Lithium ion secondary battery
By using high-graphitization graphite and a specific proportion of ethyl acetate and bisfluorosulfonyl imide lithium electrolyte in lithium iron phosphate batteries, the problems of insufficient fast charging performance and high temperature storage performance of lithium iron phosphate batteries are solved and achieved Higher energy density and better cycle performance.
Patent Information
- Application Number
- CN202411072466.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-01
AI Technical Summary
Lithium iron phosphate batteries have poor fast charging performance and low energy density, making it difficult to meet the demand for rapid recharge, and have insufficient high-temperature storage performance.
Use graphite with a high degree of graphitization as the negative active material, and use an electrolyte containing ethyl acetate and lithium bisfluorosulfonimide to adjust the degree of graphitization and the content of ethyl acetate and lithium bisfluorosulfonimide. Make it meet a specific relationship (0.1≤(B+C)/A≤0.98) to improve the battery's fast charge cycle performance and high-temperature storage performance.
It effectively takes into account the fast charging cycle performance, energy density and high-temperature storage performance of lithium iron phosphate batteries, improves the charging efficiency and structural stability of the battery, and reduces high-temperature side reactions.
Smart Images

Figure CN118738569A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a lithium ion secondary battery. Background Art
[0002] Lithium-ion batteries are widely used in 3C digital, power tools, aerospace, energy storage, power vehicles and other fields due to their high specific energy, no memory effect, and long cycle life. Lithium iron phosphate batteries have the following advantages: high safety, long cycle life, and low cost, but the ion conductivity and electronic conductivity of lithium iron phosphate are low, resulting in poor fast charging performance; compared with other types of lithium-ion batteries, lithium iron phosphate batteries have a lower energy density, that is, the energy stored per unit volume or weight is relatively small.
[0003] With consumers' demand for fast charging, such as 15 minutes to 80% SOC and 10 minutes to 80% SOC, higher requirements are placed on the fast charging performance of negative electrode materials. Developing lithium iron phosphate batteries that take into account both fast charging and energy density has become a difficulty in the industry. Summary of the invention
[0004] The object of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide a lithium-ion secondary battery. By adopting graphite with a high degree of graphitization and using an electrolyte containing ethyl acetate and lithium bis(fluorosulfonyl)imide, when the degree of graphitization, the contents of ethyl acetate and lithium bis(fluorosulfonyl)imide are adjusted to meet a specific relationship, the fast charging cycle performance and high-temperature storage performance of the battery can be improved.
[0005] In order to achieve the above object, the present invention provides a lithium ion secondary battery, which comprises a positive electrode sheet, a negative electrode sheet and an electrolyte; the positive electrode sheet comprises lithium iron phosphate;
[0006] The negative electrode sheet comprises a negative electrode current collector and a negative electrode active layer disposed on at least one side of the negative electrode current collector; the negative electrode active layer comprises a negative electrode active material, the negative electrode active material comprises graphite, and the graphitization degree of the graphite is denoted as A;
[0007] The electrolyte includes a solvent, and the solvent includes ethyl acetate; the mass percentage of ethyl acetate is recorded as B based on the total mass of the solvent;
[0008] The electrolyte includes an electrolyte lithium salt, and the electrolyte lithium salt includes lithium bis(fluorosulfonyl)imide; based on the total mass of the electrolyte, the mass percentage of lithium bis(fluorosulfonyl)imide is denoted as C;
[0009] Among them, A, B and C satisfy the relationship: 0.1≤(B+C) / A≤0.98.
[0010] The present invention adopts the above technical solution to achieve the following beneficial effects:
[0011] The lithium-ion secondary battery provided by the present invention adopts graphite with a high degree of graphitization as the negative electrode active material, and uses an electrolyte containing ethyl acetate and lithium bis(fluorosulfonyl)imide. When the degree of graphitization, the contents of ethyl acetate and lithium bis(fluorosulfonyl)imide are adjusted to meet a specific relationship, fast charging cycle performance, energy density and high-temperature storage performance can be taken into account.
[0012] The endpoints and any values of the range disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Shown is a schematic structural diagram of a negative electrode sheet in an example of the present invention.
[0014] Reference numerals: 1 - negative electrode current collector; 11 - bottom layer; 12 - surface layer. DETAILED DESCRIPTION
[0015] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0016] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0017] In the present invention, the terms "battery", "lithium battery", "lithium-ion battery" and "lithium-ion secondary battery" all have the same meaning and refer to lithium-ion secondary batteries, which generally include an electrode assembly (such as a positive electrode sheet, a negative electrode sheet and a separator), a container (shell) for accommodating the electrode assembly, and an electrolyte.
[0018] In the present invention, the term "Dv50" refers to the particle size corresponding to when the cumulative volume particle size distribution percentage of a sample reaches 50%. Dv50 can be tested using a laser particle size analyzer.
[0019] In the present invention, the term "low viscosity solvent" refers to a solvent having a viscosity of less than or equal to 0.5 mPa.s. The test method for the viscosity of the solvent includes measuring it by a rheometer according to the rotation method in the national standard GB / T 10247-2008.
