A method for preparing anti-reflective hard glass

By forming an anti-reflective layer on the glass surface and performing superhydrophilic modification, the problems of optical illusions and poor self-cleaning effects at night have been solved, achieving multi-level reflection to consume light and automatic cleaning effects.

CN118598543BActive Publication Date: 2026-11-17张敏
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410480347.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-29
Publication Date
2026-11-17
Estimated Expiration
2042-06-29

AI Technical Summary

Technical Problem

Existing glass is prone to creating optical illusions when driving at night, affecting the driver's visibility, and its self-cleaning effect is poor. Existing coatings also lack adhesion and hydrophilicity.

Method used

The glass surface is sequentially treated with spraying, secondary drying, sputtering, and deposition to form an anti-reflective layer. Then, a superhydrophilic modification treatment is performed, including spraying calcium chloride solution, ammonium bicarbonate solution, and ammonia water, microwave drying, sputtering of silicon dioxide, deposition of titanium tetrachloride, and superhydrophilic modification.

Benefits of technology

It achieves anti-reflective and self-cleaning effects, consumes light through multi-level reflection to improve the clarity of the driver's vision, and automatically removes contaminants through super-hydrophilicity to enhance the glass's self-cleaning ability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for preparing anti-reflective hard glass, relating to the field of glass technology. The method involves first spraying a calcium carbonate precursor onto molten glass, followed by secondary drying to form calcium carbonate-glass core-shell structured particles; then pressing and molding, followed by sputtering to form a porous, low-refractive-index silica layer; next, grafting titanium tetrachloride onto the silica surface and foaming it with glycerol at high temperature to form a foam structure, high-refractive-index layer, thus obtaining an anti-reflective layer with alternating high and low refractive indices; finally, modifying the anti-reflective layer with (chloromethyl)methyldiethoxysilane, pentahydroxyhexanal, 2,2-di(hydroxymethyl)propionic acid, and lysine diisocyanate to make the glass superhydrophilic and self-cleaning. The glass prepared by this invention exhibits both anti-reflective and self-cleaning properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of glass technology, specifically to a method for preparing anti-reflective hard glass. Background Technology

[0002] Glass, being hard and durable, is used in various fields, such as automobiles, electronics, and construction. Currently, car windshields are generally installed at an angle. When driving at night, if interior lights are on or a car behind illuminates the interior, light from people or objects inside the car can be reflected in the windshield as a virtual image, making it difficult for the driver to distinguish between people or objects and the images inside the car. This can easily lead to illusions and accidents. Furthermore, in strong sunlight on sunny days, it can also impair the driver's visibility. Current industrial production methods involve coating the glass surface with a thin film of silica, which has limited gain and weak interfacial adhesion.

[0003] In addition, glass has a relatively high surface activity, making it easy to attract dust and affecting the driver's vision. It requires manual cleaning to keep the car windows clean. Therefore, self-cleaning glass has begun to appear on the market. It mainly uses a coating method to cover the surface with a layer of hydrophilic organic film. However, the adhesion and repeatability of the film to the glass substrate are not high, and the hydrophilicity of the glass surface is not high, resulting in poor self-cleaning effect. Summary of the Invention

[0004] The purpose of this invention is to provide a method for preparing anti-reflective hard glass to solve the problems existing in the prior art.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution: an anti-reflective hard glass, wherein the anti-reflective hard glass comprises the following preparation method, wherein a spraying treatment, a secondary drying treatment, a sputtering treatment and a deposition treatment are sequentially performed on the surface of molten glass to form an anti-reflective layer, and a superhydrophilic modification treatment is performed.

[0006] Furthermore, the spraying process involves sequentially spraying calcium chloride solution, ammonium bicarbonate solution, and ammonia water onto the molten glass, followed by ultrasonic vibration for a period of time to obtain pretreated molten glass.

[0007] Furthermore, the secondary drying process involves heating the pretreated molten glass to a predetermined temperature under microwave conditions, holding it at that temperature, continuing to heat and hold it, then vacuuming, heating and holding it, and finally cooling and holding it to obtain the first dried material. The first dried material is then further dried to obtain glass powder, which is then pressed into shape to obtain glass sheets.

[0008] Furthermore, the sputtering process involves using pure silicon as the target material, sputtering it onto a glass sheet for a period of time in a mixed atmosphere of argon and oxygen, followed by high-temperature heat treatment to obtain a silicon dioxide glass substrate.

