Composite flash non-woven fabric and preparation method thereof

Through the combination of PBAT material and sodium alginate cross-linked starch masterbatch, a composite structure of PBAT layer-flash non-woven fabric layer-PBAT layer is constructed, which solves the problem of limited application of flash non-woven fabrics in the field of clothing and realizes It combines high mechanical properties, antibacterial properties and simulation effects, and is suitable for environmentally friendly materials in the field of clothing.

CN118721875AActive Publication Date: 2024-10-01XIAMEN DANGSHENG NEW MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410723122.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01
Estimated Expiration
2044-06-05

AI Technical Summary

Technical Problem

The application of flash-steamed non-woven fabrics in the field of clothing is limited by its hard texture, low simulation, and doubts about the environmental friendliness of polyethylene materials, and its mechanical properties are not enough to meet the antibacterial needs of humid environments.

Method used

PBAT material is used to form a film and a sandwich structure of PBAT layer-flash non-woven layer-PBAT layer is formed. A simulated surface texture is formed through kneading treatment, and sodium alginate cross-linked starch masterbatch is used as an organic filler to improve antibacterial properties. and mechanical properties.

Benefits of technology

It achieves the balance between the mechanical strength of flash-vaporized non-woven fabrics and the bioaffinity and antibacterial properties of PBAT materials, forming a fashionable composite material suitable for the field of clothing, while ensuring the product's performance and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004877799910000111
    Figure BDA0004877799910000111
  • Figure BDA0004877799910000121
    Figure BDA0004877799910000121
  • Figure BDA0004877799910000131
    Figure BDA0004877799910000131
Patent Text Reader

Abstract

The invention discloses a composite flash non-woven fabric and a preparation method thereof, and belongs to the technical field of high polymer materials. According to the method, a film is formed through a PBAT material with specific composition in advance, a sandwich structure product of a PBAT layer, a flash evaporation non-woven fabric layer and a PBAT layer is constructed, the product of the composite structure has the mechanical strength of flash evaporation non-woven fabric and the biocompatibility and antibacterial property of the PBAT material, and then the product generates surface textures with a simulation effect through rubbing treatment. The fabric is very suitable for the field of clothes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and in particular to a composite flash-steamed nonwoven fabric and a preparation method thereof. Background Art

[0002] Flash non-woven fabric is a product prepared by instantly releasing polymer raw materials (mainly polyethylene) in a high temperature and high pressure environment to normal temperature and pressure to form a spindle fiber film. Compared with traditional synthetic non-woven fabrics, it has higher strength and lighter weight.

[0003] However, compared with traditional non-woven materials, flash-steamed non-woven fabrics are harder in texture and have a lower degree of simulation. In addition, based on the characteristics of polyethylene, people are unwilling to have direct contact with polyethylene plastic products for a long time. Therefore, there are currently few products that use flash-steamed non-woven fabrics in the clothing field.

[0004] Biodegradable polyesters, led by PBAT (polybutylene adipate terephthalate), are often used in the field of food and pharmaceutical packaging. The main reasons are their good processing performance, high biocompatibility and degradability, safety and environmental protection. In addition, these materials are generally compounded with PLA (polylactic acid), which is a natural antibacterial and antifungal agent that can inhibit the growth of bacteria and mold on products in some humid environments. In theory, it is very suitable for the field of clothing. However, the mechanical properties of biodegradable polyesters are generally not as good as those of non-biodegradable plastics such as polypropylene and polyethylene, and they are very susceptible to damage. Summary of the invention

[0005] Based on the defects of the prior art, the purpose of the present application is to provide a method for preparing a composite flash-steamed non-woven fabric, which pre-films a PBAT material with a specific composition and constructs a sandwich structure product of a PBAT layer-flash-steamed non-woven fabric layer-PBAT layer. This composite structure product has both the mechanical strength of the flash-steamed non-woven fabric and the bioaffinity and antibacterial properties of the PBAT material. Subsequently, through a rubbing treatment, the product produces a surface texture with a simulation effect, has a high sense of fashion, and is very suitable for the field of clothing.

[0006] In order to achieve the above purpose, the technical solution adopted by this application is:

[0007] A method for preparing a composite flash-steamed nonwoven fabric comprises the following steps:

[0008] A PBAT composite resin is prepared, and then a first PBAT film layer and a second PBAT film layer are obtained by film blowing. The PBAT composite resin includes PBAT resin, polylactic acid, inorganic filler and organic filler. The organic filler is a sodium alginate cross-linked starch masterbatch. The average particle size of the organic filler is ≤3 μm, and the mass content of the organic filler in the PBAT composite resin is ≤5wt%.

[0009] The first PBAT film layer and the second PBAT film layer are respectively covered on both sides of the flash non-woven fabric, and the air is evacuated and hot-rolled edge-sealed to obtain a composite base fabric.

