Novel impervious waterproof material for decoration
Through the combination and modification of Portland cement and other materials, the problem of difficult degradation of volatile organic compounds in building materials in high-humidity and high-temperature environments has been solved, and the functions of moisture-proof, odor-free and TVOC reduction have been achieved, and indoor air quality has been improved. and impermeability and water resistance.
Patent Information
- Application Number
- CN202410815957.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-15
AI Technical Summary
Existing building materials are difficult to effectively reduce indoor volatile organic compounds in environments with high humidity and temperature, resulting in a decline in indoor air quality. They lack the functions of moisture-proof, odor-free, and TVOC reduction.
Using a combination of Portland cement, modified diatomite, modified titanium dioxide, gray calcium, silica fume, osmotic crystals and lubricants, the diatomite is modified through low-temperature roasting and alkali washing to increase the number of micropores and specific surface area , combined with potassium permanganate and sulfur-doped titanium dioxide, uses photocatalysis and oxidation to degrade volatile organic compounds, and prevents moisture from entering through dendrite-like crystals.
It achieves effective degradation of indoor volatile organic compounds, improves air quality, has good impermeability and waterproof performance, meets industry standard mechanical properties and reduces TVOC content requirements.
Smart Images

Figure BDA0004907627550000091 
Figure BDA0004907627550000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to a novel anti-seepage and waterproof material for decoration. Background Art
[0002] As people's requirements for quality of life continue to improve, whether indoor air quality is safe and healthy has become a focus of attention. Putty, as an essential building material before painting, will make a great contribution to the improvement of indoor air quality if it has certain functions of moisture-proof, odor-free and TVOC content reduction.
[0003] In the prior art, people often use paints with low volatile organic compound content, and open windows for ventilation to reduce indoor odor and TVOC content. Few building materials have the function of odor removal and TVOC content reduction. However, in some areas with high humidity and high temperature, volatile organic compounds will evaporate due to high humidity and high temperature, seriously reducing indoor air quality. Therefore, it has become a technical problem to be solved urgently by those skilled in the art to propose a backwater putty paste with moisture-proof, odor-free and TVOC content reduction functions. Summary of the invention
[0004] The purpose of the present invention is to provide a backwater putty paste with the functions of moisture-proof, odor-free and TVOC content reduction, which can effectively purify indoor air, degrade indoor volatile organic compounds, and thus improve indoor air quality.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] One of the technical solutions of the present invention:
[0007] A novel anti-seepage and waterproof material for decoration, comprising the following raw materials by weight: 20-40 parts of silicate cement, 10-30 parts of modified diatomaceous earth, 1-10 parts of modified titanium dioxide, 10-20 parts of lime, 5-15 parts of silica fume, 1-5 parts of permeable crystals, 1-5 parts of lubricants and 1-5 parts of water reducing agents;
[0008] Preferably, the following raw materials are included in parts by weight: 30 parts of silicate cement, 20 parts of modified diatomaceous earth, 5 parts of modified titanium dioxide, 15 parts of lime lime, 10 parts of silica fume, 2 parts of infiltration crystallization, 3 parts of lubricant and 3 parts of water reducing agent.
[0009] Furthermore, the preparation method of the modified diatomite comprises the following steps:
[0010] Step 1, calcining and alkali washing the diatomite to obtain primary modified diatomite;
[0011] Step 2, impregnating and modifying the primary modified diatomaceous earth obtained in step 1 to obtain the modified diatomaceous earth;
[0012] Furthermore, in step 1, the calcination is: calcining at 300-400° C. for 3-5 hours;
[0013] Preferably, the calcination temperature is 350°C and the calcination time is 4h;
[0014] Furthermore, in step 1, the alkaline washing is: after the diatomaceous earth is cooled to room temperature, the diatomaceous earth is washed with a sodium hydroxide solution having a concentration of 0.1 mol / L;
[0015] The mass volume ratio of diatomaceous earth to sodium hydroxide solution is 1 g: (20-40) mL, and the elution time is controlled at 30-35 s.
[0016] Preferably, the mass volume ratio of diatomaceous earth to sodium hydroxide solution is 1g:30mL.