[0020] In the present invention, the terms "primary particles" and "secondary particles" have the conventional meanings in the art. The term "primary particle" refers to a single negative electrode active particle; the term "secondary particle" refers to a particle formed by agglomeration of several primary particles, for example: the secondary particle is a particle formed by agglomeration of 2 primary particles, a particle formed by agglomeration of 5 primary particles, a particle formed by agglomeration of 10 primary particles, a particle formed by agglomeration of 50 primary particles, or a particle formed by agglomeration of 100 primary particles.
[0021] The present invention provides a lithium ion secondary battery, the battery comprising a positive electrode sheet, a negative electrode sheet and an electrolyte; the positive electrode sheet comprises lithium iron phosphate; the negative electrode sheet comprises a negative electrode current collector and a negative electrode active layer disposed on at least one side of the negative electrode current collector; the negative electrode active layer comprises a negative electrode active material, the negative electrode active material comprises graphite, and the graphitization degree of the graphite is denoted as A;
[0022] The electrolyte includes a solvent, and the solvent includes ethyl acetate; the mass percentage of ethyl acetate is recorded as B based on the total mass of the solvent;
[0023] The electrolyte includes an electrolyte lithium salt, and the electrolyte lithium salt includes lithium bis(fluorosulfonyl)imide (LiFSI); based on the total mass of the electrolyte, the mass percentage of lithium bis(fluorosulfonyl)imide is denoted as C; wherein A, B and C satisfy the relationship: 0.1≤(B+C) / A≤0.98.
[0024] When the graphitization degree of graphite is high, it has the advantages of high initial efficiency and high specific capacity, but the graphite particle size is large and the distance between graphite layers is small, which is not conducive to the rapid insertion and extraction of lithium ions, and the kinetics are poor, which reduces the fast charging ability of the negative electrode active material.
[0025] In the present invention, ethyl acetate (EA) is a low-viscosity solvent with high conductivity and low viscosity characteristics, which can reduce the migration resistance of lithium ions; LiFSI, as a new type of lithium salt, has the advantages of high ion conductivity and good thermal stability. Adding ethyl acetate and LiFSI to the electrolyte can make up for the poor fast-charging performance caused by insufficient kinetics of the negative electrode material; when B+C is too low, it is not enough to improve the kinetics of the negative electrode material; when B+C is too high, although the kinetic performance is excellent and the battery has good fast-charging performance, the electrolyte has more side reactions at high temperatures and is easy to decompose and produce gas, resulting in poor high-temperature performance of the battery (such as high-temperature storage performance). Therefore, in the present invention, by adjusting A, B and C to satisfy the relationship 0.1≤(B+C) / A≤0.98, it can be ensured that the negative electrode active material has the advantages of high first efficiency and high gram capacity, and can also improve the fast-charging performance of the negative electrode active material, so that the lithium-ion secondary battery of the present invention can take into account fast-charging cycle performance, energy density and high-temperature storage performance.
[0026] In some embodiments, the value of (B+C) / A can be, for example, 0.1, 0.1198, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.977, 0.98, preferably 0.35≤(B+C) / A≤0.85.
[0027] In some embodiments, the graphitization degree A of graphite is 90% to 96%, for example, it can be 90%, 91%, 92%, 93%, 94%, 95%, 96%, and more preferably 92 to 94%. When A, B and C satisfy 0.1≤(B+C) / A≤0.98, when the graphitization degree of graphite is adjusted within the above range, graphite can have the advantages of high first efficiency and high gram capacity. At the same time, graphite is used in combination with ethyl acetate and LiFSI, and the mass percentage relationship of the above three components is adjusted to meet the above conditions, which can further improve the fast charging performance of lithium-ion secondary batteries. If the graphitization degree is too low, the first efficiency and gram capacity of graphite are both low, affecting the energy density of the battery; if the graphitization degree is too high, it is necessary to increase the value of B+C to improve the fast charging performance of the battery, but it is not conducive to improving the high temperature storage performance of the battery.
[0028] The measurement and calculation method of graphitization degree includes determining the graphite (002) crystal plane interlayer spacing d002 by X-ray diffraction method (XRD method), and then substituting it into a specific formula (such as Franklin formula or Mering-Maire formula) for calculation to obtain the specific value of graphitization degree.
[0029] In some embodiments, the mass percentage content B of ethyl acetate is 10% to 70%, for example, it can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, more preferably 20% to 60%. When A, B and C satisfy 0.1≤(B+C) / A≤0.98, when the mass percentage content B of ethyl acetate is adjusted within the above range, the migration resistance of lithium ions can be effectively reduced, and the fast charging cycle performance and high temperature storage performance can be better taken into account, and the kinetics of the negative electrode active material cannot be improved due to too little ethyl acetate, and the electrolyte decomposition and gas production caused by too much ethyl acetate can be avoided.