[0009] Furthermore, the deposition process involves pretreating silica glass with 3-aminopropylmethoxysilane to obtain a pretreated glass substrate; mixing the pretreated glass substrate, triethylamine, and acetonitrile, adding titanium tetrachloride acetonitrile solution under ice bath conditions, raising the temperature to room temperature, reacting for a period of time, removing the substrate, adding glycerol, hexamethylenetetramine, and butanol, treating with high-temperature ultrasonication, and then calcining to obtain the antireflective glass layer.

[0010] Furthermore, the superhydrophilic modification process involves pretreating the antireflective glass with (chloromethyl)methyldiethoxysilane to obtain a glass precursor; mixing the glass precursor, pentahydroxyhexanal, toluene, glacial acetic acid, and piperidine, and then ultrasonically reacting it under nitrogen protection. After the reaction, the precursor is removed, washed, and then mixed with sodium carbonate, trifluoroethanol, and 2,2-di(hydroxymethyl)propionic acid, and ultrasonically reacted again. After the reaction, the precursor is removed, washed, and the modified precursor is obtained. The modified precursor, lysine diisocyanate, and acetone are mixed, reacted at a constant temperature, cooled, and then isopropanol is added. After ultrasonic oscillation, deionized water is added, and the mixture is ultrasonically oscillated at a high frequency. The mixture is then removed and dried.

[0011] Furthermore, a method for preparing anti-reflective hard glass includes the following preparation steps: (1) Pour the molten glass into a glass mold, and spray calcium chloride solution, ammonium bicarbonate solution and ammonia water in sequence according to the mass ratio of 1:0.7:0.1~1:1.0:0.3. The mass ratio of ammonium bicarbonate to deionized water in the ammonium bicarbonate solution is 1:10, and the mass ratio of calcium chloride solution to molten glass is 0.1:1~0.3:1. Vibrate at 30~40kHz for 20~36min to obtain pretreated molten glass; (2) Under microwaves of 400~600W, the pretreated molten glass is heated to 70~85℃ and held for 20~38min. Then it is heated to 85~96℃ and held for 22~36min. After that, the vacuum is evacuated to a vacuum degree of 70~80kPa. The glass is then heated to 92~104℃ and held for 34~44min. Finally, it is cooled to 65~75℃ and held for 3~8h to obtain the first dried material. (3) The first drying material is dried at 80~90℃ for 12~18h to obtain glass powder, which is then pressed into glass sheets at 3~5MPa and 150~160℃. (4) Place the glass slide in the container and evacuate to a vacuum level of 2.0 × 10⁻⁶. -4 ~8.0×10 -4 Pa, using pure silicon as the target material, with a distance of 100~130mm, high-purity argon and oxygen are introduced at a flow ratio of 4:1 to a pressure of 0.5~1Pa, sputtered at 35~45W for 10~18min, heated to 800~850℃, and reacted for 100~128min to obtain a silicon dioxide glass matrix; (5) Mix the pretreated glass substrate, triethylamine, and acetonitrile in a mass ratio of 1:0.7:64 to 1:1.0:74. In an ice bath, add a titanium tetrachloride acetonitrile solution with a mass ratio of 20 to 28 times the mass of the pretreated glass substrate. The mass ratio of titanium tetrachloride to acetonitrile in the titanium tetrachloride acetonitrile solution is 1:29 to 1:36. Raise to room temperature and react for 22 to 26 hours. Remove the mixture and add glycerol, hexamethylenetetramine, and butanol in a mass ratio of 1:0.5:0.4 to 1:0.8:0.6. The mass ratio of glycerol to silica glass substrate is 0.8:1 to 1.2:1. Treat at 400 to 420°C and 30 to 40 kHz for 3 to 10 minutes. Then calcine at 450 to 468°C for 1.5 to 3 hours to obtain the antireflective glass layer. (6) Mix glass raw material, pentahydroxyhexanol, toluene, glacial acetic acid and piperidine in a mass ratio of 1:0.3:0.6:0.02:0.04~1:0.5:1.0:0.05:0.07. Under nitrogen protection, sonicate at 30~40kHz for 6~9h. Remove the mixture and wash it with petroleum ether and anhydrous ethanol 4~8 times in sequence. Then mix it with sodium carbonate, trifluoroethanol and 2,2-di(hydroxymethyl)propionic acid in a mass ratio of 1:0.0002:2:0.2~1:0.0005:8:0.5. Continue to sonicate at 40~50℃ for 2~4h. Remove the mixture and wash it with ethyl acetate 3~6 times to obtain the modified precursor. (7) Mix the modified precursor, lysine diisocyanate and acetone in a mass ratio of 1:0.5:18~1:0.9:26, keep warm at 76~85℃ for 2~4h, cool down to 40~50℃, add isopropanol at 0.5~2.8 times the mass of the modified precursor, sonicate at 25~35kHz for 26~40min, add deionized water at 3~7 times the mass of the modified precursor, sonicate at 40~50kHz for 18~38min, take out and dry at room temperature for 15~20h to obtain anti-reflective hard glass.