[0010] The composite substrate is placed in water to wet it, and then placed in a kneading machine with a heating system to rotate forward and backward for the first kneading treatment. During the first kneading treatment, the drum speed of the kneading machine is 500-800r / min, the temperature is 30-40℃, and the time is 10-15min.

[0011] The composite base fabric after the first rubbing treatment is soaked in water at 0-5°C for 5-10 minutes, and then put back into the rubbing machine for the second rubbing treatment. During the second rubbing treatment, the drum speed of the rubbing machine is 900-1300r / min, the temperature is 75-85°C, and the time is 2-4min.

[0012] The composite base fabric after the second rubbing treatment is cooled and dried to obtain the composite flash-steamed non-woven fabric.

[0013] Preferably, the flash-steamed nonwoven fabric is a polyethylene flash-steamed nonwoven fabric.

[0014] Preferably, the average particle size of the organic filler is 1 to 3 μm.

[0015] Flash non-woven fabrics, especially polyethylene flash non-woven fabrics, have high mechanical strength and good barrier properties due to their special preparation process and three-dimensional fiber composite structure, and are also light in weight. They have great advantages when used in the field of clothing. However, their texture is dry and uncomfortable, and their surface is smooth. If they are used in the field of clothing, they will not look fashionable. In order to form some leather-like texture effects on the surface to enhance the sense of fashion, existing non-woven materials will be rubbed, and this treatment will also make the texture of the material fluffy to a certain extent, and the touch will be improved. However, for flash non-woven fabrics, based on the characteristics of their material texture, it is difficult to form a uniform and realistic texture effect on the surface using conventional rubbing treatment methods. However, if the intensity of the rubbing treatment is increased, the surface of the product will be damaged, which will affect the performance of the product. Furthermore, when existing users mention polyethylene materials, they all think that it is a toxic and environmentally unfriendly material, and they will not directly wear underwear made of polyethylene materials. To this end, in the technical solution of this application, the inventor first coated the flash non-woven fabric with a film layer made of environmentally friendly green PBAT resin to form a composite base fabric, eliminating people's prejudice against polyethylene materials. Even if the polyethylene flash non-woven fabric may produce some toxic substances at high temperatures, it will be isolated by the PBAT film and will not directly contact human skin; at the same time, the polylactic acid contained in the PBAT film layer has a certain antibacterial and antifungal effect. When the product is prepared into clothing, it can effectively improve the storage performance of the product and is not easy to mold and grow bacteria. Finally, PBAT resin is a degradable polyester with a certain degree of recyclability. Based on actual conditions, technicians in this field can use PBAT resin prepared from recycled materials as the raw material for preparation when preparing the PBAT film layer, which is highly environmentally friendly.

[0016] At the same time, in order to make the composite flash-steamed non-woven fabric obtain the ideal surface texture without affecting its performance, the inventor introduced sodium alginate grafted starch masterbatch as an organic filler in the PBAT film layer, and then soaked the prepared composite base fabric in water. At this time, the sodium alginate grafted starch masterbatch in the PBAT film layer will absorb water and swell, so that the tiny pores between the PBAT film layer and the flash-steamed non-woven fabric are quickly filled, and then sent to the rubbing machine for a specific two-step rubbing treatment. At this time, the PBAT film will act as a buffer layer for the flash-steamed non-woven fabric, and the PBAT film will be used as a buffer layer for the low power-high power composite base fabric. The segmented rubbing treatment can ensure that the surface of the flash-steamed non-woven fabric is fully textured, and at the same time, the surface of the flash-steamed non-woven fabric will not be damaged due to stress and gravity. On the other hand, since the sodium alginate grafted starch masterbatch will swell and gelatinize and fall off at a higher temperature after absorbing water, and the rubbing process will cause a certain amount of thermal agglomeration locally, after low-power and low-temperature rubbing treatment, it is necessary to first cool in water (or ice-water mixture) at 0-5°C. At this time, the initial texture on the surface of the flash-steamed non-woven fabric will also be quickly fixed to avoid the concentrated shedding of organic fillers during subsequent high-power rubbing treatment.

[0017] In addition, the size of the organic filler in the PBAT film layer must be controlled within a specific range. Otherwise, during high-power rubbing treatment, if the size of the organic filler is too large, the swelling, gelatinization, and shedding of the sodium alginate grafted starch masterbatch may lead to uneven rubbing, or the rubbing of the composite film layer may be damaged due to local agglomeration and adhesion, which ultimately affects the performance of the product. On the other hand, since the shedding of the organic filler after infiltration during high-power rubbing treatment is an inevitable phenomenon, if the content is too high, it will not only fail to effectively serve as an interlayer adsorbent, but may also increase the interlayer pores due to shedding and agglomeration, and even cause partial exposure of the flash non-woven fabric, and the prepared product will also have a poor impact.

