Goethite-loaded anion exchange resin, preparation method thereof and application of goethite-loaded anion exchange resin in passive monitoring of arsenic pollution of water body

The adsorbent formed by loading goethite on a modified commercial anion exchange resin solves the problem of low sensitivity and accuracy in monitoring arsenic pollution in water bodies, achieving low-cost and stable arsenic pollution monitoring, and is suitable for low-cost monitoring of arsenic pollution in a wide range of natural waters. Arsenic concentration detection.

CN118744016AActive Publication Date: 2024-10-08CHINA UNIV OF MINING & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410758530.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-08
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

The existing technology has low sensitivity and accuracy in monitoring arsenic pollution in water bodies, and high-precision detection relies on frequent manual sampling and high equipment costs, making it difficult to effectively monitor low concentrations of arsenic in large-scale natural water bodies.

Method used

Modified commercial anion exchange resin is used to form goethite-loaded anion exchange resin by loading goethite. It is used for passive monitoring of arsenic in water. Stable arsenic adsorption performance is achieved through adsorption and desorption cycles, combined with inductively coupled plasma mass spectrometry. method for testing.

Benefits of technology

It achieves stable and low-cost monitoring of arsenic in water bodies, and can effectively detect low arsenic concentrations in a wide range of natural water bodies. The monitoring results reflect the overall pollution status within the monitoring period, reducing labor and equipment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744016A_ABST
    Figure CN118744016A_ABST
Patent Text Reader

Abstract

The invention discloses goethite-loaded anion exchange resin, a preparation method thereof and application of the goethite-loaded anion exchange resin to passive monitoring of arsenic pollution in water. The commercial anion exchange resin is subjected to heating treatment after modification treatment, so that the arsenic adsorption capacity and stability are improved; the response relation between the arsenic adsorption capacity of the goethite-loaded anion exchange resin and the environment arsenic concentration under the flowing condition is obtained through the flowing permeation device, then the goethite-loaded anion exchange resin is used as an adsorption medium to be filled and distributed into a water body to be monitored, recovery is conducted after a period of time, the enriched arsenic is desorbed and detected, and the arsenic concentration in the water body to be monitored is detected. Therefore, the time weighted average concentration of arsenic in the water body in the monitoring period is obtained. Compared with the instantaneous concentration obtained by manually collecting a water sample once, the overall pollution condition in a monitoring period can be better reflected, the goethite-loaded anion exchange resin is recycled after recycling and arsenic desorption, the adsorption rate of arsenic is not obviously changed after five times of circulation, the adsorption capacity still reaches 95% or above of the original adsorption capacity, and the adsorption rate of the goethite-loaded anion exchange resin is greatly improved. And the use cost during application is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of monitoring arsenic content in polluted water bodies, and in particular to a goethite-loaded anion exchange resin and a preparation method thereof, and application of the resin in passive monitoring of arsenic pollution in water bodies. Background Art

[0002] Arsenic (As) is a toxic metalloid element. Long-term exposure to arsenic in the human body can aggravate health problems such as diabetes and cardiovascular disease, and cause cancers such as skin cancer and bladder cancer. Arsenic is used in industrial and agricultural fields such as herbicides, pesticides, semiconductors and alloy production, and is widely present in soil and water. In addition, with the mining of arsenic-containing minerals, the precipitation of arsenic during coal combustion, and the high arsenic groundwater in some areas, arsenic has become one of the most common and most concerned pollutants.