[0012] Further, the preparation method of the calcium chloride solution in step (1) is as follows: dissolve calcium chloride in 3 to 5 times the mass of calcium chloride in deionized water, filter, add ammonia water until the pH of the solution is 11 to 12, stir at 30 to 40°C and 40 to 60 rpm for 20 to 34 minutes, add 0.01 to 0.04 times the mass of calcium chloride in calcium oxide and 0.0005 to 0.0009 times the mass of calcium chloride in hydrogen peroxide, continue stirring for 30 to 42 minutes, and filter.

[0013] Further, the preparation method of the pretreated glass substrate in step (5) is as follows: the silica glass substrate is immersed in a 3-aminopropylmethoxysilane solution with a mass ratio of 4 to 8 times that of the silica glass substrate, the mass ratio of 3-aminopropylmethoxysilane to deionized water in the 3-aminopropylmethoxysilane solution is 1:25 to 1:50, glacial acetic acid is added until the pH of the solution is 4 to 5, the reaction is carried out for 4 to 7 hours, the substrate is taken out and washed with deionized water for 3 to 5 minutes.

[0014] Further, the preparation method of the glass raw material in step (6) is as follows: anti-reflective glass, (chloromethyl)methyldiethoxysilane and deionized water are mixed in a mass ratio of 1:0.2:18~1:0.5:24, reacted at 50~64℃ and 30~40kHz for 1.5~3h, taken out and washed with deionized water for 3~6min.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The present invention involves sequentially spraying, drying, sputtering, and depositing a coating onto the surface of molten glass to form an anti-reflective layer, followed by superhydrophilic modification to achieve anti-reflective and self-cleaning effects.

[0016] First, this invention uses molten glass as raw material. Calcium chloride and ammonium bicarbonate are sprayed sequentially, followed by a first drying treatment. Microwave-assisted gradient heating accelerates liquid evaporation, forming calcium carbonate particles that adhere to the glass surface using the adhesive properties of the molten glass. A second drying treatment solidifies the molten glass, forming a core-shell structured glass substrate. Next, a sputtering process is performed, sputtering silicon dioxide onto the glass substrate surface. Heating removes the calcium carbonate, and the escaping gas creates a porous silicon dioxide structure, forming a low-refractive-index layer. A deposition process is then performed, where titanium tetrachloride is grafted onto the silicon dioxide surface with a coupling agent and foamed with glycerol at high temperature, entangling the silicon dioxide pores to obtain a foamed titanium dioxide structure, forming a high-refractive-index layer. The alternation of high and low refractive indices gives the glass an anti-reflective effect. Furthermore, the tightly cross-linked composite layers and non-interconnected pores enhance multi-level reflection and dissipation of light, improving the glass's anti-reflective performance.

[0017] Secondly, this invention utilizes the silicon-oxygen bonds of (chloromethyl)methyldiethoxysilane grafted onto titanium dioxide, and then utilizes the methyl and chlorine atoms to react with the hydroxyl groups of pentahydroxyhexanal and 2,2-di(hydroxymethyl)propionic acid, respectively. Subsequently, the surface hydroxyl groups react with the isocyanate groups of lysine diisocyanate to form a superhydrophilic polymer, giving the glass a self-cleaning effect. At the same time, the inorganic antireflective layer is modified with superhydrophilicity, reducing the problems of traditional superhydrophilic treatment agents not adhering and easily failing after repeated use. In addition, titanium dioxide has a photocatalytic effect, and the combination of the two significantly improves the self-cleaning effect of the glass. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0019] To more clearly illustrate the method provided by the present invention, the following embodiments are provided in detail. The testing methods for various indicators of the anti-reflective hard glass produced in the following embodiments are as follows: Anti-reflective properties: The anti-reflective effect of the same thickness sample and the comparative sample was tested. The reflectance and transmittance of the sample were measured with a spectrophotometer.