[0030] In some embodiments, the mass percentage C of lithium bis(fluorosulfonyl)imide is 1.5% to 18%, for example, it can be 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 13.5%, 14%, 15%, 16%, 17%, 18%, more preferably 3% to 13.5% (1MLiFSI is 15% by mass). When A, B and C satisfy 0.1≤(B+C) / A≤0.98, when the mass percentage C of lithium bis(fluorosulfonyl)imide is adjusted within the above range, the ionic conductivity of the electrolyte can be more effectively improved, the migration of lithium ions can be promoted, and the fast charging performance of the battery can be further improved; it can effectively avoid that too little lithium bis(fluorosulfonyl)imide causes B+C to be too low to improve the kinetics of the negative active material, and it can also avoid that too much lithium bis(fluorosulfonyl)imide causes the interface to be unstable, and the fast charging cycle of the battery will deteriorate.
[0031] In some embodiments, the electrolyte lithium salt further includes lithium hexafluorophosphate.
[0032] In some embodiments, the OI value of the graphite in the negative electrode sheet is 5 to 20, for example, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20. The OI value of graphite is achieved by X-ray diffraction (XRD) method, and the OI value of graphite can be obtained by calculating the ratio of the diffraction peak intensity of the (004) crystal plane to the diffraction peak intensity of the (110) crystal plane. The calculation formula is: OI = I (004) / I (110).
[0033] The OI value of graphite represents the orientation of graphite. The lower the OI value, the better the isotropy and dynamics of graphite. However, too low an OI value will cause poor adhesion between graphite and the negative electrode current collector, and low peeling force, resulting in poor battery cycle performance. If the OI value is too high, the dynamics will be poor, the fast charging performance will be poor, the battery cycle expansion will be large, and the cycle performance will be poor. When A, B and C meet 0.1≤(B+C) / A≤0.98, adjusting the OI value of graphite in the range of 1 to 10 can better improve the fast charging performance of the negative electrode active material and the structural stability of the negative electrode, further improve the fast charging performance and cycle performance of lithium-ion secondary batteries, and reduce battery expansion.
[0034] In some embodiments, the Dv50 of the graphite is 1 μm to 30 μm, for example, 1 μm, 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 14 μm, 15 μm, 18 μm, 20 μm, 22 μm, 24 μm, 25 μm, 26 μm, 28 μm, 30 μm, preferably 5 μm to 20 μm. When A, B and C satisfy 0.1≤(B+C) / A≤0.98, when the Dv50 of the graphite is adjusted within the above range, the graphite particles make the lithium ion embedding process easier, and the channels for lithium ion embedding and extraction are shorter, which is beneficial to improving the rate performance and fast charging performance of the battery.
[0035] In some embodiments, the graphite includes artificial graphite and / or natural graphite. The type of graphite is not particularly limited and can be selected as needed. For example, the graphite includes needle coke graphite.
[0036] In some embodiments, Figure 1 As shown, the negative electrode active layer includes a bottom layer 11 close to the negative electrode current collector 1 and a surface layer 12 away from the negative electrode current collector 1, the thickness of the surface layer 12 is H1, and the thickness of the bottom layer 11 is H2. The surface layer includes a first graphite material, and the Dv50 of the first graphite material is 3μm to 10μm; the bottom layer includes a second graphite material, and the Dv50 of the second graphite material is 10μm to 20μm.
[0037] When A, B and C satisfy 0.1≤(B+C) / A≤0.98, although the fast charging performance of the battery can be improved, in order to take into account the high temperature performance of the battery, the amount of ethyl acetate and LiFSI added to the electrolyte cannot be too much, so the improvement of the fast charging performance is limited. Furthermore, the negative electrode active layer adopts a double-layer coating method, the Dv50 of the first graphite material in the surface layer is small, the compaction density is low, the hardness is relatively high, and it is not easy to deform, which can ensure that the surface porosity is high and the surface fast charging ability is relatively strong; the Dv50 of the second graphite material in the bottom layer is large, the compaction density is high, the capacity is high, the degree of graphitization is high, the defects are relatively few, the high-temperature side reactions are few, and the high-temperature performance is relatively good. Therefore, the gradient distribution of the porous structure of the negative electrode sheet is further adjusted to achieve high porosity on the surface and high compaction structure on the bottom layer. While taking into account the high temperature performance, the lithium insertion speed of lithium ions in the negative electrode can be greatly improved, the battery charging efficiency is greatly improved, and the fast charging performance of the battery is further improved.
[0038] In some embodiments, the thickness H1 of the surface layer is 10 μm to 50 μm, for example, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm. The thickness H2 of the bottom layer is 50 μm to 100 μm, for example, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm. When A, B and C satisfy 0.1≤(B+C) / A≤0.98, the high porosity of the surface layer of the negative electrode sheet and the high compaction structure of the bottom layer are adjusted, and the thickness of the surface layer and the bottom layer are adjusted within the above range. The thickness of the surface layer is small, which has little effect on the battery energy density and is also beneficial to improving the fast charging performance of the battery; the thickness of the bottom layer is high, which can ensure that the lithium battery has a high energy density and can better balance the high energy density and fast charging performance of the lithium battery.
[0039] In some embodiments, the first graphite material includes needle coke primary particles; and / or the second graphite material includes needle coke primary particles and needle coke secondary particles. Needle coke is one of the artificial graphites, and has the advantages of low thermal expansion coefficient, low impurity content, high conductivity and easy graphitization.