[0003] Arsenic exists mainly in inorganic form in environmental water bodies, and it is generally believed that inorganic arsenic is more toxic than organic arsenic. There are many monitoring methods for pollutants in water bodies, including arsenate. Common methods include using colorimetric kits or electrochemical methods based on the Gu Cai method, molybdenum blue method, fluorescence method, etc. to conduct on-site determination of water samples, but the sensitivity and accuracy of the above on-site determination methods are relatively low. Manually collecting water samples and bringing them back to the laboratory for high-sensitivity detection using methods such as inductively coupled plasma mass spectrometry, hydride generation atomic spectrometry, and graphite furnace atomic absorption spectrometry, but the effectiveness of this type of monitoring is highly dependent on the sampling frequency. When applied on a large scale, it often faces the problem of insufficient human resources, and the discrete monitoring data obtained may miss specific pollution events, such as intermittent industrial source pollutant emissions or arsenic release from farmland soil caused by heavy rains. The above shortcomings can be avoided by using online monitoring devices deployed on site, such as the C310 total arsenic water quality online monitor developed by ZTE Instrument Co., Ltd. (Shenzhen) and the PhotoTek 6000 total arsenic water quality automatic online analyzer developed by Longstone Scientific Instrument Co., Ltd. (Shenzhen). However, the required equipment cost and maintenance costs are relatively high, and they are more suitable for real-time monitoring of point pollution sources such as industrial wastewater discharge outlets, but are difficult to use in scenarios that require large-scale monitoring, such as water source protection and agricultural water environment.

[0004] Since the concentration of arsenic in natural water bodies is usually low, mostly at the microgram per liter level, certain requirements are placed on the accuracy of the monitoring method. There are many methods for detecting arsenic content in the prior art, but the accuracy is low. For example, the on-site monitoring method of the colorimetric kit has relatively low sensitivity and strong subjectivity, while high-precision laboratory analysis relies on frequent manual sampling and transportation. Therefore, there is a lack of a method that has relatively low manpower and equipment costs and is suitable for monitoring arsenic levels in a large range of natural water bodies. Summary of the invention

[0005] Arsenic in surface oxygenated water bodies mainly exists in the form of arsenate, and anion exchange resin can adsorb arsenate in water bodies. However, due to its principle of non-specific adsorption based on ion exchange reaction, it is difficult to ensure the fixation effect of arsenate under the interference of other anions in the environment. In view of the shortcomings of the prior art, the purpose of the present invention is to provide a goethite-loaded anion exchange resin and a preparation method thereof and its application in passive monitoring of arsenic pollution in water bodies. The exchange resin used is based on commercial anion exchange resin and is modified and easy to obtain. The synthesized goethite-loaded anion exchange resin can be recycled after recovery and arsenic desorption to meet the demand as a water arsenic enrichment medium, and has good application prospects.

[0006] In order to solve the deficiencies of the prior art, the technical solution adopted by the present invention is:

[0007] A method for preparing goethite-loaded anion exchange resin comprises the following steps:

[0008] Step 1, weigh 30 g of commercial anion exchange resin as a base material, add it into a 500 mL polypropylene plastic bottle, add 250 mL of 1 mol / L nitric acid, and shake and culture;

[0009] Step 2: After the shaking culture is completed, pour out the nitric acid solution, add 250 ml of deionized water, shake for 10 minutes and then pour out, repeat washing with deionized water twice, add 100 mL of 0.5 mol / L ferric nitrate, shake evenly, add 100 mL of 4 mol / L sodium hydroxide, dilute to a total volume of 500 mL with deionized water, heat the reaction, and complete the loading and conversion of iron ions on the resin;

[0010] Step 3, wash the composite resin twice with deionized water, then add 250 mL of 1 mol / L sodium chloride, shake and react to exchange the hydroxide ions on the surface of the resin, and then wash with deionized water until neutral, to obtain goethite-loaded anion exchange resin.

[0011] As an improvement, the basic skeleton of the anion exchange resin in step 1 is a polypropylene group, and the functional group is a quaternary ammonium group.

[0012] As an improvement, the shaking culture speed in step 1 and step 2 is 100 rpm and the shaking time is 1 hour.

[0013] As an improvement, the heating temperature in step 2 is 70° C. and the heating time is 60 hours.

[0014] As an improvement, the shaking culture speed in step 3 is 100 rpm and the shaking time is 1 hour.