[0018] Preferably, the heating system of the grain kneading machine includes at least one of a hot air heating system and a steam heating system.

[0019] More preferably, the heating system of the grain kneading machine has a heating rate of ≥5°C / min during heating.

[0020] More preferably, the heating system of the grain kneading machine has a heating rate of 5 to 8° C. / min.

[0021] When the composite base fabric inside the rubbing machine is heated at different preheating rates, if the heating time is too long, the flash-evaporated fibers in the composite base fabric will expand for too long. At the same time, the probability of the impregnated organic filler in the PBAT film falling off is higher in the high temperature and high power stage, which has a greater impact on the protective effect of the product.

[0022] Preferably, the PBAT composite resin comprises the following components in parts by weight:

[0023] 80-85 parts of PBAT resin, 5-10 parts of polylactic acid, 6-9 parts of inorganic filler, and 1-4 parts of organic filler.

[0024] More preferably, the melt index of the PBAT resin tested according to ISO 1133-2011 is 5 to 10 g / min, the test load is 2.16 kg, and the test temperature is 190°C.

[0025] More preferably, the PBAT resin includes at least one of new material and recycled material.

[0026] In the present application, the mechanical properties of the product are mainly derived from the flash-steamed non-woven fabric. Therefore, based on actual needs, those skilled in the art can use new PBAT materials to prepare the film layer, or use recycled materials or other recycled materials (for example, PBAT recycled materials newly made from PET waste) as the base resin for preparation. It has been verified that it will basically not affect the performance of the product, nor will it cause obvious differences in the rubbing effect.

[0027] More preferably, the melt index of the polylactic acid tested according to ISO 1133-2011 is 1 to 10 g / min, the test load is 2.16 kg, and the test temperature is 190°C.

[0028] More preferably, the average particle size of the inorganic filler is 1 to 3 μm.

[0029] More preferably, the inorganic filler includes at least one of talc, montmorillonite, wollastonite, calcite, granite, kaolin, aerosol clay, titanium dioxide, silicon dioxide, mica powder, and glass fiber.

[0030] More preferably, the sodium alginate cross-linked starch masterbatch can be purchased commercially available starch masterbatch prepared by cross-linking with sodium alginate, or can be prepared by cross-linking starch with sodium alginate and then preparing it in the form of masterbatch. It should be noted that both methods can obtain sodium alginate cross-linked starch masterbatch, and this masterbatch can exert the expected adsorption and expansion properties, and at the same time has good relative stability, so that the composite base cloth can obtain the ideal technical effect after rubbing treatment.

[0031] More preferably, the method for preparing sodium alginate cross-linked starch masterbatch comprises the following steps:

[0032] Starch and sodium alginate are mixed in water, and then the pH of the resulting mixture is adjusted to 9-10, a cross-linking agent is added and a cross-linking reaction is carried out. After the reaction is completed, the pH of the resulting mixture is adjusted to 6.5-7.5, the solid-liquid is separated, and the mixture is dried to obtain sodium alginate cross-linked starch.

[0033] The sodium alginate cross-linked starch and the auxiliary agent are mixed and stirred, extruded into granules by a twin-screw extruder, and sieved to obtain the sodium alginate cross-linked starch masterbatch.

[0034] More preferably, the starch is plant starch, and the plant starch is at least one of corn starch, wheat starch and potato starch.

[0035] More preferably, the auxiliary agent includes at least one of a plasticizer, a solvent, a compatibilizer, a filler, and a lubricant.

[0036] More preferably, the mass content of sodium alginate cross-linked starch in the sodium alginate cross-linked starch masterbatch is ≥ 95wt%.

[0037] More preferably, the temperature during the cross-linking reaction is 20 to 40° C., and the time is 1 to 2 hours.

[0038] Preferably, the mass ratio of starch to sodium alginate is 1:(0.1-0.2).

[0039] Sodium alginate can improve the stability and adsorption performance of starch after being grafted with starch, so that the PBAT film layer has a stronger fit to the flash-steamed non-woven fabric after infiltration, which is more conducive to ensuring that the flash-steamed non-woven fabric will not be seriously damaged during the graining process. However, relatively speaking, if too much sodium alginate is grafted, its overall viscosity will increase, especially during the high-temperature and high-power graining process, it is easy to gelatinize and denature, and then fall off and agglomerate. Therefore, it is better to prepare the raw materials with the mass ratio of the above-mentioned starch and sodium alginate and prepare the sodium alginate cross-linked starch masterbatch.

[0040] Preferably, the preparation method of the PBAT composite resin is: mixing the components, and then placing them in a twin-screw extruder for melt extrusion at 160-180° C. to obtain the PBAT composite resin.