[0020] Self-cleaning property: The hydrophilicity effect was tested on the same size of the example and the comparative example. The hydrophilic contact angle of the surface was measured with a contact angle meter. The water droplet volume was 1 μL. Each sample was measured 5 times and the average value was taken.

[0021] Example 1 (1) Dissolve calcium chloride in 3 times the mass of deionized water, filter, add ammonia to the solution pH 11, stir at 30℃ and 40 rpm for 20 min, add 0.01 times the mass of calcium chloride and 0.0005 times the mass of calcium chloride and hydrogen peroxide, continue stirring for 30 min, filter to obtain calcium chloride solution; pour molten glass into a glass mold, spray calcium chloride solution, ammonium bicarbonate solution and ammonia in sequence at a mass ratio of 1:0.7:0.1, the mass ratio of ammonium bicarbonate to deionized water in the ammonium bicarbonate solution is 1:10, the mass ratio of calcium chloride solution to molten glass is 0.1:1, shake at 30 kHz for 20 min to obtain pretreated molten glass; (2) Under 400W microwave, the pretreated molten glass is heated to 70°C and held for 20 minutes, then heated to 85°C and held for 22 minutes. After that, the vacuum is drawn to a vacuum degree of 70kPa, heated to 92°C and held for 34 minutes, then cooled to 65°C and held for 3 hours to obtain the first dried material. (3) The first drying material is dried at 80℃ for 12 hours to obtain glass powder, which is then pressed into glass sheets at 3MPa and 150℃. (4) Place the glass slide in the container and evacuate to a vacuum level of 2×10⁻⁶. -4 Pa, using pure silicon as the target material, with a distance of 100 mm, high-purity argon and oxygen were introduced at a flow ratio of 4:1 to a pressure of 0.5 Pa, sputtered at 35 W for 10 min, heated to 800 °C, and reacted for 100 min to obtain a silicon dioxide glass matrix; (5) Immerse the silica glass substrate in a 3-aminopropylmethoxysilane solution with a mass ratio of 4 times the silica glass substrate mass, wherein the mass ratio of 3-aminopropylmethoxysilane to deionized water in the 3-aminopropylmethoxysilane solution is 1:25. Add glacial acetic acid until the pH of the solution is 4, react for 4 hours, remove the substrate, and wash with deionized water for 3 minutes to obtain the pretreated glass substrate. Mix the pretreated glass substrate, triethylamine, and acetonitrile in a mass ratio of 1:0.7:64 and place the mixture in an ice bath. Add a titanium tetrachloride acetonitrile solution with a mass ratio of 1:29 to 20 times that of the pretreated glass substrate. Rise to room temperature and react for 22 hours. Remove the solution and add glycerol, hexamethylenetetramine, and butanol in a mass ratio of 1:0.5:0.4. The mass ratio of glycerol to silica glass substrate is 0.8:1. Treat at 400℃ and 30kHz for 3 minutes, and then calcine at 450℃ for 1.5 hours to obtain the antireflective glass layer. (6) Mix antireflective glass, (chloromethyl)methyldiethoxysilane, and deionized water in a mass ratio of 1:0.2:18, react at 50℃ and 30kHz for 1.5h, remove the mixture, wash with deionized water for 3min to obtain glass precursor; mix glass precursor, pentahydroxyhexanal, toluene, glacial acetic acid, and piperidine in a mass ratio of 1:0.3:0.6:0.02:0.04, react with sonication at 30kHz for 6h under nitrogen protection, remove the mixture, wash with petroleum ether and anhydrous ethanol 4 times in sequence, then mix with sodium carbonate, trifluoroethanol, and 2,2-di(hydroxymethyl)propionic acid in a mass ratio of 1:0.0002:2:0.2, continue sonication at 40℃ for 2h, remove the mixture, wash with ethyl acetate 3 times to obtain modified precursor; (7) Mix the modified precursor, lysine diisocyanate and acetone in a mass ratio of 1:0.5:18, keep warm at 76°C for 2 hours, cool down to 40°C, add isopropanol at 0.5 times the mass of the modified precursor, sonicate at 25 kHz for 26 minutes, add deionized water at 3 times the mass of the modified precursor, sonicate at 40 kHz for 18 minutes, take it out, and dry at room temperature for 15 hours to obtain anti-reflective hard glass.