[0015] The composite resin material prepared based on the above preparation method is reddish-brown spherical particles with a particle size of 0.65-0.8 mm; the iron content in the goethite-loaded anion exchange resin is 19.8 mg / g, and it is in the form of goethite and is stably loaded on the resin.

[0016] The goethite-loaded anion exchange resin prepared by the above preparation method is used in passive monitoring of arsenic pollution in water bodies.

[0017] The application of the goethite-loaded anion exchange resin in passive monitoring of arsenic pollution in water bodies comprises the following steps:

[0018] Step 1: Use a flow-through device to confirm the adsorption of arsenate by goethite-loaded anion exchange resin and the response relationship between arsenate in the environment

[0019] Sodium arsenate is dissolved in 0.01 mol / L sodium chloride to prepare a 0.2 mg / L arsenic stock solution; 2 g of goethite-loaded anion exchange resin is weighed and placed in a reaction chamber of a flow-through device, a peristaltic pump is turned on to allow the arsenic solution to flow through the reaction chamber at a uniform speed, and after running for 1-12 hours, the goethite-loaded anion exchange resin is recovered to a 50 mL centrifuge tube, 20 mL of a mixed solution of 0.5 mol / L sodium hydroxide and 0.5 mol / L sodium sulfate is added, and the mixture is shaken at 50 rpm for 16 hours to desorb and extract the arsenic adsorbed on the goethite-loaded anion exchange resin; then, the mixture is filtered through a 0.45 μM filter membrane, and the arsenic content in the filtrate is determined by inductively coupled plasma mass spectrometry, and converted into the adsorption amount of arsenic; and then the response coefficient of the goethite-loaded anion exchange resin to arsenate is obtained by linear fitting;

[0020] Step 2, using a 100-mesh polyester fiber mesh bag to fill 2g of goethite-loaded anion exchange resin, sealing it and placing it in the water body to be monitored, determining the deployment time according to actual conditions, and regularly taking out and replacing the adsorption bag containing the goethite-loaded anion exchange resin; washing the recovered goethite-loaded anion exchange resin with deionized water, transferring it to a 50mL centrifuge tube, and desorbing and extracting arsenic with 20mL of a mixed solution of 0.5mol / L sodium hydroxide and 0.5mol / L sodium sulfate; then passing through a 0.45μM filter membrane, determining the arsenic content in the filtrate by inductively coupled plasma mass spectrometry, and converting the response coefficient to obtain the time-weighted average concentration of arsenic in the water body during the monitoring period.

[0021] As an improvement, the goethite-loaded anion exchange resin has a stable adsorption rate for arsenic during passive monitoring of arsenic pollution in water bodies, and after five adsorption-desorption cycles, the adsorption capacity still reaches more than 95% of the initial adsorption capacity.

[0022] Beneficial Effects

[0023] Compared with the prior art, the goethite-loaded anion exchange resin and its preparation method and application in passive monitoring of arsenic pollution in water bodies involved in the present invention have the following advantages:

[0024] 1. After the commercial anion exchange resin was modified and heated and aged, the iron loading in the goethite-loaded anion exchange resin was firm and the arsenic adsorption performance was stable. After 5 times of adsorption and desorption, the adsorption capacity of the composite resin for arsenic can still reach more than 95% of the original, and the adsorption rate remains stable.

[0025] 2. The monitoring method proposed in the present invention is to obtain the response relationship between the arsenic adsorption amount of the goethite-loaded anion exchange resin and the environmental arsenic concentration through indoor experiments, and then the goethite-loaded anion exchange resin is loaded as an adsorption medium and deployed in the water body to be monitored, recovered after a period of time, and the arsenic enriched in the material is desorbed and detected, thereby obtaining the time-weighted average concentration of arsenic in the water body during the monitoring period. Compared with the instantaneous concentration obtained by manually collecting water samples once, it can better reflect the overall pollution status during the monitoring period.