[0041] Preferably, the temperature during film blowing of the PBAT composite resin is 120-150°C.

[0042] Preferably, in the composite base fabric, the thickness ratio of the first PBAT film layer, the flash non-woven fabric and the second PBAT film layer is (0.8-1.2):3:(0.8-1.2).

[0043] Preferably, the temperature during hot rolling edge banding treatment is 300-360° C., and the pressure is 10-30N.

[0044] Another object of the solution of the present application is to provide a composite flash-steamed non-woven fabric prepared by the preparation method of the composite flash-steamed non-woven fabric.

[0045] Preferably, the composite flash-steamed non-woven fabric has a tensile strength of 6 to 7 kN / m and an elongation at break of 25 to 30% tested according to GB / T 12914-2018 (specimen width 25.4 mm, tensile rate 100 mm / min, MD).

[0046] Preferably, the tear strength of the composite flash-steamed nonwoven fabric tested according to GB / T 4744-2013 (constant radius cutting method, MD) is 10-11N.

[0047] Preferably, the composite flash nonwoven fabric has a gram weight of 160 to 180 g / m2 as tested according to GB / T 451.2-2002. 2 .

[0048] Another object of the present application is to provide an application of the composite flash-spun nonwoven fabric in the preparation of clothing products.

[0049] The beneficial effect of the present application is that the present application provides a composite flash-steamed non-woven fabric and a preparation method thereof, wherein the method pre-films a PBAT material of a specific composition and constructs a sandwich structure product of a PBAT layer-flash-steamed non-woven fabric layer-PBAT layer. The composite structure product has both the mechanical strength of the flash-steamed non-woven fabric and the bioaffinity and antibacterial properties of the PBAT material. Subsequently, through a rubbing treatment, the product produces a surface texture with a simulation effect, has a high sense of fashion, and is very suitable for the field of clothing. DETAILED DESCRIPTION

[0050] In order to better illustrate the purpose, technical solutions and advantages of the present application, the present application will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present application in detail, rather than to limit the present application. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application. Unless otherwise specified, the experimental reagents and instruments involved in the implementation of this application are all commonly used ordinary reagents and instruments. The flash non-woven fabric used in this application is the same polypropylene flash non-woven fabric material as the Rowelk product for flash spinning protective clothing developed by the applicant. The vertical drum kneading machine is a commercially available product with a hot air heating system. The meltblowing machine is a commercially available product with a meltblowing nozzle, a traction belt and a collection net.

[0051] Example 1

[0052] An embodiment of a composite flash-steamed nonwoven fabric and a method for preparing the same described in the present application comprises the following steps:

[0053] (1) preparing a PBAT composite resin, and then blowing a film at 145° C. in a film blowing machine to obtain a first PBAT film layer and a second PBAT film layer, wherein 100 parts of the PBAT composite resin include 80 parts of PBAT resin, 10 parts of polylactic acid, 6 parts of inorganic fillers and 4 parts of organic fillers, the melt index of the PBAT resin tested according to ISO 1133-2011 is 6 g / min, and the THJS-7801 produced by Lanshan Tunhe; the polylactic acid is tested according to ISO The melt index of 1133-2011 is 8g / min, and LX930 is produced by Purak; the inorganic filler is talcum powder with an average particle size of 3μm, and the organic filler is sodium alginate cross-linked starch masterbatch, and the preparation method is: 99wt% of sodium alginate cross-linked starch and 1wt% of an auxiliary agent (commercially available lubricant erucic acid amide) are mixed and stirred, and a twin-screw extruder is used to extrude and granulate at 100-180°C (screw speed is 400rpm), and sieved to obtain sodium alginate cross-linked starch masterbatch with an average particle size of 2μm;

[0054] The preparation method of sodium alginate cross-linked starch is as follows: corn starch and sodium alginate are mixed in water at a mass ratio of 1:0.2, and then the pH value of the obtained mixed solution is adjusted to 10, and a cross-linking agent phosphorus oxychloride (1wt% of the total mass of starch and sodium alginate) is added, and a cross-linking reaction is carried out at 30°C for 1.5h. After the reaction is completed, the pH value of the obtained mixed solution is adjusted to 7, and the solid-liquid separation is performed, and the mixture is dried to obtain sodium alginate cross-linked starch.

[0055] The preparation method of the PBAT composite resin is as follows: the components are mixed, and then placed in a twin-screw extruder for melt extrusion at 160-180° C. (screw speed 400 rpm) to obtain the PBAT composite resin.