[0022] Example 2 (1) Dissolve calcium chloride in 4 times the mass of deionized water, filter, add ammonia to the solution pH 11.5, stir at 35℃ and 50 rpm for 27 min, add 0.025 times the mass of calcium chloride calcium oxide and 0.0007 times the mass of calcium chloride hydrogen peroxide, continue stirring for 36 min, filter to obtain calcium chloride solution; pour molten glass into a glass mold, spray calcium chloride solution, ammonium bicarbonate solution and ammonia in sequence at a mass ratio of 1:0.9:0.2, the mass ratio of ammonium bicarbonate to deionized water in the ammonium bicarbonate solution is 1:10, the mass ratio of calcium chloride solution to molten glass is 0.2:1, shake at 35 kHz for 28 min to obtain pretreated molten glass; (2) Under 500W microwave, the pretreated molten glass was heated to 77°C and held for 29 minutes. Then it was heated to 90°C and held for 29 minutes. After that, the vacuum was drawn to a vacuum degree of 75kPa, heated to 98°C and held for 39 minutes. Then it was cooled to 70°C and held for 5.5 hours to obtain the first dried material. (3) The first drying material is dried at 85°C for 15 hours to obtain glass powder, which is then pressed into glass sheets at 4MPa and 155°C. (4) Place the glass slide in the container and evacuate to a vacuum level of 5×10⁻⁶. -4 Pa, using pure silicon as the target material, with a distance of 115 mm, high-purity argon and oxygen were introduced at a flow ratio of 4:1 until the pressure reached 0.8 Pa, sputtered at 40 W for 14 min, heated to 825 °C, and reacted for 114 min to obtain a silicon dioxide glass matrix; (5) Immerse the silica glass substrate in a 3-aminopropylmethoxysilane solution with a mass ratio of 6 times the mass of the silica glass substrate, wherein the mass ratio of 3-aminopropylmethoxysilane to deionized water in the 3-aminopropylmethoxysilane solution is 1:38. Add glacial acetic acid until the pH of the solution is 4.5, react for 5.5 h, remove the substrate, and wash it with deionized water for 4 min to obtain the pretreated glass substrate. Mix the pretreated glass substrate, triethylamine, and acetonitrile in a mass ratio of 1:0.9:69, and... Under ice bath conditions, a titanium tetrachloride acetonitrile solution with a mass ratio of 24 times that of the pretreated glass substrate was added, with the mass ratio of titanium tetrachloride to acetonitrile in the titanium tetrachloride acetonitrile solution being 1:32. The mixture was heated to room temperature and reacted for 24 hours. The mixture was then removed from the ice bath, and glycerol, hexamethylenetetramine, and butanol were added in a mass ratio of 1:0.6:0.5, with the mass ratio of glycerol to silica glass substrate being 1:1. The mixture was then treated at 410℃ and 35kHz for 6 minutes, and then calcined at 459℃ for 2 hours to obtain the antireflective glass layer. (6) Mix antireflective glass, (chloromethyl)methyldiethoxysilane, and deionized water in a mass ratio of 1:0.3:21, react at 57°C and 35kHz for 2.5h, remove the mixture, wash with deionized water for 4min to obtain glass precursor; mix glass precursor, pentahydroxyhexanal, toluene, glacial acetic acid, and piperidine in a mass ratio of 1:0.4:0.8:0.04:0.06, react with sonication at 35kHz for 7.5h under nitrogen protection, remove the mixture, wash with petroleum ether and anhydrous ethanol 6 times in sequence, then mix with sodium carbonate, trifluoroethanol, and 2,2-di(hydroxymethyl)propionic acid in a mass ratio of 1:0.0003:5:0.4, continue sonication at 45°C for 3h, remove the mixture, wash with ethyl acetate 4 times to obtain modified precursor; (7) Mix the modified precursor, lysine diisocyanate and acetone in a mass ratio of 1:0.7:22, keep warm at 80°C for 3 hours, cool down to 45°C, add isopropanol at 1.7 times the mass of the modified precursor, sonicate at 30 kHz for 33 minutes, add deionized water at 5 times the mass of the modified precursor, sonicate at 45 kHz for 28 minutes, take it out, and dry at room temperature for 17 hours to obtain anti-reflective hard glass.