[0026] 3. Due to the enrichment of arsenic in the adsorption medium, this method also has a good monitoring effect on natural water bodies with low arsenic concentrations. That is, when the arsenic desorbed from the composite resin is measured by inductively coupled plasma mass spectrometry with a detection limit of 0.2μg / L, the corresponding water arsenic detection concentration is 0.021μg / L under the condition of a monitoring period of 7 days, which effectively expands the detection limit of arsenic in water bodies.

[0027] 4. The materials required for the monitoring method of the present invention are cheap and easily available, and the goethite-loaded anion exchange resin can be recycled after recovery and arsenic desorption, which is green and environmentally friendly and further reduces the cost of use in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The X-ray diffraction pattern of goethite-loaded anion exchange resin HD730 prepared in Example 1;

[0029] Figure 2 (a) is the adsorption kinetic curve of arsenic by different anion exchange resins;

[0030] Figure 2 (b) is the pseudo-second-order kinetic model fitting curve of different anion exchange resins, and k is the adsorption rate constant obtained by fitting;

[0031] Figure 3 (a) is the isothermal adsorption curve of arsenic by different anion exchange resins;

[0032] Figure 3 (b) is the Langmuir fitting curve of different anion exchange resins, and Q is the arsenic adsorption capacity obtained by fitting;

[0033] Figure 4 The iron content (a), arsenic adsorption rate constant (b) and arsenic adsorption capacity (c) of the goethite-loaded anion exchange resin prepared in Example 1 after multiple adsorption-elution cycles;

[0034] Figure 5 Schematic diagram of the flow permeation device used in the present invention, wherein 1-Marsh flask, 2-reaction chamber, 3-peristaltic pump;

[0035] Figure 6 The cumulative adsorption amount of arsenic in the goethite-loaded anion exchange resin prepared in Example 1 at different operating times in the response coefficient acquisition experiment;

[0036] Figure 7 To verify the effectiveness of the water arsenic monitoring method;

[0037] Figure 8 The iron content (a), arsenic adsorption rate constant (b) and arsenic adsorption capacity (c) of the iron-loaded anion exchange resin prepared in Comparative Example 1 after multiple adsorption-elution cycles. DETAILED DESCRIPTION

[0038] Example 1 Preparation method of goethite-loaded anion exchange resin

[0039] A method for preparing goethite-loaded anion exchange resin, wherein a commercial anion exchange resin (D730, Hydrolite TM , Zhejiang) as the base material. Specifically, 30g of commercial anion exchange resin was weighed into a 500mL polypropylene plastic bottle, 250mL of 1mol / L nitric acid was added, and the mixture was shaken at 100rpm for 1 hour in an oscillating incubator. After washing with deionized water twice, 100mL of 0.5mol / L ferric nitrate was added, and the mixture was shaken at 100rpm for 1 hour. Then 100mL of 4mol / L sodium hydroxide was added, and deionized water was added to a total volume of 500mL, and the mixture was placed in a 70°C oven and heated for 60 hours to complete the loading and conversion of iron ions on the resin. Finally, the composite resin was washed twice with deionized water, 250mL of 1mol / L sodium chloride was added, and the mixture was shaken at 100rpm for 1 hour to exchange the hydroxide ions on the surface of the resin. After washing with deionized water again, the goethite-loaded anion exchange resin HD730 was obtained.

[0040] To characterize the iron loading of the synthesized resin, 0.1 g of HD730 was weighed and added to a mixed solution of 100 mL of 5% hydroxylamine hydrochloride and 5 mol / L hydrochloric acid. After 10 minutes of ultrasonic water bath at 40 kHz and 120 W, the mixture was shaken at 100 rpm for 24 hours. The supernatant was then filtered through a 0.45 μm filter membrane. The iron concentration in the solution was determined using an inductively coupled plasma mass spectrometer (Agilent 7900, USA) and converted to the iron content in HD730. The result was 19.8 mg / g. In addition, the morphology of the loaded iron was analyzed using X-ray diffraction (XRD). The spectrum showed that the peak shape of the material completely matched the characteristic peak of goethite, proving that the iron loaded by the composite resin HD730 prepared in this example was all in the form of goethite ( Figure 1 Compared with other forms such as amorphous form, goethite is more stable, which is conducive to maintaining constant adsorption characteristics of arsenic (as shown in the following adsorption-desorption cycle test), and meets the needs of being used as an adsorption medium for monitoring arsenic in water bodies.