[0056] (2) Covering the first PBAT film layer and the second PBAT film layer on both sides of the flash non-woven fabric respectively, evacuating the air and performing hot rolling edge sealing treatment at 350° C. and 20N to obtain a composite base fabric, wherein the thickness ratio of the first PBAT film layer, the flash non-woven fabric layer and the second PBAT film layer in the obtained composite base fabric is 1:3:1;

[0057] (3) Wetting the composite substrate in water, and then placing it in a grain kneading machine with a heating system and turning it forward and backward to perform a first grain kneading treatment. During the first grain kneading treatment, the drum speed of the grain kneading machine is 600 r / min, the temperature is 35° C., the time is 12 min, and the heating rate of the grain kneading machine during heating is 5° C. / min;

[0058] (4) soaking the composite base fabric after the first rubbing treatment in 3° C. water for 10 min, and then placing it back into the rubbing machine for a second rubbing treatment. During the second rubbing treatment, the drum speed of the rubbing machine is 1000 r / min, the temperature is 80° C., and the time is 3 min;

[0059] (5) Cooling and drying the composite base fabric after the second rubbing treatment to obtain the composite flash-steamed non-woven fabric.

[0060] Example 2

[0061] An embodiment of a composite flash-steamed nonwoven fabric and a method for preparing the same described in the present application comprises the following steps:

[0062] (1) Same as step (1) of Example 1;

[0063] (2) Same as step (2) of Example 1;

[0064] (3) Wetting the composite substrate in water, and then placing it in a grain kneading machine with a heating system and turning it forward and backward to perform the first grain kneading treatment. During the first grain kneading treatment, the drum speed of the grain kneading machine is 700 r / min, the temperature is 35° C., and the time is 11 minutes.

[0065] (4) The composite base fabric after the first rubbing treatment was soaked in 3°C water for 10 minutes, and then placed in the rubbing machine for the second rubbing treatment. During the second rubbing treatment, the drum speed of the rubbing machine was 1100 r / min, the temperature was 80°C, and the time was 4 minutes.

[0066] (5) Cooling and drying the composite base fabric after the second rubbing treatment to obtain the composite flash-steamed non-woven fabric.

[0067] Example 3

[0068] An embodiment of a composite flash nonwoven fabric and a preparation method thereof described in the present application is different from embodiment 1 only in that the PBAT composite resin, calculated as 100 parts, includes 85 parts of PBAT resin, 5 parts of polylactic acid, 7 parts of inorganic filler and 3 parts of organic filler. The melt index of polylactic acid tested according to ISO 1133-2011 is 5g / min, 4043D is produced by Natureworks of the United States, and the inorganic filler is wollastonite with an average particle size of 2μm.

[0069] Example 4

[0070] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof described in the present application is different from Embodiment 1 only in that the heating rate of the kneading machine during heating is 6° C. / min.

[0071] Example 5

[0072] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof described in the present application is different from Embodiment 1 only in that the heating rate of the kneading machine during heating is 8° C. / min.

[0073] Example 6

[0074] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof described in the present application is different from Embodiment 1 only in that the heating rate of the kneading machine during heating is 3° C. / min.

[0075] Example 7

[0076] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof described in the present application is different from Embodiment 1 only in that, during the preparation of sodium alginate cross-linked starch, starch and sodium alginate are added in a mass ratio of 1:0.1.

[0077] Example 8

[0078] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof described in the present application is different from Embodiment 1 only in that, during the preparation of sodium alginate cross-linked starch, starch and sodium alginate are added in a mass ratio of 1:0.05.

[0079] Example 9

[0080] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof described in the present application is different from Embodiment 1 only in that, during the preparation of sodium alginate cross-linked starch, starch and sodium alginate are added in a mass ratio of 1:0.5.

[0081] Example 10

[0082] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof described in the present application is different from Embodiment 1 only in that the average particle size of the sodium alginate cross-linked starch masterbatch is 1 μm.

[0083] Embodiment 11

[0084] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof described in the present application is different from Embodiment 1 only in that the average particle size of the sodium alginate cross-linked starch masterbatch is 3 μm.

[0085] Comparative Example 1

[0086] A composite flash-steamed nonwoven fabric and a preparation method thereof, comprising the following steps:

[0087] (1) Same as step (1) of Example 1;

[0088] (2) Same as step (2) of Example 1;

[0089] (3) Wetting the composite substrate in water, and then placing it in a grain kneading machine with a heating system and turning it forward and backward to perform grain kneading treatment. During the grain kneading treatment, the drum speed of the grain kneading machine is 600 r / min, the temperature is 35° C., the time is 15 min, and the heating rate of the grain kneading machine during heating is 5° C. / min;

[0090] (4) Cooling and drying the composite base fabric after the rubbing treatment to obtain the composite flash-steamed non-woven fabric.