[0017] The diatomaceous earth used in the present invention has a certain function of absorbing odor and volatile organic compounds such as formaldehyde. By low-temperature calcination, the number of micropores of the diatomaceous earth can be increased to a certain extent, and the specific surface area of the diatomaceous earth can be increased, thereby effectively improving the absorption of odor and volatile organic compounds by the diatomaceous earth. Moreover, the number of micropores and the pore diameter of the micropores are controlled within a certain range (i.e., the micropore morphology sintered at 300 to 400° C.), which can effectively increase the contact opportunity of titanium dioxide with visible light and ultraviolet rays, and effectively improve the performance of titanium dioxide in photocatalytic decomposition of volatile organic compounds. Furthermore, the present invention controls the calcination temperature to 300~400℃. This is because when the temperature is lower than 300℃, the temperature is too low to effectively increase the number of micropores, the specific surface area is too small, and the adsorption capacity is reduced. When the temperature is too high, the micropore diameter increases, the specific surface area decreases, and the adsorption capacity decreases. In addition, when the temperature is 400~450℃, the number of micropores and the specific surface area are better than 300~400℃, but the reason why the present invention abandons it is that when the temperature is 400~450℃, the micropore diameter is further increased, which is not conducive to the subsequent dendrite-like crystals formed by the infiltration crystallization to block the moisture in the atmosphere, thereby reducing the anti-seepage and waterproof performance.
[0018] The diatomaceous earth used in the present invention has high hydrophilicity, that is, the surface of the diatomaceous earth has more hydrophilic groups, which is very unfavorable for the anti-seepage and waterproof performance of the final putty. The surface modification of the diatomaceous earth with alkali can effectively destroy the hydrophilic groups on the surface of the diatomaceous earth, thereby reducing the absorption of moisture in the atmosphere by the diatomaceous earth, thereby improving the anti-seepage and waterproof performance of the putty.
[0019] Furthermore, in step 2, the impregnation modification is: placing the primary modified diatomaceous earth obtained in step 1 in a potassium permanganate solution with a concentration of 0.1 mol / L, and impregnating for 20 to 40 minutes;
[0020] Wherein, the mass volume ratio of the primary modified diatomaceous earth to the potassium permanganate solution is 1 g: (5-15) mL;
[0021] Preferably, the immersion treatment time is 30 min, and the mass volume ratio of the primary modified diatomaceous earth to the potassium permanganate solution is 1 g:10 mL.
[0022] The invention attaches potassium permanganate to diatomaceous earth, and can achieve degradation of volatile organic matter in an environment with poor light conditions; potassium permanganate has strong oxidizing property, and when attached to diatomaceous earth, it can oxidize reducing volatile organic matter such as formaldehyde into carbon dioxide and water, thereby achieving the effect of reducing the content of indoor volatile organic matter; and the oxidizing property of potassium permanganate is not affected by environmental conditions such as light, so it can effectively improve the air quality in an environment with poor light conditions.
[0023] Furthermore, the preparation method of the modified titanium dioxide comprises the following steps:
[0024] Step 1: mixing thiourea, polyethylene glycol and titanium tetrachloride, and reacting them to obtain sulfur-grafted titanium dioxide;
[0025] Step 2, mixing the sulfur-grafted titanium dioxide obtained in step 1 with activated alumina, and grinding them to obtain the modified titanium dioxide;
[0026] Furthermore, in step 1, the mass volume ratio of the thiourea, polyethylene glycol and titanium tetrachloride (1.5 mol / L) is 2 g: (0.1-0.5) mL: (20-30) mL; the mixing is controlled at a speed of 30 rpm and stirred for 20-30 min;
[0027] Preferably, the mass volume ratio of thiourea, polyethylene glycol and titanium tetrachloride is 2g:0.1mL:25mL, and the stirring time is 25min;
[0028] Furthermore, in step 1, the reaction is: reacting at 5-10 MPa and 200-250° C. for 2-5 h, washing with water after cooling to room temperature, and drying at 50-60° C. for 6-8 h;
[0029] Preferably, the reaction is: reacting at 8 MPa and 220° C. for 3 h, washing with water after cooling to room temperature, and drying at 55° C. for 7 h.