[0040] Preferably, in the bottom layer of the negative electrode active material layer, the mass ratio of the needle coke primary particles to the needle coke secondary particles is (1-4):1, for example, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1. When the mass ratio of the needle coke primary particles to the needle coke secondary particles is within the above range, the large and small particles are mixed, which is beneficial to improve the compaction density of the bottom layer and improve the capacity of the negative electrode.
[0041] In some embodiments, the negative electrode active material also includes hard carbon; the hard carbon is composed of highly disordered carbon layers, has a large interlayer spacing and a randomly arranged crystal structure, provides more embedding points for lithium ions, and graphite mixed with hard carbon can make the lithium battery have a higher capacity. Preferably, the mass ratio X of graphite to hard carbon satisfies: 1≤X≤2.4, for example, X can be 1, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, 2.2, 2.4, 2.5, 2.8, 3, 3.2, 3.4, 3.5, 3.8, 4.0. When A, B and C satisfy 0.1≤(B+C) / A≤0.98, adding ethyl acetate and LiFSI to the electrolyte and adjusting the graphitization degree of graphite can improve the fast charging performance of the battery, but because the high temperature performance of the battery must be taken into account, the improvement of fast charging performance is limited. Further adjusting the blending of hard carbon into graphite and controlling the blending amount of hard carbon can further improve the fast charging performance of the battery without deteriorating the high temperature performance.
[0042] In some embodiments, when the negative electrode active layer is double-layer coated, the surface layer may include hard carbon, and the bottom layer may include hard carbon, that is, the surface layer includes a first graphite material and hard carbon, and the bottom layer includes a second graphite material and hard carbon. When the negative electrode active layer is double-layer coated, graphite mixed with hard carbon can further improve the fast charging performance of the battery.
[0043] In some embodiments, a carbon coating layer is provided on the surface of at least one side of the negative electrode current collector, and the negative electrode active layer is provided on the surface of the carbon coating layer and / or the surface of the negative electrode current collector. For example, the surfaces of the negative electrode current collector on both opposite sides are provided with carbon coating layers, and the negative electrode active layer is provided on the surface of the carbon coating layer away from the negative electrode current collector; or, the surface of one side of the negative electrode current collector is provided with a carbon coating layer, and the negative electrode active material layer is provided on the surface of the carbon coating layer away from the negative electrode current collector, and the negative electrode active layer is also provided on the surface of the negative electrode current collector where the carbon coating layer is not provided. The carbon coating layer can enhance the stripping rate of the negative electrode sheet, prevent the negative electrode active layer from separating from the negative electrode current collector, and improve the stability of the negative electrode structure.
[0044] In some embodiments, the thickness of the carbon coating layer is recorded as Kμm, and K and B satisfy: 0.07≤K / B≤1.7, for example, the ratio of K / B can be 0.07, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7. Preferably, the thickness K of the carbon coating layer satisfies: 0.5μm≤K≤10μm, for example, K can be 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, more preferably 1μm≤K≤5μm. When the K / B ratio is too large, if K is too large, the carbon coating layer is too thick, the negative electrode active layer is reduced, and the battery energy density is reduced; if B is too small, the ethyl acetate content is too small, and the electrolyte dynamics cannot be effectively improved, which is not conducive to improving the fast charging performance of the battery. When the K / B ratio is too small, if K is too small, the carbon coating layer is too thin, and LiFSI has a corrosive effect on the negative electrode current collector; if B is too large, the ethyl acetate content is high, and the boiling point of ethyl acetate is low, which easily causes the electrolyte to decompose and produce gas, affecting the high-temperature storage performance of the battery. When A, B and C satisfy 0.1≤(B+C) / A≤0.98, when the K / B ratio is adjusted within the above range, the battery's energy density, fast charging performance and high-temperature storage performance can be better balanced.
[0045] In some embodiments, the carbon coating layer includes one or more of carbon black, carbon nanotubes, graphene, hard carbon, and soft carbon.
[0046] In some embodiments, the electrolyte includes a cyclic sulfate additive; based on the total mass of the electrolyte, the mass percentage of the cyclic sulfate additive is 0.1% to 2%, for example, 0.1%, 0.2%, 0.5%, 0.8%, 1.0%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%. When A, B and C satisfy 0.1≤(B+C) / A≤0.98, the cyclic sulfate additive is added to the electrolyte, and the cyclic sulfate additive reacts with the electrolyte to generate lithium sulfite, which can increase ionic conductivity, reduce battery impedance, make the transmission of lithium ions inside the battery smoother, and improve the high-temperature fast charging performance of the battery.
[0047] In some embodiments, the cyclic sulfate additive includes one or more of the following compounds: (Formula I-1, vinyl sulfate DTD), (Formula I-2), (Formula I-3), (Formula I-4),
[0048] (Formula I-5), (Formula I-6),
[0049] (Formula I-7), (Formula I-8, methylene methanedisulfonate, MMDS).
[0050] In some embodiments, the electrolyte includes a carbonate additive; based on the total mass of the electrolyte, the mass percentage of the carbonate additive is 0.1% to 5%, for example, 0.1%, 0.2%, 0.5%, 0.8%, 1.0%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.5%, 4%, 4.5%, 5%. When A, B and C satisfy 0.1≤(B+C) / A≤0.98, the carbonate additive is added to the electrolyte, and the carbonate additive is reduced to form a SEI film at the negative electrode before the ethyl acetate solvent, inhibiting the side reaction on the electrode surface, reducing the generation of side reaction products, and improving the high temperature performance of the battery.