[0091] Comparative Example 2

[0092] A composite flash-steamed nonwoven fabric and a preparation method thereof, comprising the following steps:

[0093] (1) Same as step (1) of Example 1;

[0094] (2) Same as step (2) of Example 1;

[0095] (3) Wetting the composite substrate in water, and then placing it in a grain kneading machine with a heating system and rotating it forward and backward to perform grain kneading treatment. During the grain kneading treatment, the drum speed of the grain kneading machine is 1000 r / min, the temperature is 80° C., the time is 15 min, and the heating rate of the grain kneading machine during heating is 5° C. / min;

[0096] (4) Cooling and drying the composite base fabric after the rubbing treatment to obtain the composite flash-steamed non-woven fabric.

[0097] Comparative Example 3

[0098] A composite flash-steamed nonwoven fabric and a preparation method thereof, comprising the following steps:

[0099] (1) Same as step (1) of Example 1;

[0100] (2) Same as step (2) of Example 1;

[0101] (3) Same as step (3) of Example 1;

[0102] (4) placing the composite substrate after the first rubbing treatment into a rubbing machine for a second rubbing treatment, wherein the drum speed of the rubbing machine during the second rubbing treatment is 1000 r / min, the temperature is 80° C., and the time is 3 min;

[0103] (5) Same as step (5) of Example 1.

[0104] Comparative Example 4

[0105] A composite flash-steamed nonwoven fabric and a preparation method thereof, the difference from Example 1 being that the temperature during the first rubbing treatment is 80°C.

[0106] Comparative Example 5

[0107] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof is different from Embodiment 1 only in that the organic filler is replaced by talcum powder with an average particle size of 2 μm.

[0108] Comparative Example 6

[0109] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof, the only difference from embodiment 1 is that the organic filler is a starch masterbatch, and the preparation method is: 99wt% of starch and 1wt% of an auxiliary agent (commercially available lubricant erucamide) are mixed and stirred, extruded and granulated at 100-180°C using a twin-screw extruder (screw speed 400rpm), and sieved to obtain starch masterbatch with an average particle size of 2μm.

[0110] Comparative Example 7

[0111] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof is different from Embodiment 1 only in that the average particle size of the sodium alginate cross-linked starch masterbatch is 5 μm.

[0112] Comparative Example 8

[0113] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof is different from Embodiment 1 only in that 100 parts of the PBAT composite resin include 80 parts of PBAT resin, 10 parts of polylactic acid, and 10 parts of organic filler.

[0114] Comparative Example 9

[0115] An embodiment of a composite flash-steamed nonwoven fabric and a preparation method thereof is different from Embodiment 1 only in that 100 parts of the PBAT composite resin include 70 parts of PBAT resin, 10 parts of polylactic acid, 12 parts of inorganic filler, and 8 parts of organic filler.

[0116] Effect example

[0117] In order to verify the performance effect of the composite flash-steamed nonwoven fabric described in the present application, the products of each embodiment and comparative example were subjected to the following tests:

[0118] (1) Appearance three-dimensional texture test: Using commercial cowhide leather as a reference, a group of five people scored the appearance three-dimensional texture of each embodiment and comparative example product, and the average score was calculated. The scoring criteria are as follows:

[0119] The highest score is 5 points and the lowest score is 1 point.

[0120] 5 points: The texture is even and three-dimensional.

[0121] 4 points: The texture is uniform and three-dimensional, or the texture is three-dimensional and uniform.

[0122] 3 points: The texture is more three-dimensional and more uniform.

[0123] 2 points: The texture is uneven or not three-dimensional.

[0124] 1 point: The texture is uneven and not three-dimensional.

[0125] (2) Tensile strength & elongation at break retention test: Before the implementation of each embodiment and comparative example, the un-crumpled composite base fabric was tested in advance according to GB / T 12914-2018 (specimen width 25.4 mm, tensile rate 100 mm / min, MD), and the tensile strength of each un-crumpled composite base fabric was measured to be 7-7.5 kN / m, and the elongation at break was 25-35%, which was consistent with the test situation. The tensile strength and elongation at break test values ​​of the untreated composite base fabric of each embodiment and comparative example were calibrated as the initial values, and then the same test was performed on the composite flash-steamed non-woven fabric obtained after the implementation of each embodiment and comparative example, and the tensile strength & elongation at break retention (%) was calculated based on the initial value = tensile strength & elongation at break of composite flash-steamed non-woven fabric / initial value × 100%.

[0126] (3) Tear strength retention rate test: Before the implementation of each embodiment and comparative example, the composite base fabric without rubbing treatment was tested in advance according to GB / T 4744-2013 (constant radius cutting method, MD), and the tensile strength of each composite base fabric without rubbing treatment was measured to be 10.5-11.5N, which was in line with the test situation. The tear strength test value of the untreated composite base fabric of each embodiment and comparative example was calibrated as the initial value, and then the composite flash nonwoven fabric obtained after the implementation of each embodiment and comparative example was subjected to the same test, and the tear strength retention rate (%) was calculated based on the initial value = tear strength of composite flash nonwoven fabric / initial value × 100%.

