improved, which makes it difficult for water to adhere to the coating, and the possibility of ice coating is greatly reduced or ice formation is delayed;

[0033] Under the combined effect of the photothermal performance and low surface free energy of the coating, the ice layer on the surface of the coating can fall off from the surface of the coating in just a few seconds when irradiated. DETAILED DESCRIPTION

[0034] The present invention will be described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, and do not limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.

[0035] Example 1: In this embodiment, the preparation method of the dimming temperature-increasing UV-resistant anti-icing coating and the coating is achieved by the following steps:

[0036] The preparation of hydrophobic nano-silica with different particle sizes is specifically carried out as follows: anhydrous ethanol and a certain amount of NH3·H2O are mixed and placed in a conical flask, and magnetically stirred at 50°C for uniform mixing; ethyl orthosilicate is slowly dripped into the mixture, and magnetic stirring is continued for 3 hours to obtain hydrophilic nano-SiO2 particles; a certain amount of (3,3,3-trifluoropropyl)trimethoxysilane and an organic tin catalyst are slowly dripped into the mixture obtained above, and magnetic stirring is continued for 3 hours; the mixture obtained by the reaction is centrifuged at high speed, washed with anhydrous ethanol for multiple times, and dried in an oven at 70°C for 24 hours to obtain hydrophobic nano-SiO2 particles with different particle sizes;

[0037] Based on the surface response method, hydrophobic nano-SiO2 particles with particle sizes of 100nm, 400nm, and 700nm were prepared respectively with optimal parameters. The specific steps are as follows:

[0038] 1. Use single-factor experiments to determine the influencing factors and their levels. The factors are reaction temperature, ethanol concentration, pH value, and ethyl orthosilicate concentration. The control variable method is used to study the influence of single factors on the final particle size, and select the appropriate variable range to design the surface response method experiment.

[0039] 2. Experiments have shown that the size of silica microspheres is negatively correlated with the reaction temperature. The higher the reaction temperature, the smaller the particle size. The size of silica microspheres is also negatively correlated with the concentration of anhydrous ethanol. The higher the ethanol concentration, the smaller the particle size. However, the size of silica microspheres is not linearly related to the pH value. The particle size first increases and then slowly decreases with the increase of pH value. The size of silica microspheres is positively correlated with the concentration of ethyl orthosilicate. The higher the concentration, the larger the particle size.

[0040] 3. Based on the single-factor experiment, a four-factor three-level experiment was designed, with the intention of establishing a model between the response value and the four factors to synthesize silica microspheres of a specific size. The four factors of reaction temperature, ethanol concentration, pH value, and ethyl orthosilicate concentration were used as independent variables, represented by X1, X2, X3, and X4 respectively. Each factor took three levels, coded as -1, 0, and +1, and the particle size of silica microspheres was used as the response value to design the experiment.

[0041] 4. According to the Box-Behnken (BBD) model experimental design, X1 values ​​30℃, 50℃, and 70℃ correspond to levels -1, 0, and +1 respectively; X2 values ​​8M, 11M, and 14M correspond to levels -1, 0, and +1 respectively; X3 values ​​12.6, 12.9, and 13.2 correspond to levels -1, 0, and +1 respectively; X4 values ​​0.35M, 0.55M, and 0.75M correspond to levels -1, 0, and +1 respectively.

[0042] 5. The quadratic regression fitting analysis was performed using Design-Expert.V8.0 software to obtain the quadratic multiple regression equation of the model. After optimization, based on the optimization fitting results, the significance ranking of the effects of various factors on particle size was obtained: anhydrous ethanol concentration > reaction temperature > pH value > interaction between anhydrous ethanol concentration and TEOS concentration > TEOS concentration.

[0043] 6. Using Design-Expert.V8.0 software, select three particle sizes that you want to synthesize and obtain the corresponding optimal synthesis parameter conditions.

[0044] 100nm: reaction temperature 50℃, ethanol concentration 13M, pH 12, ethyl orthosilicate concentration 0.4M;

[0045] 400nm: reaction temperature 50℃, ethanol concentration 9M, pH 12.5, ethyl orthosilicate concentration 0.4M

[0046] 700nm: reaction temperature 50℃, ethanol concentration 9M, pH 13, ethyl orthosilicate concentration 0.7M.