[0051] In some embodiments, the carbonate additive includes at least one of vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VEC), trifluoromethylethylene carbonate (TFEC), 1,2-difluoroethylene carbonate (DFEC), and bis(ethylene carbonate) (EC).
[0052] In some embodiments, the electrolyte further comprises an organic additive containing heteroatoms, wherein the heteroatoms comprise at least one of N, P, B, Si, and F; based on the total mass of the electrolyte, the mass percentage of the organic additive containing heteroatoms is 0.1% to 2.0%, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, etc. Preferably, the organic additive containing heteroatoms comprises at least one of tris(trimethylsilyl)phosphate, triphenylphosphite (TPP), trimethyl phosphite (TMP), tris(trimethylsilyl)borate, and trimethyl borate (TB). When A, B and C satisfy 0.1≤(B+C) / A≤0.98, the above-mentioned organic additive containing heteroatoms is added to the electrolyte. The organic additive containing heteroatoms can react with the electrolyte to form an inorganic layer with high ionic conductivity, which can stabilize the electrode / electrolyte interface, improve the ionic conductivity of the battery and reduce the impedance, thereby improving the fast charging performance of the battery and reducing battery expansion.
[0053] In some embodiments, the electrolyte further includes a lithium salt additive; based on the total mass of the electrolyte, the mass percentage of the lithium salt additive is 0.1% to 1%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%. Preferably, the lithium salt additive includes at least one of lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium tetrafluoroborate, and lithium tetrafluorooxalatophosphate. When A, B, and C satisfy 0.1≤(B+C) / A≤0.98, the above-mentioned lithium salt additive is added to the electrolyte. The lithium salt additive can improve the ionic conductivity of the electrolyte, make the migration rate of lithium ions in the electrolyte faster, and thus improve the fast charging performance of the battery.
[0054] In some embodiments, the electrolyte further includes a second solvent, and the second solvent includes one or more of propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and methyl formate (MA). When A, B, and C satisfy 0.1≤(B+C) / A≤0.98, the electrolyte is adjusted to further add the second solvent, which can make the interface generated by the electrolyte at the negative electrode more stable, reduce the decomposition and gas production of the electrolyte, and reduce the expansion of the battery.
[0055] In some embodiments, the battery further comprises a diaphragm, the diaphragm comprising a base film, a glue layer and a ceramic layer; the ceramic layer is disposed on the surface of at least one side of the base film; the glue layer is disposed on the surface of at least one side of the base film, or is disposed on the surface of the ceramic layer away from the base film. For example, the structure of the diaphragm can be glue layer + ceramic + base film, glue layer + ceramic + base film + glue layer, glue layer + ceramic + base film + ceramic + glue layer, and the structure of the diaphragm is preferably glue layer + ceramic + base film + ceramic + glue layer.
[0056] Preferably, the porosity of the diaphragm is 20% to 60%, for example, it can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, more preferably 35% to 45%. The test method of the porosity of the diaphragm includes using a true density meter for test analysis, applying the Archimedean principle-gas expansion displacement method, using the Boyle's law (PV=nRT) of an inert gas with a small molecular diameter under certain conditions, and measuring the porosity of the sample test cavity (volume 10cm 3 ) is used to accurately measure the true volume of the sample, also called the skeleton volume, by the change in the gas volume of the sample test chamber caused by the sample placed in the test chamber, so as to obtain its true density, true density = mass / true volume Vtrue. The test object is generally a regular shape, V1 = length × width × height. If it is not regular, the drainage method can be used to convert V1, and the porosity = (V1-Vtrue) / V1*100%.
[0057] When A, B and C satisfy 0.1≤(B+C) / A≤0.98, the diaphragm is adjusted to have the above-mentioned structure and porosity. The diaphragm has high porosity and low tortuosity pores, which can improve the liquid phase transmission rate of lithium ions, effectively reduce the average transmission distance of lithium ions, make the lithium ion transmission between the positive and negative electrodes smoother, greatly reduce the lithium ion transmission resistance, and enhance the fast charging capability of the battery.
[0058] In some embodiments, the base film includes at least one of polyethylene PE, polypropylene PP, polyethylene terephthalate, polyimide, and a composite structure of PE and PP.
[0059] In some embodiments, the ceramic layer includes one or more of aluminum oxide Al2O3, aluminum hydroxide, magnesium oxide, aluminum oxide, zirconium oxide, titanium oxide, and silicon oxide.
[0060] In some embodiments, the adhesive layer is a conventional spray-coated adhesive layer, for example, including one or more of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyacrylic resin, polymethyl acrylate, butyl acrylate-acrylonitrile copolymer, polyacrylonitrile, ethylene-acrylic acid copolymer, polyethyl acrylate or sodium carboxymethyl cellulose.
[0061] In some embodiments, in the lithium-ion secondary battery, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector; the positive electrode active material layer includes a positive electrode active material; the positive electrode active material includes lithium iron phosphate. Preferably, the Dv50 of the lithium iron phosphate is 0.5μm-1.5μm; the specific surface area BET is 5m 2 / g-15m 2 / g.