[0127] The test results are shown in Table 1.

[0128] Table 1

[0129]

[0130]

[0131]

[0132]

[0133] It can be seen from the results that the composite flash-steamed non-woven fabric described in this application has excellent appearance and good leather texture effect. The appearance score of each embodiment product can reach 4 points or more, and it can be used in the field of clothing in terms of fashion appearance. At the same time, after the rubbing treatment, the mechanical properties of the composite flash-steamed non-woven fabric are basically maintained at a high level, among which the tensile strength can be maintained at more than 85% before rubbing, reaching 6-7kN / m, the elongation at break can be maintained at more than 80% before rubbing, reaching 25-30%, and the tear strength can be maintained at more than 90% before rubbing, reaching more than 10N.

[0134] Among them, according to the performance results of the products of Examples 1 and 4 to 6, it can be seen that during the rubbing treatment, the heating rate during heating determines the overall heating time length of the composite base fabric. If the heating time is too long, it may cause the probability of organic fillers in the PBAT film layer to fall off. Increased, thereby affecting the performance of the product, the heating rate of the rubbing machine is better at 5 ° C / min and above.

[0135] According to Example 1, Examples 7 to 9 and Comparative Example 6, it can be seen that whether the starch masterbatch in the PBAT film layer is grafted with sodium alginate has a decisive effect on the performance of the product. When there is no sodium alginate grafting modification, the stability and adsorption of the starch masterbatch are poor, so that the PBAT film layer cannot adequately adhere to and protect the flash non-woven fabric during the rubbing process. Not only is the texture effect of the rubbing not good, but the performance of the product after rubbing is significantly attenuated compared to before rubbing, as shown in Comparative Example 6. As shown in the figure, the retention rate of tensile strength after rubbing is only 84.2%. With the grafting of sodium alginate, the starch masterbatch can fully absorb water and swell and adsorb between layers, thereby improving the protective effect on the flash-steamed non-woven fabric. However, since the viscosity of the masterbatch will change to a certain extent after sodium alginate grafting, if too much grafting is carried out, the probability of the masterbatch falling off and agglomeration will increase during subsequent high-power rubbing. Therefore, when preparing sodium alginate grafted starch masterbatch, the mass ratio of sodium alginate to starch is 1: (0.1-0.2), the best effect is achieved.

[0136] According to Example 1, Examples 10 to 11 and Comparative Example 7, it can be seen that when used as a filler in the PBAT film layer, the size of the sodium alginate grafted starch masterbatch also affects the final performance of the product. The size cannot be too large, otherwise it will be as shown in the product of Comparative Example 7. Not only is the appearance score less than 4 points, but the tensile strength, elongation at break and tear resistance are all at a low level after rubbing treatment.

[0137] Comparative Examples 1 and 2 adopted traditional one-step rubbing treatment after constructing the composite base fabric. The former adopted a low-power rubbing treatment condition, while the latter was a high-power condition. The results showed that the rubbing effect of the product of Comparative Example 1 was poor and there was no expected texture effect. Although the texture of the product of Comparative Example 2 was deeper, its uniformity was poor. The main reason was that the rubbing was too intense and uneven. Therefore, the score was less than 4 points, and the product's performance attenuation was high. The tensile strength, elongation at break and tear resistance after rubbing were the lowest among all products.

[0138] The product of Comparative Example 3 was subjected to segmented rubbing on the basis of Comparative Examples 1 and 2, but no water cooling treatment was used in the intermediate process. The appearance of the product reached 4 points, but the performance retention rate of the product was lower than that of Example 1, especially the tensile strength, which was only 82.8% after rubbing.

[0139] Compared with Example 1, the temperature of the product of Comparative Example 4 during the segmented kneading is 80°C. Under such high temperature conditions, the organic filler of the PBAT film layer expands and gelatinizes to a high degree. The results show that its performance is equivalent to that of the product of Comparative Example 2, indicating that in the segmented kneading, in addition to the kneading power, the kneading temperature must also be specifically limited.

[0140] In the comparative example 5 product, no organic filler is introduced, but the PBAT film layer is prepared with the traditional inorganic filler system. Compared with the organic filler compound film layer, its adsorption and protection for the flash non-woven fabric are not high. The appearance score of the prepared product is only 3.6 points, and the retention rate of various properties after rubbing is low.

[0141] However, the introduction of organic fillers cannot be too much, because during high-power rubbing treatment, the expansion, gelatinization and shedding of organic fillers are inevitable. If the introduction amount is too much, the shedding amount will also increase, which will cause the composite base cloth to stick together during rubbing, thereby causing the rubbing effect of the product to be uneven. As shown in Comparative Examples 8 and 9, regardless of whether the content of the matrix PBAT resin changes, if the proportion of organic fillers exceeds 5wt%, the performance of the product is not ideal.