[0023] Example 3 (1) Dissolve calcium chloride in 5 times the mass of deionized water, filter, add ammonia to the solution pH 12, stir at 40℃ and 60 rpm for 34 min, add 0.04 times the mass of calcium chloride calcium oxide and 0.0009 times the mass of calcium chloride hydrogen peroxide, continue stirring for 42 min, filter to obtain calcium chloride solution; pour molten glass into a glass mold, spray calcium chloride solution, ammonium bicarbonate solution and ammonia in sequence at a mass ratio of 1:1.0:0.3, the mass ratio of ammonium bicarbonate to deionized water in the ammonium bicarbonate solution is 1:10, the mass ratio of calcium chloride solution to molten glass is 0.3:1, shake at 40 kHz for 36 min to obtain pretreated molten glass; (2) Under 600W microwave, the pretreated molten glass was heated to 85°C and held for 38 minutes. Then it was heated to 96°C and held for 36 minutes. After that, the vacuum was drawn to a vacuum degree of 80kPa, heated to 104°C and held for 44 minutes. Then it was cooled to 75°C and held for 8 hours to obtain the first dried material. (3) The first drying material is dried at 90℃ for 18h to obtain glass powder, which is then pressed into glass sheets at 5MPa and 160℃. (4) Place the glass slide in the container and evacuate to a vacuum level of 8.0 × 10⁻⁶. -4 Pa, using pure silicon as the target material, with a distance of 130 mm, high-purity argon and oxygen were introduced at a flow ratio of 4:1 to the pressure of 1 Pa, sputtered at 45 W for 18 min, heated to 850 °C, and reacted for 128 min to obtain a silicon dioxide glass matrix. (5) Immerse the silica glass substrate in a 3-aminopropylmethoxysilane solution with a mass ratio of 8 times the mass of the silica glass substrate, wherein the mass ratio of 3-aminopropylmethoxysilane to deionized water in the 3-aminopropylmethoxysilane solution is 1:50. Add glacial acetic acid until the pH of the solution is 5, react for 7 hours, remove the substrate, and wash it with deionized water for 5 minutes to obtain the pretreated glass substrate. Mix the pretreated glass substrate, triethylamine, and acetonitrile in a mass ratio of 1:1.0:74 and place the mixture in an ice bath. Add a titanium tetrachloride acetonitrile solution with a mass ratio of 28 times that of the pretreated glass substrate (titanium tetrachloride to acetonitrile in the solution is 1:36), raise the temperature to room temperature, react for 26 hours, remove the solution, and then add glycerol, hexamethylenetetramine, and butanol in a mass ratio of 1:0.8:0.6 (glycerol to silica glass substrate in a mass ratio of 1.2:1). Treat at 420℃ and 40kHz for 10 minutes, and then calcine at 468℃ for 3 hours to obtain the antireflective glass layer. (6) Mix antireflective glass, (chloromethyl)methyldiethoxysilane, and deionized water in a mass ratio of 1:0.5:24, react at 64℃ and 40kHz for 3h, remove the mixture, wash with deionized water for 6min to obtain glass precursor; mix glass precursor, pentahydroxyhexanal, toluene, glacial acetic acid, and piperidine in a mass ratio of 1:0.5:1.0:0.05:0.07, react with sonication at 40kHz for 9h under nitrogen protection, remove the mixture, wash with petroleum ether and anhydrous ethanol 8 times in sequence, then mix with sodium carbonate, trifluoroethanol, and 2,2-di(hydroxymethyl)propionic acid in a mass ratio of 1:0.0005:8:0.5, continue sonication at 50℃ for 4h, remove the mixture, wash with ethyl acetate 6 times to obtain modified precursor; (7) Mix the modified precursor, lysine diisocyanate and acetone in a mass ratio of 1:0.9:26, keep warm at 85°C for 4 hours, cool down to 50°C, add isopropanol at 2.8 times the mass of the modified precursor, sonicate at 35 kHz for 40 minutes, add deionized water at 7 times the mass of the modified precursor, sonicate at 50 kHz for 38 minutes, take it out, and dry at room temperature for 20 hours to obtain anti-reflective hard glass.

[0024] Comparative Example 1 The difference between Comparative Example 1 and Example 2 is that steps (1) and (2) are omitted, and step (3) is changed to: molten glass is dried at 85°C for 24 hours to obtain glass powder, which is then pressed into a glass sheet at 4MPa and 155°C. The remaining steps are the same as in Example 2.