[0030] The present invention uses sulfur-doped titanium dioxide as a photocatalytic photocatalyst, which can effectively narrow the band gap of titanium dioxide, so that it can absorb and utilize visible light; titanium dioxide is a photocatalyst material with good performance, but only using titanium dioxide for photocatalysis can only utilize ultraviolet rays to form photogenerated holes and electrons, and the application conditions are relatively harsh. If it is used in the preparation of putty, combined with natural environmental conditions, it is difficult to achieve effective photocatalytic decomposition of volatile organic compounds in the indoor environment. If sulfur is doped into titanium dioxide, the band gap of titanium dioxide can be effectively narrowed, that is, it can absorb and utilize visible light to form holes and electrons, and effectively enhance the photocatalytic degradation performance in an environment with poor ultraviolet rays.
[0031] Furthermore, in step 2, the mass ratio of the sulfur-grafted titanium dioxide to the activated alumina is 1:(3-5); the grinding is grinding until it passes through a 400-mesh sieve;
[0032] Preferably, the mass ratio of the sulfur-grafted titanium dioxide to the activated alumina is 1:4.
[0033] The present invention mixes titanium dioxide with activated alumina, utilizes the high adsorption of activated alumina to adsorb volatile organic matter in air and modified diatomaceous earth, and transfers the adsorbed volatile organic matter to titanium dioxide, thereby realizing efficient titanium dioxide photocatalytic degradation of organic matter; moreover, activated alumina also has a large number of micropores, which can increase the contact opportunities of titanium dioxide with ultraviolet rays and visible light; in addition, activated chlorine dioxide itself also has excellent properties, such as dehumidification and fire prevention, which add many excellent properties to putty.
[0034] Furthermore, the osmotic crystallization is tartaric acid, sodium silicate or calcium chloride.
[0035] The infiltration crystals added in the present invention can form dendrite-like crystals with the hydration product of putty, calcium hydroxide, that is, if moisture in the atmosphere enters the putty, the formed hydration product will react with the infiltration crystals to form dendrite-like crystals. The presence of dendrite-like crystals can effectively prevent moisture from further entering the putty, reduce the contact between the putty and water, and thus achieve the effect of anti-seepage and waterproofing.
[0036] The second technical solution of the present invention:
[0037] The preparation method of the novel anti-seepage and waterproof material for decoration comprises the following steps:
[0038] The raw materials are weighed according to the mass parts, the silicate cement, modified diatomaceous earth, modified titanium dioxide and lime are premixed, and then the infiltration crystallization, lubricant and water reducing agent are added and mixed to obtain the novel anti-seepage and waterproof material for decoration.
[0039] The third technical solution of the present invention:
[0040] The above-mentioned new anti-seepage and waterproof materials for decoration are used in wall construction.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] The present invention adopts the technical scheme of roasting diatomite and impregnating potassium permanganate, doping sulfur with titanium dioxide to composite activated alumina, and adding infiltration crystallization, so that the back water putty paste has the functions of moisture-proof, odor-free, and reducing TVOC content, effectively purifying indoor air, degrading indoor volatile organic compounds, and improving indoor air quality. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Unless otherwise specified, the "parts" described in the present invention are all based on mass parts; in the following examples, the raw materials are weighed according to 1 part = 1 g.
[0045] The room temperature described in the present invention is 25±2°C.
[0046] In the following embodiments, the novel anti-seepage and waterproof material for decoration comprises the following raw materials in parts by weight: 20 to 40 parts of silicate cement, 10 to 30 parts of modified diatomaceous earth, 1 to 10 parts of modified titanium dioxide, 10 to 20 parts of lime, 5 to 15 parts of silica fume, 1 to 5 parts of infiltration crystals, 1 to 5 parts of lubricants and 1 to 5 parts of water reducers.