[0047] The hydrophobic nano-SiO2 particles with different particle sizes were prepared with the preferred parameters, and the specific steps were as follows: 50 ml of anhydrous ethanol and 2 g of NH3·H2O were mixed and placed in a conical flask, and magnetically stirred at 50°C for uniform mixing; 40 ml of ethyl orthosilicate was slowly dripped in, and magnetic stirring was continued for 3 hours to obtain hydrophilic nano-SiO2 particles; 5 g of (3,3,3-trifluoropropyl)trimethoxysilane and 1 g of an organic tin catalyst were slowly dripped into the above-obtained mixed solution, and magnetic stirring was continued for 3 hours; the obtained mixed solution was centrifuged at 4000 r / min, washed with anhydrous ethanol for many times, and dried in an oven at 70°C for 24 hours to obtain hydrophobic nano-SiO2 particles with a particle size of 100 nm;

[0048] Mix 40 ml of anhydrous ethanol and 3 g of NH3·H2O and place in a conical flask, stir magnetically at 50°C to mix evenly; slowly drop 40 ml of ethyl orthosilicate, continue magnetic stirring for 3 hours to obtain hydrophilic nano-SiO2 particles; slowly drop 5 g of (3,3,3-trifluoropropyl)trimethoxysilane and 1 g of organic tin catalyst into the above-obtained mixed solution, continue magnetic stirring for 3 hours; centrifuge the obtained mixed solution at 4000 r / min, wash with anhydrous ethanol several times, and dry in a 70°C oven for 24 hours to obtain hydrophobic nano-SiO2 particles with a particle size of 400 nm;

[0049] 40 ml of anhydrous ethanol and 4 g of NH3·H2O were mixed and placed in a conical flask, and magnetically stirred at 50°C to mix evenly; 70 ml of ethyl orthosilicate was slowly dripped in, and magnetic stirring was continued for 3 hours to obtain hydrophilic nano-SiO2 particles; 5 g of (3,3,3-trifluoropropyl)trimethoxysilane and 1 g of organic tin catalyst were slowly dripped into the above-obtained mixed solution, and magnetic stirring was continued for 3 hours; the obtained mixed solution was centrifuged at 4000 r / min, washed with anhydrous ethanol for many times, and dried in a 70°C oven for 24 hours to obtain hydrophobic nano-SiO2 particles with a particle size of 700 nm;

[0050] Preparation method of rare earth organic dimming complex:

[0051] 50g of lutetium oxide was dissolved in 100ml of 10% (mass) hydrochloric acid, and magnetically stirred at 800rpm for 30min to obtain a salt solution of lutetium element; 50ml of 2-fluoro-pyridinecarboxylic acid was reacted with 20g of sodium bicarbonate to generate an organic acid ion solution, and the above two solutions were magnetically stirred at 1000rpm for 1h at 50°C, and the reaction mixture was separated by high-speed centrifugation at 3500rpm, washed with anhydrous ethanol for multiple times, and dried in an oven at 70°C for 24h to obtain 2-fluoro-pyridinecarboxylic acid lutetium dimming complex;

[0052] Preparation of composite coatings:

[0053] Weigh 40g of fluorinated silicone resin and 15g of butyl acetate solvent, disperse them at a high speed of 800rpm for 5min, then add 2g of BYK163 dispersant and disperse them for another 5min; gradually add 1g, 0.5g and 0.8g of 100nm / 400nm / 700nm hydrophobic nano-SiO2 particles respectively, and disperse them at a high speed of 1200rpm for 20min; add 20g of lutetium 2-fluoro-pyridinecarboxylate dimming complex, 2g of titanium dioxide, 5g of barium sulfate, 10g of aluminum oxide, 0.5g of BYK066 defoamer and 1g of silane coupling agent, disperse them at a high speed of 800rpm for 40min, and obtain the dimming warming UV-resistant anti-icing coating after filtration.

[0054] Preparation of dimming temperature-increasing UV-resistant anti-icing coating:

[0055] The prepared coating was evenly sprayed on the surface of the pretreated tinplate sheet using a manual spray gun and allowed to stand and cure at room temperature for 30 minutes to obtain a dimming, warming, UV-resistant and anti-icing coating.

[0056] After 24 hours of complete curing, the coating performance can be tested

[0057] Hydrophobic angle: 169.5°

[0058] Roll angle: 2°

[0059] Anti-icing effect: At -15℃, it takes only 12s for water droplets to completely freeze on the surface of tinplate, and 240s for water droplets to completely freeze on the anti-icing coating, which has an excellent delayed icing effect.

[0060] Warming effect: The initial temperature of the coating surface was 25°C, and after 1 minute of irradiation, its surface temperature rose to 45°C; after 30 minutes of irradiation, the surface temperature of the composite coating reached 56°C, which shows that the dimming temperature-increasing UV-resistant anti-icing coating has a good warming effect.

[0061] Deicing effect: It takes 95 seconds for ice drops to melt and roll down on the surface of tinplate sheets, and only 9 seconds for ice drops to melt and roll down on the dimming temperature-increasing UV-resistant anti-icing coating.