[0025] Comparative Example 2 The difference between Comparative Example 2 and Example 2 is that step (5) is omitted, and step (4) is changed to: placing the glass slide in a container and evacuating to a vacuum degree of 8.0 × 10⁻⁶. -4Using pure silicon as the target material, with a distance of 130 mm, high-purity argon and oxygen were introduced at a flow ratio of 4:1 until the pressure reached 1 Pa. Sputtering was performed at 45 W for 18 min, followed by heating to 850 °C and reacting for 128 min to obtain the anti-reflective glass layer. The remaining steps were the same as in Example 2.

[0026] Comparative Example 3 The difference between Comparative Example 3 and Example 2 lies in step (6). Step (6) is changed as follows: antireflective glass, pentahydroxyhexanal, toluene, glacial acetic acid, and piperidine are mixed in a mass ratio of 1:0.4:0.8:0.04:0.06. Under nitrogen protection, the mixture is ultrasonically reacted at 35 kHz for 7.5 h. After being removed, it is washed 6 times with petroleum ether and anhydrous ethanol, respectively. Then, it is mixed with sodium carbonate, trifluoroethanol, and 2,2-di(hydroxymethyl)propionic acid in a mass ratio of 1:0.0003:5:0.4. The mixture is ultrasonically reacted again at 45°C for 3 h. After being removed, it is washed 4 times with ethyl acetate to obtain the modified precursor. The remaining steps are the same as in Example 2.

[0027] Comparative Example 4 The difference between Comparative Example 4 and Example 2 lies in step (6). Step (6) is changed to: mixing the antireflective glass, (chloromethyl)methyldiethoxysilane, and deionized water at a mass ratio of 1:0.3:21, reacting at 57°C and 35kHz for 2.5 hours, removing the mixture, and washing it with deionized water for 4 minutes to obtain the modified precursor. The remaining steps are the same as in Example 2.

[0028] Comparative Example 5 The difference between Comparative Example 5 and Example 2 is that step (7) is omitted, while the remaining steps are the same as in Example 2.

[0029] Example of effect Table 1 below presents the performance analysis results of the anti-reflective hard glass using Examples 1 to 3 and Comparative Examples 1 to 5 of the present invention.

[0030] Table 1 Hydrophilic contact angle (°) Transmittance (%) Reflectivity (%) Example 1 2.3 95.0 4.4 Example 2 2.1 95.3 4.2 Example 3 2.4 94.9 4.5 Comparative Example 1 2.4 89.9 7.8 Comparative Example 2 15.7 90.0 7.6 Comparative Example 3 29.8 94.9 4.6 Comparative Example 4 20.1 94.1 4.7 Comparative Example 5 20.3 94.5 4.5 A comparison of the transmittance and reflectance experimental data from the examples and comparative examples reveals that the present invention involves spraying calcium chloride and ammonium bicarbonate onto molten glass, followed by secondary drying to form calcium carbonate-glass core-shell structured particles; sputtering silica, during the removal of calcium carbonate, generates gases that create a porous silica structure, forming a low-refractive-index layer; then, under the action of a coupling agent, titanium tetrachloride is grafted onto the silica surface and foamed with glycerol at high temperature to obtain a foamed titanium dioxide structure, forming a high-refractive-index layer. Through the alternation of high and low refractive indices, the glass achieves an anti-reflective effect, while the silica... The non-interconnected channels of silicon and titanium dioxide enhance multi-level reflection and dissipation of light, improving the anti-reflective effect of the glass. A comparison of the hydrophilic contact angle experimental data from the examples and comparative examples reveals that this invention utilizes (chloromethyl)methyldiethoxysilane, pentahydroxyhexanal, 2,2-di(hydroxymethyl)propionic acid, and lysine diisocyanate to modify the anti-reflective properties, making the surface superhydrophilic. This allows it to wet contaminants and remove them by its own gravity, giving the glass a self-cleaning effect. Simultaneously, titanium dioxide has a photocatalytic effect; the combination of these two significantly improves the self-cleaning effect of the glass.

[0031] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No markings in the claims should be construed as limiting the scope of the claims.