[0047] Wherein, the preparation method of the modified diatomite comprises the following steps:
[0048] 1) calcining diatomite at 350° C. for 4 h, and after the diatomite is cooled to room temperature, eluting the diatomite with 30 mL of 0.1 mol / L sodium hydroxide solution, with the elution time controlled at 30 to 35 s, to obtain a primary modified diatomite;
[0049] 2) placing the primary modified diatomite obtained in step 1 in a potassium permanganate solution with a concentration of 0.1 mol / L, with a mass volume ratio of the primary modified diatomite to the potassium permanganate solution of 1 g:10 mL, and immersing for 30 min to obtain the modified diatomite.
[0050] Wherein, the preparation method of the modified titanium dioxide comprises the following steps:
[0051] 1) thiourea, polyethylene glycol and titanium tetrachloride (1.5 mol / L) were mixed in a mass volume ratio of 2 g:0.1 mL:25 mL, the speed was controlled to be 30 rpm and stirred for 25 min, then reacted at 8 MPa and 220° C. for 3 h, washed with water after cooling to room temperature, and dried at 55° C. for 7 h to obtain sulfur-grafted titanium dioxide;
[0052] 2) The sulfur-grafted titanium dioxide obtained in step 1 is mixed with activated alumina in a mass ratio of 1:4, and ground until it passes through a 400-mesh sieve to obtain the modified titanium dioxide.
[0053] Among them, the osmotic crystals are tartaric acid, sodium silicate or calcium chloride. It has been verified that the selection of any one of the three osmotic crystals will not have a decisive influence on the experimental results. Therefore, in the following examples, only tartaric acid is used as an example.
[0054] In the following embodiments, the silicate cement is white silicate cement purchased from Jinan Zhongxin Chemical Co., Ltd.; the diatomaceous earth is high-purity diatomaceous earth purchased from Qiangdong Mineral Products Processing Plant in Lingshou County; the activated alumina is purchased from Jiangxi Xintao Technology Co., Ltd.; the lime is 2000 mesh lime powder purchased from Quzhou Liangcheng Calcium Industry Co., Ltd.; the silica fume is needle-shaped lime silica purchased from Jiangxi Xuerui Powder New Materials Co., Ltd.; the lubricant is a thixotropic lubricant for gypsum cement mortar purchased from Jinan Junhai Chemical Co., Ltd.; the water reducer is a polycarboxylic acid water reducer purchased from Jinan Junhai Chemical Co., Ltd.
[0055] Example 1
[0056] A new type of anti-seepage and waterproof material for decoration
[0057] 1) Weigh each raw material according to the mass fraction recorded in 1# in Table 1;
[0058] 2) primary modification of diatomite: calcining the diatomite weighed in step 1) at 350° C. for 4 h, and after the diatomite is cooled to room temperature, eluting the diatomite with 30 mL of 0.1 mol / L sodium hydroxide solution, the elution time is controlled at 35 s, to obtain primary modified diatomite;
[0059] 3) Impregnating diatomite with potassium permanganate: placing the primary modified diatomite obtained in step 2) in a potassium permanganate solution with a concentration of 0.1 mol / L, the mass volume ratio of the primary modified diatomite to the potassium permanganate solution being 1 g:10 mL, and impregnating for 30 min to obtain modified diatomite;
[0060] 4) Preparation of sulfur-grafted titanium dioxide: thiourea, polyethylene glycol and titanium tetrachloride (1.5 mol / L) were mixed in a mass volume ratio of 2 g:0.1 mL:25 mL, and the mixture was stirred at a speed of 30 rpm for 25 min, and then reacted at 8 MPa and 220°C for 3 h. After cooling to room temperature, the mixture was washed with water and dried at 55°C for 7 h to obtain sulfur-grafted titanium dioxide;
[0061] 5) Titanium dioxide composited with activated alumina: The sulfur-grafted titanium dioxide obtained in step 4) is mixed with activated alumina in a mass ratio of 1:4, and ground to pass through a 400-mesh sieve to obtain modified titanium dioxide;
[0062] 6) Premixing: Mix the silicate cement, lime lime, silica fume weighed in step 1), the modified diatomaceous earth obtained in step 3), and the modified titanium dioxide obtained in step 5), and stir for 30 minutes to obtain a premix;
[0063] 7) Mixing: adding the infiltration crystals, lubricant and water reducing agent weighed in step 1) to the premix obtained in step 6), and mixing for 30 minutes to obtain the novel anti-seepage and waterproof material for decoration.