[0041] Batch experiments were conducted to study the kinetics of arsenic adsorption by goethite-loaded anion exchange resin. Weigh 0.1 g of resin D730 and HD730 into 50 mL centrifuge tubes, add 30 mL of 10 mg / L sodium arsenate solution, and incubate at 25 °C with shaking at 100 rpm. Samples were taken at different times and filtered through a 0.45 μm filter membrane. The arsenic content in the solution was determined using an inductively coupled plasma mass spectrometer (Agilent 7900, USA) in accordance with the national standard "HJ700-2014". The results are shown in Figure 2. Figure 2 As shown in the figure, the solid line is HD730 and the dotted line is D730. It can be seen from the figure that the adsorption of arsenic by the two resins conforms to the pseudo-second-order kinetic model. After loading goethite, the adsorption rate of arsenic by the resin is significantly improved, and the rate constant reaches 0.04g / mg / min.

[0042] The arsenic adsorption capacity of goethite-loaded anion exchange resin was obtained by isothermal adsorption test. Weigh 0.1g of resin D730 and HD730 into 50mL centrifuge tubes, add 30mL of sodium arsenate solution with concentrations ranging from 3-50mg / L, and shake at 100rpm for 1 hour at 25℃. Then take the supernatant and filter it through a 0.45μm filter membrane to determine the arsenic content in the solution. The arsenic adsorption amount was fitted with the arsenic equilibrium concentration, and the results are shown in Figure 3 As shown in the figure, the solid line is HD730 and the dotted line is D730. Figure 3 (a) and Figure 3As can be seen from (b), the adsorption of arsenate by the goethite-loaded anion exchange resin HD730 prepared by the present invention is significantly higher than that by D730, and the adsorption curve conforms to the Langmuir model. Under the condition of initial arsenic concentration of 3-50 mg / L, the maximum adsorption capacity is 11.2 mg / g, which meets the requirements of being used as an adsorption medium for arsenic monitoring in water bodies.

[0043] A mixed solution of 20 mL of 0.5 mol / L sodium hydroxide and 0.5 mol / L sodium sulfate was added to the goethite-loaded anion exchange resin after the above isothermal adsorption test to desorb arsenic. After oscillating at 100 rpm for 24 hours, the resin was washed with deionized water until neutral and oscillated at 100 rpm for 48 hours. Thereafter, the iron content in the resin was determined according to the above method, and the adsorption kinetics and isothermal adsorption tests were performed again. After completion, the arsenic was desorbed again. After 5 cycles, the iron content of each resin and the arsenic adsorption capacity were as follows: Figure 4 As shown in the figure, the solid line is HD730 and the dotted line is D730. It can be seen that after 5 adsorption-elution cycles, the iron content of the composite resin HD730 still reached 94.7% of the original, the adsorption rate constant did not change significantly, and the arsenic adsorption capacity still reached 95.6% of the original.

[0044] Example 2 Acquisition of response coefficient

[0045] In order to effectively monitor the target, the amount of adsorption of the target by the adsorption medium must be linearly related to the exposure amount (proportional to concentration and time). Figure 5 The flow-through device shown in the figure is used to confirm the response relationship between the adsorption amount of arsenate by goethite-loaded anion exchange resin HD730 and the arsenate in the environment. The flow-through device is composed of a Martens flask 1, a reaction chamber 2, and a peristaltic pump 3, wherein the Martens flask 1 is connected to the upper part of the reaction chamber 2 with a 5mm hose, and the lower part of the reaction chamber 2 is connected to the peristaltic pump 3 with a 5mm hose. After passing through the peristaltic pump, the sample liquid to be tested is collected in a plastic bottle.

