Rubber composition for tires

Snow, wet road and wear performance balance is addressed by using specific proportions of styrene-butadiene copolymer, butadiene copolymer and thermoplastic resin in the tire rubber composition, combined with white fillers and functional group modifications problem, achieving excellent performance of tires under different road conditions.

CN118786174APending Publication Date: 2024-10-15THE YOKOHAMA RUBBER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023107.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-16
Filing Date
2023-03-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

It is difficult for existing rubber compositions for tires to achieve a high level of balance between snow, wet road and wear resistance properties.

Method used

Using rubber containing styrene-butadiene copolymer and butadiene copolymer, combined with white filler and thermoplastic resin, ensuring a specific difference in glass transition temperature, optimizing the ratio of diene rubber and thermoplastic resin, using a specific Functional group modifications and oil loading to improve snow, wet road and wear resistance.

Benefits of technology

It significantly improves the snow performance, wet road performance and wear resistance of the tire to meet high performance requirements, and ensures good performance of the tire under different road conditions by optimizing the composition of the composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005075100000111
    Figure BDA0005005075100000111
  • Figure BDA0005005075100000121
    Figure BDA0005005075100000121
Patent Text Reader

Abstract

Provided is a rubber composition for tires, which has improved snow performance, wet performance, and wear resistance, and which is capable of highly combining these performances in a balanced manner. A rubber composition for tires, which is obtained by blending 30 parts by mass or more and less than 100 parts by mass of a white filler and 15 parts by mass or more and 80 parts by mass or less of a thermoplastic resin with respect to 100 parts by mass of a diene rubber comprising 55% by mass or more of a styrene-butadiene copolymer having a glass transition temperature of-55 DEG C or less and 5% by mass or more of a butadiene copolymer, in a mixture obtained by blending the diene rubber and the thermoplastic resin at a mass ratio of 1: 1, the difference (Tga-Tgm) between a theoretical value (Tga) of the glass transition temperature of the mixture calculated from the glass transition temperatures of the diene rubber and the thermoplastic resin and a measured value (Tgm) of the glass transition temperature of the mixture is 10 DEG C or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a tire rubber composition intended to be used mainly in the tread portion of a winter tire or an all-season tire. Background Art

[0002] In tires (winter tires, all-season tires) that are assumed to be used on snowy roads, excellent driving performance on snowy roads (snow performance) is required. In addition, as basic performance of tires, excellent driving performance on wet roads (wet road performance) and wear resistance are also required. For example, regarding the tire of Patent Document 1, it is proposed to mix silica and various resin components with styrene-butadiene rubber with a low glass transition temperature, while suppressing the reduction of low-temperature performance and improving performance at room temperature such as wet road performance.

[0003] However, in recent years, the performance requirements for tires have become higher, and the above-mentioned countermeasures alone cannot necessarily be sufficient. Therefore, in the rubber composition for tires, countermeasures for more highly balanced snow performance, wet road performance, and wear resistance are required.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 6888948 Summary of the invention

[0007] Problems to be solved by the invention

[0008] An object of the present invention is to provide a rubber composition for a tire which has improved snow performance, wet performance, and wear resistance and which can achieve these properties in a well-balanced manner.

[0009] Means for solving problems

[0010] The tire rubber composition of the present invention for achieving the above-mentioned object is characterized in that, with respect to 100 parts by mass of a diene rubber comprising 55% by mass or more of a styrene-butadiene copolymer having a glass transition temperature of -55°C or less and 5% by mass or more of a butadiene copolymer, 30 parts by mass or more and less than 100 parts by mass of a white filler and 15 parts by mass or more and less than 80 parts by mass of a thermoplastic resin are mixed, and in a mixture obtained by mixing the diene rubber and the thermoplastic resin in a mass ratio of 1:1, a difference Tga-Tgm between a theoretical value Tga of the glass transition temperature of the mixture calculated from the glass transition temperatures of the diene rubber and the thermoplastic resin and a measured value Tgm of the glass transition temperature of the mixture is 10°C or less.

[0011] Effects of the Invention

[0012] The tire rubber composition of the present invention can improve snow performance, wet performance, and wear resistance by blending a specific thermoplastic resin and a white filler into a diene rubber containing a styrene-butadiene copolymer having a specific glass transition temperature and a predetermined amount of a butadiene copolymer.

[0013] In the present invention, the total amount of oil contained in the tire rubber composition is preferably less than 25 parts by mass based on 100 parts by mass of the diene rubber. This contributes to improving the snow performance.

[0014] In the present invention, the glass transition temperature of the styrene butadiene copolymer is preferably -64°C or lower. In addition, at least one terminal of the styrene butadiene copolymer is preferably modified with a functional group. This contributes to improving snow performance and wet performance.