[0064] Example 2
[0065] A new type of anti-seepage and waterproof material for decoration
[0066] Same as Example 1, except that: each raw material was weighed according to the mass fraction recorded in 2# in Table 1.
[0067] Example 3
[0068] A new type of anti-seepage and waterproof material for decoration
[0069] Same as Example 1, except that: each raw material was weighed according to the mass fraction recorded in 3# in Table 1.
[0070] Table 1 Raw material dosage (parts)
[0071] raw material 1# 2# 3# Portland cement 30 20 40 diatomite 20 10 30 Activated Alumina 4 0.8 8 Gray calcium 15 10 20 Silica Fume 10 5 15 Osmotic crystallization 2 1 5 Lubricants 3 1 5 Water reducing agent 3 1 5
[0072] Comparative Example 1
[0073] A decoration material
[0074] The same as Example 1, except that: Step 2) is to calcine the diatomaceous earth weighed in Step 1) at 350° C. for 4 h, and after the diatomaceous earth is cooled to room temperature, a primary modified diatomaceous earth is obtained.
[0075] Comparative Example 2
[0076] A decoration material
[0077] The same as Example 1, except that: Step 2) is to wash the diatomaceous earth weighed in Step 1) with 30 mL of 0.1 mol / L sodium hydroxide solution, and the washing time is controlled at 35 s to obtain a primary modified diatomaceous earth.
[0078] Comparative Example 3
[0079] A decoration material
[0080] Same as Example 1, except that the calcination temperature in step 2) is 250°C.
[0081] Comparative Example 4
[0082] A decoration material
[0083] Same as Example 1, except that the calcination temperature in step 2) is 425°C.
[0084] Comparative Example 5
[0085] A decoration material
[0086] Same as Example 1, except that the calcination temperature in step 2) is 500°C.
[0087] Comparative Example 6
[0088] A decoration material
[0089] The same as Example 1, except that step 3) is omitted, that is, the addition of potassium permanganate is omitted.
[0090] Comparative Example 7
[0091] A decoration material
[0092] The same as Example 1, the only difference is that step 4) is omitted, that is, titanium dioxide and activated alumina are directly used for compounding.
[0093] Comparative Example 8
[0094] A decoration material
[0095] The same as Example 1, the only difference is that step 5) is omitted, that is, the compounding of titanium dioxide is omitted.
[0096] Comparative Example 9
[0097] A decoration material
[0098] Same as Example 1, except that the addition of osmotic crystallization is omitted.
[0099] Effect verification:
[0100] The mechanical properties of the decoration materials (backwater putty paste) prepared in Examples 1 to 3 and Comparative Examples 1 to 9 were tested according to the method described in the industry standard JC / T 2514-2019. The test results are shown in Table 2.
[0101] Table 2 Mechanical properties test
[0102]
[0103] It can be seen from Table 2 that the decoration material (water-repellent putty paste) prepared by the present invention can meet the mechanical properties specified in the industry standards, and the bonding strength is significantly better than the standard state ≥0.50 given in the industry standards, and ≥0.30 after immersion in water.
[0104] The decoration materials (water-repellent putty pastes) prepared in Examples 1 to 3 and Comparative Examples 1 to 9 were tested for reducing TVOC content. The test method is as follows:
[0105] The decoration materials prepared in Examples 1 to 3 and Comparative Examples 1 to 9 were painted on the wall surface according to the conventional indoor decoration dosage. Under natural conditions (12 h light), air quality was tested according to the national standard GB / T 18883-2022 3 days, 5 days, 10 days, 15 days, 30 days and 60 days after painting. The experimental results are shown in Table 3 (three parallel experiments, and the TVOC content was averaged);
[0106] Table 3 Air quality detection
[0107]
[0108] As shown in Table 3, the decoration material (water-repellent putty paste) prepared by the present invention can effectively absorb indoor volatile organic compounds. After three days, the indoor TVOC content is very close to the national standard (≤0.60 mg / m 3 ), in five days, it fully meets the national standard, and after ten days, the indoor TVOC content can be controlled at 0.35mg / m 3 , which is far below the national standard;
[0109] It can be seen from Comparative Example 1 that the performance of improving indoor air quality is significantly reduced by omitting alkali washing. This is because the excessive hydrophilic groups in the diatomaceous earth increase the moisture in the putty, causing volatile organic matter to evaporate into the indoor air along with the moisture, thereby causing the air quality to deteriorate.