[0046] Specifically, sodium arsenate is dissolved in 0.01 mol / L sodium chloride to prepare a 0.2 mg / L arsenic stock solution, which is poured into a Martens flask. 2 g of goethite-loaded anion exchange resin HD730 is weighed and placed in the reaction chamber of a flow-through device, and a peristaltic pump is turned on to allow the arsenic solution to flow through the reaction chamber at a uniform speed. After running for different times (1-12 hours), the resin is recovered to a 50 mL centrifuge tube, and after adding 20 mL of a mixed solution of 0.5 mol / L sodium hydroxide and 0.5 mol / L sodium sulfate, the mixture is shaken at 50 rpm for 16 hours to desorb and extract the arsenic adsorbed by the resin (by preparing a resin with a known arsenic adsorption amount, desorbing and extracting it, and calculating the extraction rate after detection, it is known that the extraction rate of the leaching method of the present invention is 99.2%). Afterwards, the arsenic content in the filtrate is determined by inductively coupled plasma mass spectrometry after passing through a 0.45 μM filter membrane, and the arsenic content in the filtrate is converted into the adsorption amount of arsenic by the goethite-loaded anion exchange resin HD730.

[0047] The device operation time and arsenic adsorption amount were fitted (such as Figure 6 ), confirm that the two satisfy a linear relationship within the test range, described by the following formula:

[0048] m t =R s ·c·t

[0049] The response coefficient Rs obtained by the above linear fitting is 0.0023 (hours / liter). Where t is the running time, m t is the amount of arsenic adsorption, and c is the concentration of arsenic in the solution.

[0050] Example 3 Verification of the effect of passive monitoring of arsenic in water based on goethite-loaded anion exchange resin

[0051] Use a 100-mesh polyester fiber mesh bag to fill 2g of goethite-loaded anion exchange resin HD730, seal it and place it in the water body to be monitored. Determine the deployment time according to the actual situation, and regularly remove and replace it with a new HD730 adsorption bag.

[0052] The recovered goethite-loaded anion exchange resin HD730 was washed with deionized water, transferred to a 50 mL centrifuge tube, and then arsenic was desorbed and extracted with a mixed solution of 20 mL 0.5 mol / L sodium hydroxide and 0.5 mol / L sodium sulfate. After that, the arsenic content in the filtrate was determined by inductively coupled plasma mass spectrometry according to the national standard "HJ700-2014" through a 0.45 μM filter membrane, and the time-weighted average concentration of arsenic in the water body during the monitoring period was obtained by the following formula: TWA :

[0053]

[0054] From March to April 2024, a tributary of the Baimahe River in Zoucheng City, Shandong Province (35.43 north latitude, 116.85 east longitude) was selected to verify the monitoring effect according to the above test method. According to the situation of this embodiment, the periodicity was set to 7 days.

[0055] In order to evaluate the monitoring results of arsenic concentration in water bodies using the above method, water samples were collected manually every 3-4 days during the monitoring period, and the arsenic concentration level was determined by inductively coupled plasma mass spectrometry.

[0056] The results are as follows Figure 7 As shown, the solid line represents the time-weighted average concentration of arsenic in water bodies during different monitoring periods of HD730, and the scattered points represent the arsenic content measured by manually collected water samples during the same period. It can be seen from the results in the figure that the water arsenic concentrations obtained by the two monitoring methods are basically the same, which further verifies that the new monitoring method based on goethite-loaded anion exchange resin of the present invention can realize the effective monitoring of arsenic concentration in water bodies.

[0057] In addition, due to the enrichment of arsenic in the goethite-loaded anion exchange resin, the present invention can reflect the overall arsenic pollution level during the two sampling periods and effectively expand the detection limit of arsenic in water bodies. That is, when the arsenic desorbed from the composite resin is measured by inductively coupled plasma mass spectrometry with a detection limit of 0.2 μg / L, the corresponding detection concentration of arsenic in water bodies is 0.021 μg / L when the monitoring period is 7 days.