Claims

1. A method for preparing anti-reflective hard glass, characterized in that, The preparation steps include the following: (1) Dissolve calcium chloride in 4 times the mass of deionized water, filter, add ammonia to the solution pH 11.5, stir at 35℃ and 50 rpm for 27 min, add 0.025 times the mass of calcium chloride calcium oxide and 0.0007 times the mass of calcium chloride hydrogen peroxide, continue stirring for 36 min, filter to obtain calcium chloride solution; pour molten glass into a glass mold, spray calcium chloride solution, ammonium bicarbonate solution and ammonia in sequence at a mass ratio of 1:0.9:0.2, the mass ratio of ammonium bicarbonate to deionized water in the ammonium bicarbonate solution is 1:10, the mass ratio of calcium chloride solution to molten glass is 0.2:1, shake at 35 kHz for 28 min to obtain pretreated molten glass; (2) Under 500W microwave, the pretreated molten glass was heated to 77°C and held for 29 minutes. Then it was heated to 90°C and held for 29 minutes. After that, the vacuum was drawn to a vacuum degree of 75kPa, heated to 98°C and held for 39 minutes. Then it was cooled to 70°C and held for 5.5 hours to obtain the first dried material. (3) The first drying material is dried at 85°C for 15 hours to obtain glass powder, which is then pressed into glass sheets at 4MPa and 155°C. (4) The glass sheet is placed in a container, vacuumed to a vacuum degree of 5x10 -4 Pa, pure silicon is used as a target material, the distance between the target material and the glass sheet is 115 mm, high-purity argon and oxygen are introduced at a flow ratio of 4:1 to a pressure of 0.8 Pa, sputtering is performed at 40 W for 14 min, heating is performed to 825 ℃, and reaction is performed for 114 min to obtain a silicon dioxide glass substrate; (5) Immerse the silica glass substrate in a 3-aminopropylmethoxysilane solution with a mass ratio of 6 times the mass of the silica glass substrate, wherein the mass ratio of 3-aminopropylmethoxysilane to deionized water in the 3-aminopropylmethoxysilane solution is 1:

38. Add glacial acetic acid until the pH of the solution is 4.5, react for 5.5 h, remove the substrate, and wash it with deionized water for 4 min to obtain the pretreated glass substrate. Mix the pretreated glass substrate, triethylamine, and acetonitrile in a mass ratio of 1:0.9:69, and... Under ice bath conditions, a titanium tetrachloride acetonitrile solution with a mass ratio of 24 times that of the pretreated glass substrate was added, with the mass ratio of titanium tetrachloride to acetonitrile in the titanium tetrachloride acetonitrile solution being 1:

32. The mixture was heated to room temperature and reacted for 24 hours. The mixture was then removed from the ice bath, and glycerol, hexamethylenetetramine, and butanol were added in a mass ratio of 1:0.6:0.5, with the mass ratio of glycerol to silica glass substrate being 1:

1. The mixture was then treated at 410℃ and 35kHz for 6 minutes, and then calcined at 459℃ for 2 hours to obtain the antireflective glass layer. (6) Mix antireflective glass, (chloromethyl)methyldiethoxysilane, and deionized water in a mass ratio of 1:0.3:21, react at 57°C and 35kHz for 2.5h, remove the mixture, wash with deionized water for 4min to obtain glass precursor; mix glass precursor, pentahydroxyhexanal, toluene, glacial acetic acid, and piperidine in a mass ratio of 1:0.4:0.8:0.04:0.06, react with sonication at 35kHz for 7.5h under nitrogen protection, remove the mixture, wash with petroleum ether and anhydrous ethanol 6 times in sequence, then mix with sodium carbonate, trifluoroethanol, and 2,2-di(hydroxymethyl)propionic acid in a mass ratio of 1:0.0003:5:0.4, continue sonication at 45°C for 3h, remove the mixture, wash with ethyl acetate 4 times to obtain modified precursor; (7) Mix the modified precursor, lysine diisocyanate and acetone in a mass ratio of 1:0.7:22, keep warm at 80°C for 3 hours, cool down to 45°C, add isopropanol at 1.7 times the mass of the modified precursor, sonicate at 30 kHz for 33 minutes, add deionized water at 5 times the mass of the modified precursor, sonicate at 45 kHz for 28 minutes, take it out, and dry at room temperature for 17 hours to obtain anti-reflective hard glass.

Citation Information

Patent Citations

  • Glass substrate coated with anti-reflective layer

    CN103813993A

  • Antiskid water permeable brick and preparation method thereof

    CN114163180A