[0142] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.

Claims

1. A method for preparing a composite flash-steamed nonwoven fabric, characterized in that: The following steps are involved: A PBAT composite resin is prepared, and then a first PBAT film layer and a second PBAT film layer are obtained by film blowing, wherein the PBAT composite resin comprises a PBAT resin, polylactic acid, an inorganic filler and an organic filler, wherein the organic filler is a sodium alginate cross-linked starch masterbatch, wherein the average particle size of the organic filler is less than or equal to 3 μm, and the mass content of the organic filler in the PBAT composite resin is less than or equal to 5 wt %; The first PBAT film layer and the second PBAT film layer are respectively covered on both sides of the flash non-woven fabric, and the air is evacuated and hot-rolled edge-sealed to obtain a composite base fabric; The composite substrate is placed in water to wet it, and then placed in a kneading machine with a heating system to rotate forward and reverse to perform a first kneading treatment, wherein the drum speed of the kneading machine is greater than or equal to 500 r / min and less than or equal to 800 r / min, the temperature is greater than or equal to 30° C. and less than or equal to 40° C., and the time is greater than or equal to 10 min and less than or equal to 15 min; The composite base fabric after the first rubbing treatment is soaked in water at 0-5°C for 5-10 minutes, and then placed in the rubbing machine for the second rubbing treatment, wherein the drum speed of the rubbing machine is greater than or equal to 900 r / min and less than or equal to 1300 r / min, the temperature is greater than or equal to 75°C and less than or equal to 85°C, and the time is greater than or equal to 2 minutes and less than or equal to 4 minutes during the second rubbing treatment; The composite base fabric after the second rubbing treatment is cooled and dried to obtain the composite flash-steamed non-woven fabric.

2. The method for preparing the composite flash-steamed nonwoven fabric according to claim 1, characterized in that: The heating system of the grain kneading machine has a heating rate greater than or equal to 5°C / min during heating.

3. The method for preparing the composite flash-steamed nonwoven fabric according to claim 1, characterized in that: The PBAT composite resin comprises the following components in parts by weight: 80-85 parts of PBAT resin, 5-10 parts of polylactic acid, 6-9 parts of inorganic filler, and 1-4 parts of organic filler.

4. The method for preparing the composite flash-steamed nonwoven fabric according to claim 1, characterized in that: The preparation method of sodium alginate cross-linked starch masterbatch, The following steps are included: Mix starch and sodium alginate in water, then adjust the pH of the resulting mixture to 9-10, add a cross-linking agent and perform a cross-linking reaction, after the reaction is completed, adjust the pH of the resulting mixture to 6.5-7.5, separate the solid and liquid, and dry to obtain sodium alginate cross-linked starch; The sodium alginate cross-linked starch and the auxiliary agent are mixed and stirred, extruded into granules by a twin-screw extruder, and sieved to obtain the sodium alginate cross-linked starch masterbatch.

5. The method for preparing the composite flash-steamed nonwoven fabric according to claim 4, characterized in that: The mass ratio of the starch to the sodium alginate is 1:(0.1-0.2).

6. The method for preparing the composite flash-steamed nonwoven fabric according to claim 1, characterized in that: In the composite base fabric, the thickness ratio of the first PBAT film layer, the flash non-woven fabric and the second PBAT film layer is (0.8-1.2):3:(0.8-1.2).

7. The composite flash-steamed nonwoven fabric prepared by the method for preparing the composite flash-steamed nonwoven fabric according to any one of claims 1 to 6.

8. The composite flash-steamed nonwoven fabric according to claim 7, characterized in that: The tensile strength of the composite flash-steamed non-woven fabric tested according to GB / T12914-2018 is greater than or equal to 6 kN / m and less than or equal to 7 kN / m.

9. The composite flash-steamed nonwoven fabric according to claim 7, characterized in that: The composite flash-steamed non-woven fabric has an elongation at break greater than or equal to 25% and less than or equal to 30% tested according to GB / T12914-2018.

10. The composite flash-steamed nonwoven fabric according to claim 7, characterized in that: The tear strength of the composite flash-steamed non-woven fabric tested according to GB / T4744-2013 is greater than or equal to 10N and less than or equal to 11N.

Citation Information

Patent Citations

  • Biomass based composite material with high degradability for non-woven fabric and processing technology of biomass based composite material

    CN110129918A

  • Stable moisture-absorbing fresh-keeping plastic film for food packaging and preparation method thereof

    CN110511416A

  • Micro-nano overlapped bio-based fiber material as well as preparation method and application thereof

    CN116005356A

  • Inorganic filler for PLA (polylactic acid) and PBAT (poly (butyleneadipate-co-terephthalate)) blended degradable plastic

    CN116874884A