[0062] Preferably, the positive electrode current collector is a plain foil or a carbon-coated aluminum foil, and the thickness of the carbon coating layer is 0.5 μm to 5 μm, preferably 1 μm to 3 μm. The carbon coating layer material includes one or more of carbon black, carbon nanotubes, graphene, hard carbon, and soft carbon.
[0063] In some embodiments, the lithium-ion secondary battery may be a power lithium battery, a consumer lithium battery, or an energy storage lithium battery.
[0064] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0065] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0066] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.
[0067] The batteries of the examples and comparative examples of the present invention were prepared according to the following preparation method, and the differences from Example 1-1 are shown below.
[0068] Example 1-1
[0069] (1) Preparation of positive electrode sheet:
[0070] Lithium iron phosphate (LiFePO4), conductive carbon (Super-P) and polyvinylidene fluoride (PVDF) are mixed in a solvent N-methylpyrrolidone at a mass ratio of about 97:1:2, and stirred evenly to obtain a positive electrode slurry. The slurry is coated on a carbon-coated aluminum foil with a thickness of about 12 μm, dried, cold pressed, and then cut and welded to obtain a positive electrode sheet.
[0071] (2) Preparation of negative electrode sheet:
[0072] Graphite, conductive carbon (Super-P), styrene-butadiene rubber and sodium carboxymethyl cellulose (CMC) were mixed in a solvent deionized water at a mass ratio of about 96.5:1.5:1:1, and stirred evenly to obtain a negative electrode slurry. The slurry was coated on a carbon-coated copper foil with a thickness of about 8 μm, dried, cold pressed, and then cut into pieces and welded to the tabs to obtain a negative electrode sheet.
[0073] (3) Preparation of electrolyte
[0074] In a glove box filled with argon (water <10ppm, oxygen <1ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and ethyl acetate (EA) were mixed uniformly in a mass ratio of 30:(70-B):B, and fully dried lithium hexafluorophosphate, 2.5wt% vinylene carbonate (VC), 0.5wt% fluoroethylene carbonate (FEC) and other additives and LiFSI (specific amounts and selections are shown in Table 1) were quickly added to the mixed solution based on the total mass percentage of the electrolyte, and the electrolyte was obtained by stirring.
[0075] (4) Preparation of lithium-ion batteries
[0076] The positive electrode sheets, separators and negative electrode sheets prepared above are stacked by a Z-type stacking machine to obtain bare cells without liquid injection; the bare cells are placed in outer packaging foil, and the prepared electrolyte is injected into the dried bare cells. After vacuum packaging, standing, formation, secondary sealing, sorting and other processes, the required lithium-ion batteries are obtained.
[0077] (5) Test battery
[0078] Electrochemical performance test: The electrochemical performance test is carried out using the following test methods using a Blue Electric charge and discharge test cabinet:
[0079] (i) 25℃ 4C stage filling anatomy test
[0080] Place the battery in an environment of 25±2℃ for 180min, charge it with 1C0 constant current to 10% SOCC0, and record the voltage V1;
[0081] Transfer 5C0 to constant current charge until 20% SOCC0, record the voltage V2;
[0082] Transfer 5C0 to constant current charge until 30% SOCC0, record the voltage V3;
[0083] Switch to 4.5C0 constant current charging until 40% SOCC0, record the voltage V4;
[0084] Switch to 4.0C0 constant current charging until 50% SOCC0, record the voltage V5;
[0085] Switch to 3.5C0 constant current charging until 60% SOCC0, record the voltage V6;
[0086] Switch to 3.0C0 constant current charging until 70% SOCC0, record the voltage V7;
[0087] Switch to 2.3C0 constant current charging until 82% SOCC0, record the voltage V8;
[0088] Switch to 0.5C0 constant current charging until 95% SOCC0, record the voltage V9;
[0089] Switch to 0.33C constant voltage charging to the upper limit voltage of 3.8V, cut-off current of 0.05C, and stand for 30 minutes; discharge to 2.5V at 1.0C0 constant current, cycle 20 weeks according to the above charge and discharge system, dissect and observe the lithium deposition of the battery. The degree of lithium deposition is divided into four levels: no lithium deposition, slight lithium deposition, lithium deposition and severe lithium deposition. No lithium deposition means that no gray or silver lithium is produced on the surface of the negative electrode; slight lithium deposition means that line-like lithium deposition appears in the middle of the negative electrode, which appears gray; moderate lithium deposition means that the lithium deposition area of the negative electrode diffuses to the edge of the negative electrode on the basis of slight lithium deposition in the middle, and it also appears gray; severe lithium deposition means that the negative electrode has diffused to the entire surface of the electrode on the basis of lithium deposition in the middle, and the silver-white lithium appears on the entire surface of the negative electrode.