[0110] It can be seen from Comparative Examples 2 to 5 that omitting roasting or roasting at too high or too low a temperature will significantly reduce the performance of improving indoor air quality.
[0111] From Comparative Example 6, it can be seen that even without adding potassium permanganate, the indoor TVOC content can be controlled at 0.35 mg / m 3 , but the TVOC content decreases slowly;
[0112] From Comparative Example 7, it can be seen that although it is possible to absorb TVOC without using sulfur-doped titanium dioxide, the TVOC content decreases very slowly because visible light cannot be used;
[0113] It can be seen from Comparative Example 8 that the addition of titanium is omitted, and only the adsorption performance of diatomaceous earth is utilized. At 15 days, the TVOC content drops to the minimum, and then the TVOC content gradually increases until it stabilizes. This is because diatomaceous earth cannot completely degrade TVOC, and there is adsorption saturation. After adsorption saturation, diatomaceous earth decomposes;
[0114] It can be seen from Comparative Example 9 that the osmotic crystallization can inhibit the further entry of moisture, thereby inhibiting the volatile organic compounds from volatilizing into the indoor air along with the moisture.
[0115] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A new type of anti-seepage and waterproof material for decoration. It is characterized in that The invention comprises the following raw materials in parts by weight: 20 to 40 parts of silicate cement, 10 to 30 parts of modified diatomaceous earth, 1 to 10 parts of modified titanium dioxide, 10 to 20 parts of lime, 5 to 15 parts of silica fume, 1 to 5 parts of infiltration crystallization, 1 to 5 parts of lubricant and 1 to 5 parts of water reducing agent.
2. A novel anti-seepage and waterproof material for decoration according to claim 1, It is characterized in that The preparation method of the modified diatomite comprises the following steps: Step 1, calcining and alkali washing the diatomite to obtain primary modified diatomite; Step 2: The primary modified diatomaceous earth obtained in step 1 is impregnated and modified to obtain the modified diatomaceous earth.
3. A novel anti-seepage and waterproof material for decoration according to claim 2, It is characterized in that The calcination is as follows: calcining at 300-400° C. for 3-5 hours.
4. A novel anti-seepage and waterproof material for decoration according to claim 2, It is characterized in that The impregnation modification is: placing the primary modified diatomaceous earth obtained in step 1 in a potassium permanganate solution for impregnation treatment.
5. A novel anti-seepage and waterproof material for decoration according to claim 1, It is characterized in that The preparation method of the modified titanium dioxide comprises the following steps: Step 1: mixing thiourea, polyethylene glycol and titanium tetrachloride, and reacting them to obtain sulfur-grafted titanium dioxide; Step 2: Mix the sulfur-grafted titanium dioxide obtained in step 1 with activated alumina, and grind them to obtain the modified titanium dioxide.
6. A novel anti-seepage and waterproof material for decoration according to claim 5, It is characterized in that The mass ratio of the sulfur-grafted titanium dioxide to the activated alumina is 1:(3-5).
7. A novel anti-seepage and waterproof material for decoration according to claim 1, It is characterized in that The osmotic crystal is tartaric acid, sodium silicate or calcium chloride.
8. A method for preparing the novel anti-seepage and waterproof material for decoration as claimed in any one of claims 1 to 7, It is characterized in that The following steps are involved: The raw materials are weighed according to the mass parts, the silicate cement, modified diatomaceous earth, modified titanium dioxide and lime are premixed, and then the infiltration crystallization, lubricant and water reducing agent are added and mixed to obtain the novel anti-seepage and waterproof material for decoration.
9. Use of the novel anti-seepage and waterproof material for decoration as claimed in any one of claims 1 to 7 in wall construction.