[0062] Table 1 Effect of different particle sizes of hydrophobic nano-silica on the hydrophobic angle

[0063]

[0064]

[0065] The above describes the specific embodiments of the present invention. It should be noted that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various modifications or variations within the scope of the claims, which does not affect the essential content of the present invention.

Claims

1. A method for preparing a dimming temperature-increasing UV-resistant anti-icing coating, It is characterized in that The following steps are involved: Step 1: Based on the surface response method, hydrophilic nano-SiO with particle sizes of 100 nm, 400 nm, and 700 nm were prepared respectively. 2 The particles were then all modified using (3,3,3-trifluoropropyl)trimethoxysilane; Step 2: Rare earth oxide Re 2 O 3 Dissolve in hydrochloric acid and stir magnetically for at least 30 minutes to obtain a salt solution of rare earth elements. At the same time, react 2-fluoro-pyridinecarboxylic acid with sodium bicarbonate to generate L 2+ The above two solutions are reacted at 50°C with magnetic stirring for at least 1 hour, and then separated by high-speed centrifugation, washed with anhydrous ethanol for several times, and dried to obtain Re 2 L 3 ; Step 3: Take fluorinated silicone resin and butyl acetate, disperse at high speed for 5 minutes, then add BYK163 dispersant, disperse for 5 minutes, and then add 100nm, 400nm and 700nm hydrophobic nano-SiO 2 Particles, disperse at high speed for 20 minutes, then add Re 2 L 3 , titanium dioxide, barium sulfate, aluminum oxide, BYK066 defoamer and silane coupling agent, disperse at high speed for 40 minutes, and filter to obtain a dimming temperature-increasing UV-resistant anti-icing coating; Wherein, the Re in step 2 is lutetium, terbium or europium.

2. The preparation method according to claim 1, It is characterized in that The process of step one is as follows: Ethanol and a certain amount of NH 3 ·H 2 O was mixed, and then magnetic stirring was performed at 50°C to mix evenly. Ethyl orthosilicate was slowly added dropwise, and magnetic stirring was continued for 3 h to obtain hydrophilic nano-SiO 2 particle; Slowly add a certain amount of (3,3,3-trifluoropropyl)trimethoxysilane and organic tin catalyst, continue magnetic stirring for 3 hours, centrifuge at high speed, wash with anhydrous ethanol for many times, and dry at 70 °C for 24 hours to obtain nano-SiO 2 particle.

3. The preparation method according to claim 2, It is characterized in that Hydrophilic Nano-SiO 2 Parameters for particle size of 100 nm: reaction temperature 50°C, ethanol concentration 13M, pH 12, and ethyl orthosilicate concentration 0.4M.

4. The preparation method according to claim 2, It is characterized in that Hydrophilic Nano-SiO 2 Parameters for particle size of 400 nm: reaction temperature 50°C, ethanol concentration 9M, pH 12.5, and ethyl orthosilicate concentration 0.4M.

5. The preparation method according to claim 2, It is characterized in that Hydrophilic Nano-SiO 2 Parameters for particle size of 700 nm: reaction temperature 50°C, ethanol concentration 9M, pH 13, and ethyl orthosilicate concentration 0.7M.

6. The preparation method according to claim 1, It is characterized in that Step 2: 50g rare earth oxide Re 2 O 3 Dissolve in 100ml of 10% hydrochloric acid; react 50ml of 2-fluoro-pyridinecarboxylic acid with 20g of sodium bicarbonate.

7. The preparation method according to claim 4, It is characterized in that 40g fluorinated silicone resin, 15g butyl acetate, 100nm hydrophobic nano-SiO 2 Particles 1g, 400nm hydrophobic nano-SiO 2 Particles 0.5g, 700nm hydrophobic nano-SiO 2 Particle 0.8g, Re 2 L 3 20g, titanium dioxide 2g, barium sulfate 5g, aluminum oxide 10g, BYK066 defoamer 0.5g, silane coupling agent 1g.

8. The preparation method according to claim 1, It is characterized in that In step 2, the mixture was dried at 70 °C for 24 h.

9. A coating prepared by the method according to any one of claims 1 to 8.

10. A dimming temperature-increasing UV-resistant anti-icing coating, It is characterized in that The coating is obtained by spraying the coating prepared by the method according to any one of claims 1 to 8 onto the surface of a substrate and curing it at room temperature for 30 minutes.

Citation Information

Patent Citations

  • Anti-icing coating with photothermal effect and fan blade

    CN117264493A

  • Preparation method of photo-thermal super-hydrophobic anti-icing and deicing composite coating

    CN117903665A

  • Europium-complex modified fluorosilicone acrylate luminous agent and preparation method thereof

    CN103319643A

  • Super-hydrophobic coating with anti-icing function and preparation method thereof

    CN114773996A