[0090] (ii) 45℃ 4C fast charge cycle test
[0091] Place the battery in a 45±2℃ environment for 180min, charge it with 1C0 constant current to 10% SOCC0, and record the voltage V1;
[0092] Transfer 5C0 to constant current charge until 20% SOCC0, record the voltage V2;
[0093] Transfer 5C0 to constant current charge until 30% SOCC0, record the voltage V3;
[0094] Switch to 4.5C0 constant current charging until 40% SOCC0, record the voltage V4;
[0095] Switch to 4.0C0 constant current charging until 50% SOCC0, record the voltage V5;
[0096] Switch to 3.5C0 constant current charging until 60% SOCC0, record the voltage V6;
[0097] Switch to 3.0C0 constant current charging until 70% SOCC0, record the voltage V7;
[0098] Switch to 2.3C0 constant current charging until 82% SOCC0, record the voltage V8;
[0099] Switch to 0.5C0 constant current charging until 95% SOCC0, record the voltage V9;
[0100] Charge at 0.33C constant voltage to an upper limit voltage of 3.8V, with a cut-off current of 0.05C, and let stand for 30min; discharge at 1.0C0 constant current to 2.5V, record the initial discharge capacity C0, and when the cycle reaches n times, record the last discharge capacity Cn. The capacity retention rate of the nth cycle is calculated as follows: Capacity retention rate (%) = Cn / C0 × 100%.
[0101] (iii) Thickness change test at 60℃ 100% SOC for 30 days
[0102] At 25°C, the battery was left to stand for 30 minutes, then charged to 3.8V at a constant current rate of 1C, then charged to 0.05C at a constant voltage of 3.65V and left to stand for 5 minutes. After being stored at 60°C for 30 days, the thickness expansion rate of the battery was measured and calculated by the following formula: Thickness expansion rate = [(thickness after storage - thickness before storage) / thickness before storage] × 100%.
[0103] Examples Example 1-3 and Comparative Example 1-2 were carried out with reference to Example 1-1, with the main differences shown in Table 1. In Example 1, the amount of EA added to the electrolyte was changed; in Examples 1-5, the solvent was 10% EC + 10% EMC + 80% EA. In Example 2, the LiFSI content was changed. In Example 3, the degree of graphitization was changed. In Comparative Example 1, EA was not added. In Comparative Example 2, neither EA nor LiFSI was added.
[0104] Table 1
[0105]
[0106]
[0107] Note: "*" indicates that the corresponding parameter in this embodiment or comparative example is the same as that in Example 1-1. " / " indicates that the corresponding parameter was not tested.
[0108] It can be seen from Table 1 that the present invention adopts graphite with a high degree of graphitization, uses an electrolyte containing ethyl acetate and lithium bis(fluorosulfonyl)imide, and adjusts the degree of graphitization, ethyl acetate and lithium bis(fluorosulfonyl)imide to meet 0.1≤(B+C) / A≤0.98, thereby improving the fast charging cycle performance and high temperature storage performance of the battery.
[0109] Examples The examples 4 to 5 were prepared with reference to the examples 1 to 1, with the main differences shown in Table 2. In the example 4, a negative electrode double-layer coating was added. In the example 5, a negative electrode double-layer coating and a carbon coating layer were added.
[0110] Table 2
[0111]
[0112]
[0113] It can be seen from Table 2 that when A, B and C satisfy 0.1≤(B+C) / A≤0.98, in the negative electrode sheet, the negative electrode active layer adopts a double-layer coating method, which can further improve the fast charging performance of the battery while taking into account the high temperature performance.
[0114] Example 6 was carried out with reference to Example 1-1, except that hard carbon was mixed into the graphite and the mixing ratio of the hard carbon was adjusted. The specific differences are shown in Table 3.
[0115] Table 3
[0116]
[0117] It can be seen from Table 3 that when A, B and C satisfy 0.1≤(B+C) / A≤0.98, mixing hard carbon into graphite and controlling the mixing amount of hard carbon can further improve the fast charging performance of the battery without deteriorating the high temperature performance.
[0118] The Example 7 and Example 8 groups were carried out with reference to Example 1-1, and the specific differences are shown in Table 4. In the Example 7 group, the type of additive in the electrolyte was changed. In the Example 8 group, the porosity of the diaphragm was changed (the porosity of the diaphragm was changed by adjusting the coating of the glue layer).
[0119] Table 4
[0120]
[0121]
[0122] It can be seen from Table 4 that adding cyclic sulfate additives, organic additives containing heteroatoms and lithium salt additives to the electrolyte can improve the high temperature cycle performance of the battery and reduce battery expansion. When the porosity of the separator is within an appropriate range, the high temperature cycle performance of the battery can be improved and the battery expansion can be reduced.
[0123] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0124] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A lithium ion secondary battery, It is characterized in that The lithium-ion secondary battery comprises a positive electrode, a negative electrode and an electrolyte; the positive electrode comprises lithium iron phosphate; The negative electrode sheet comprises a negative electrode current collector and a negative electrode active layer disposed on at least one side of the negative electrode current collector; the negative electrode active layer comprises a negative electrode active material, the negative electrode active material comprises graphite, and the graphitization degree of the graphite is denoted as A; The electrolyte includes a solvent, and the solvent includes ethyl acetate; the mass percentage of ethyl acetate is recorded as B based on the total mass of the solvent; The electrolyte includes an electrolyte lithium salt, and the electrolyte lithium salt includes lithium bis(fluorosulfonyl)imide; based on the total mass of the electrolyte, the mass percentage of lithium bis(fluorosulfonyl)imide is denoted as C; Among them, A, B and C satisfy the relationship: 0.1≤(B+C) / A≤0.