[0058] Example 4 Passive monitoring of arsenic in water based on goethite-loaded anion exchange resin under different ionic conditions

[0059] In order to test whether different ion conditions interfere with the water arsenic monitoring method of the present invention, the following test was performed.

[0060] Sodium arsenate was used to prepare 0.1, 1, and 10 mg / L arsenic stock solutions, and sodium hydroxide or hydrochloric acid was used to adjust the pH of the solution, or sodium chloride, sodium nitrate, sodium carbonate, and sodium hydrogen phosphate of varying concentrations were added. The prepared solutions were poured into the Martens flask of the flow permeation device, 2 g of goethite-loaded anion exchange resin was weighed and placed in the reaction chamber, and the peristaltic pump was turned on to allow the arsenic solution to flow through the reaction chamber at a uniform speed. After running for 24 hours, the resin was recovered to a 50 mL centrifuge tube, and after adding 20 mL of a mixed solution of 0.5 mol / L sodium hydroxide and 0.5 mol / L sodium sulfate, the resin was shaken at 50 rpm for 16 hours to desorb and extract the arsenic adsorbed on the resin. After that, the 0.45 μM filter membrane was used to determine the arsenic content in the filtrate by inductively coupled plasma mass spectrometry, and converted to the arsenic adsorption amount of the resin and the corresponding arsenic concentration of the stock solution. The results are shown in Table 1.

[0061] Table 1 Arsenic concentration measured by the monitoring method of the present invention under different ion conditions

[0062]

[0063] Note: * indicates that the measured arsenate concentration is significantly different from the result measured under the non-interfering ion environment (p<0.05)

[0064] It can be seen from the table that, except for the highest concentration of phosphate ions coexisting, the arsenic concentrations measured under other ion conditions have no significant difference from the results measured under the non-interfering ion environment.

[0065] Comparative Example 1

[0066] The process is the same as Example 1 except that the step of "heating in an oven at 70° C. for 60 hours" is omitted.

[0067] The material prepared in Comparative Example 1 was subjected to an iron content test, an adsorption kinetics test and an isothermal adsorption test after an adsorption-elution cycle according to the method described in Example 1. The results are shown in FIG. Figure 8 As shown in the figure, without heating treatment, the iron loading on the anion exchange resin is not firm, and the iron content decreases significantly after multiple adsorption-elution cycles. The adsorption rate constant and adsorption capacity of arsenic also decrease significantly, and a stable response coefficient cannot be obtained. Therefore, it is not suitable for passive monitoring of arsenic in water.

[0068] In addition, the cost of the commercial anion resin D730 selected in the present invention is 0.16 yuan / gram, and the cost of the prepared goethite-loaded anion exchange resin is 0.25 yuan / gram. Compared with manual single sampling detection, the additional cost required for the monitoring method proposed in the present invention is less than 0.5 yuan.

Claims

1. A method for preparing goethite-loaded anion exchange resin, characterized in that: The following steps are involved: Step 1, weigh 30 g of commercial anion exchange resin as a base material, add it into a 500 mL polypropylene plastic bottle, add 250 mL of 1 mol / L nitric acid, and shake and culture; Step 2: After the shaking culture is completed, pour out the nitric acid solution, add 250 ml of deionized water, shake for 10 minutes and then pour out, repeat washing with deionized water twice, add 100 mL of 0.5 mol / L ferric nitrate, shake evenly, add 100 mL of 4 mol / L sodium hydroxide, dilute to a total volume of 500 mL with deionized water, heat the reaction, and complete the loading and conversion of iron ions on the resin; Step 3, wash the composite resin twice with deionized water, then add 250 mL 1 mol / L sodium chloride, shake and react to exchange the hydroxide ions on the surface of the resin, and then wash with deionized water until neutral, so as to obtain goethite-loaded anion exchange resin.