98.
2. The lithium ion secondary battery according to claim 1, It is characterized in that A, B and C satisfy the relationship: 0.35≤(B+C) / A≤0.85; Preferably, the graphitization degree A of the graphite is 90% to 96%; Preferably, the mass percentage content B of ethyl acetate is 10% to 70%; Preferably, the mass percentage C of lithium bis(fluorosulfonyl)imide is 1.5% to 18%.
3. The lithium ion secondary battery according to claim 1, It is characterized in that The OI value of the graphite in the negative electrode sheet is 5 to 20; Preferably, the Dv50 of the graphite is 1 μm to 30 μm; Preferably, the graphite comprises artificial graphite and / or natural graphite; Preferably, the Dv50 of the lithium iron phosphate is 0.5 μm-1.5 μm; and / or the specific surface area of the lithium iron phosphate is 5 m 2 / g-15m 2 / g.
4. The lithium ion secondary battery according to claim 3, It is characterized in that The negative electrode active layer includes a bottom layer close to the negative electrode current collector and a surface layer away from the negative electrode current collector; the surface layer includes a first graphite material, and the Dv50 of the first graphite material is 3 μm to 10 μm; the bottom layer includes a second graphite material, and the Dv50 of the second graphite material is 10 μm to 20 μm; Preferably, the first graphite material comprises needle coke primary particles; and / or, the second graphite material comprises needle coke primary particles and needle coke secondary particles; Preferably, the thickness H1 of the surface layer is 10 μm to 50 μm; and / or the thickness H2 of the bottom layer is 50 μm to 100 μm.
5. The lithium ion secondary battery according to claim 1, It is characterized in that The negative electrode active material also includes hard carbon; Preferably, the mass ratio X of the graphite to the hard carbon satisfies: 1≤X≤2.
4.
6. The lithium ion secondary battery according to any one of claims 1 to 5, It is characterized in that A carbon coating layer is disposed on at least one side of the negative electrode current collector, and the negative electrode active layer is disposed on the surface of the carbon coating layer and / or the surface of the negative electrode current collector; Preferably, the thickness of the carbon coating layer is recorded as K μm, and K and B satisfy: 0.07≤K / B≤1.7; Preferably, K satisfies: 0.5≤K≤10, more preferably 1≤K≤5; Preferably, the carbon coating layer includes one or more of carbon black, carbon nanotubes, graphene, hard carbon and soft carbon.
7. The lithium ion secondary battery according to any one of claims 1 to 5, It is characterized in that The electrolyte includes a cyclic sulfate ester additive; the mass percentage of the cyclic sulfate ester additive is 0.1% to 2% based on the total mass of the electrolyte; Preferably, the cyclic sulfate additive comprises one or more of the following compounds:
8. The lithium ion secondary battery according to any one of claims 1 to 5, It is characterized in that The electrolyte includes a carbonate additive; the mass percentage of the carbonate additive is 0.1% to 5% based on the total mass of the electrolyte; Preferably, the carbonate additive includes at least one of vinylene carbonate, fluoroethylene carbonate, vinyl ethylene carbonate, trifluoromethyl vinyl carbonate, 1,2-difluoroethylene carbonate and bisethylene carbonate.
9. The lithium ion secondary battery according to any one of claims 1 to 5, It is characterized in that The electrolyte further comprises an organic additive containing heteroatoms, wherein the heteroatoms comprise at least one of N, P, B, Si, and F; the mass percentage of the organic additive containing heteroatoms is 0.1% to 2.0% based on the total mass of the electrolyte; Preferably, the heteroatom-containing organic additive includes at least one of tris(trimethylsilyl)phosphate, triphenylphosphite, trimethyl phosphite, tris(trimethylsilyl)borate, and trimethyl borate; Preferably, the electrolyte further comprises a lithium salt additive; the mass percentage of the lithium salt additive is 0.1% to 1% based on the total mass of the electrolyte; Preferably, the lithium salt additive includes at least one of lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium tetrafluoroborate, and lithium tetrafluorooxalatophosphate.
10. The lithium ion secondary battery according to any one of claims 1 to 5, It is characterized in that The solvent also includes one or more of propylene carbonate (PC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and methyl formate (MA); Preferably, the battery further comprises a diaphragm, the diaphragm comprising a base film, a glue layer and a ceramic layer; the ceramic layer is arranged on the surface of at least one side of the base film; the glue layer is arranged on the surface of at least one side of the base film, or is arranged on the surface of the ceramic layer away from the base film; Preferably, the porosity of the separator is 20% to 60%.
Citation Information
Cited By
Lithium ion secondary battery, assembly for preparing lithium ion secondary battery, preparation method, lithium supplementing negative plate and power utilization device
CN119133575A
Battery cell, battery device, and electric device
CN119153759A
Lithium ion battery
CN119181856A
Lithium ion secondary battery
CN119447417A
Lithium ion battery
CN119695245A