2. The method for preparing a goethite-loaded anion exchange resin according to claim 1, characterized in that: The basic skeleton of the anion exchange resin in step 1 is a polypropylene group, and the functional group is a quaternary ammonium group.

3. The method for preparing a goethite-loaded anion exchange resin according to claim 1, characterized in that: The shaking culture speed in step 1 and step 2 is 100 rpm, and the shaking time is 1 hour.

4. The method for preparing a goethite-loaded anion exchange resin according to claim 1, characterized in that: The heating temperature in step 2 is 70° C. and the heating time is 60 hours.

5. The method for preparing a goethite-loaded anion exchange resin according to claim 1, characterized in that: The shaking culture speed in step 3 is 100 rpm, and the shaking time is 1 hour.

6. The goethite-loaded anion exchange resin prepared by any one of the preparation methods described in claims 1 to 5, characterized in that: The composite resin material is reddish brown spherical particles with a particle size of 0.65-0.8 mm; the iron content in the goethite-loaded anion exchange resin is 19.8 mg / g, and it is in the form of goethite and is stably loaded on the resin.

7. Use of goethite-loaded anion exchange resin prepared by any one of the preparation methods described in claims 1-5 in passive monitoring of arsenic pollution in water bodies.

8. The use according to claim 7, characterized in that: The following steps are involved: Step 1: Use a flow-through device to confirm the adsorption of arsenate by goethite-loaded anion exchange resin and the response relationship between arsenate in the environment Sodium arsenate was dissolved in 0.01 mol / L sodium chloride to prepare a 0.2 mg / L arsenic stock solution; 2 g of goethite-loaded anion exchange resin was weighed and placed in the reaction chamber of the flow permeation device, and the peristaltic pump was turned on to allow the arsenic solution to flow through the reaction chamber at a uniform speed. After running for 1-12 hours, the goethite-loaded anion exchange resin was recovered to a 50 mL centrifuge tube, and 20 mL of a mixed solution of 0.5 mol / L sodium hydroxide and 0.5 mol / L sodium sulfate was added, and the mixture was shaken at 50 rpm for 16 hours to desorb and extract the arsenic adsorbed on the goethite-loaded anion exchange resin; then, the arsenic content in the filtrate was determined by inductively coupled plasma mass spectrometry after passing through a 0.45 µM filter membrane, and the arsenic content was converted into the adsorption amount of arsenic; and the response coefficient of the goethite-loaded anion exchange resin to arsenate was obtained by linear fitting; Step 2, using a 100-mesh polyester fiber mesh bag to fill 2 g of goethite-loaded anion exchange resin, sealing it and placing it in the water body to be monitored, determining the deployment time according to the actual situation, and regularly taking out and replacing the adsorption bag containing the goethite-loaded anion exchange resin; The recovered goethite-loaded anion exchange resin was washed with deionized water and transferred to a 50 mL centrifuge tube. Arsenic was then desorbed and extracted using a mixed solution of 20 mL of 0.5 mol / L sodium hydroxide and 0.5 mol / L sodium sulfate. The arsenic content in the filtrate was then determined by inductively coupled plasma mass spectrometry after passing through a 0.45 µM filter membrane. The time-weighted average concentration of arsenic in the water body during the monitoring period was obtained by converting the response coefficient.

9. The use according to claim 7, characterized in that: The goethite-loaded anion exchange resin has a stable adsorption rate for arsenic during passive monitoring of arsenic pollution in water bodies, and after five adsorption-desorption cycles, the adsorption capacity still reaches more than 95% of the initial adsorption capacity.

Citation Information

Patent Citations

  • Goethite modified biochar as well as preparation method and application thereof

    CN108816188A

  • Method for directly separating arsenic from arsenic-containing solution

    CN114892027A

  • Method for determining form of ultra-trace inorganic arsenic in water

    CN114994003A

  • Device for treating arsenic-polluted wastewater by using gangue-based arsenic adsorbent

    CN116212834A

  • Anion resin-based nano cerium-manganese oxide composite material as well as preparation method and application thereof

    CN117181202A