[0015] In the present invention, the glass transition temperature of the thermoplastic resin is preferably 40° C. to 120° C. In addition, the thermoplastic resin is preferably at least one selected from a resin containing at least one selected from terpene, modified terpene, rosin, rosin ester, C5 component, C9 component, and a resin in which at least a part of the double bonds of these resins are hydrogenated.

[0016] In the present invention, the amount of oil extension in the styrene-butadiene copolymer is preferably 10 parts by mass or less based on 100 parts by mass of the styrene-butadiene copolymer. This contributes to improving the wear resistance.

[0017] In the present invention, it is preferred that the maximum value of the loss tangent tanδ of the tire rubber composition at -40°C to 60°C is tanδ in relation to a rubber composition B having the same composition as the tire rubber composition except that all of the thermoplastic resin is replaced with oil. MAXA , and the maximum value of the loss tangent tanδ of the rubber composition B at -40°C to 60°C MAXB The following formula (1) is satisfied.

[0018] tanδ MAXA / tanδ MAXB > 0.8 (1)

[0019] The above-mentioned tire rubber composition can be suitable for the tread of winter tires and all-season tires. The tire having the tread formed by the above-mentioned tire rubber composition can play a good role in snow performance, wet road performance, and wear resistance due to the excellent physical properties of the above-mentioned tire rubber composition. In addition, the tire using the tire rubber composition of the present invention is preferably a pneumatic tire, but can also be a non-pneumatic tire. In the case of a pneumatic tire, inert gas such as air, nitrogen or other gas can be filled inside it. DETAILED DESCRIPTION

[0020] The rubber component constituting the rubber composition for tire of the present invention is a diene rubber, and in 100% by mass of the diene rubber, 55% by mass or more of a styrene-butadiene copolymer having a glass transition temperature (hereinafter sometimes referred to as "Tg") of -55°C or less must be included. By including a styrene-butadiene copolymer having a Tg of -55°C or less, the dispersibility of silica can be improved, and wear resistance and wet road performance can be ensured. The styrene-butadiene copolymer having a Tg of -55°C or less can be 55% by mass or more in 100% by mass of the diene rubber, preferably 55% to 80% by mass, and more preferably 60% to 75% by mass. If the styrene-butadiene copolymer is less than 55% by mass, the effect of improving the dispersibility of silica cannot be fully obtained, and the wet road performance is reduced.

[0021] If the Tg of the styrene-butadiene copolymer is higher than -55°C, the wet road performance cannot be sufficiently ensured. The Tg may be preferably -64°C or lower, more preferably -65°C or lower, and further preferably -70°C or lower. The Tg of the styrene-butadiene copolymer can be measured as the temperature of the midpoint of the transition region from a thermal analysis chart obtained by differential scanning calorimetry (DSC) under a temperature increase rate condition of 20°C / min. In addition, when the styrene-butadiene copolymer is an oil-extended product, the Tg of the styrene-butadiene copolymer in a state without the oil-extending component (oil) is measured.

[0022] At least one end of the styrene-butadiene copolymer having a Tg of -55°C or less may be modified with a functional group. By modifying the styrene-butadiene copolymer having a Tg of -55°C or less, the dispersibility of silica can be improved, and the rolling resistance of the tire can be reduced. Examples of the functional group include epoxy, carboxyl, amino, hydroxyl, alkoxy, silyl, alkoxysilyl, amide, oxysilyl, silanol, isocyanate, isothiocyanate, carbonyl, aldehyde, and the like, and preferably, a functional group having a polyorganosiloxane structure or an aminosilane structure can be used. By containing a functional group having a polyorganosiloxane structure or an aminosilane structure, the dispersibility of silica can be improved, and the wet road performance can be excellent.

[0023] The styrene content of the styrene-butadiene copolymer is not particularly limited, but can be preferably 5% to 30% by mass, more preferably 8% to 25% by mass. By making the styrene content within such a range, the tire can be made to have low rolling resistance, which is preferred. The styrene content of styrene-butadiene rubber can be measured by 1H-NMR.

[0024] The vinyl content of styrene-butadiene copolymer is not particularly limited, but can be preferably 9 mol% to 45 mol%, more preferably 20 mol% to 45 mol%, further preferably 25 mol% to 45 mol%, and particularly preferably 28 mol% to 42 mol%. By making the vinyl content in such a range, the dispersibility of silica can be made good, the temperature dependence of rolling resistance is small, and wear resistance can be ensured in addition, which is preferred. The vinyl content of styrene-butadiene rubber can be measured by 1H-NMR.

[0025] The styrene butadiene copolymer may contain an oil-filling component. The amount of the oil-filling component may be preferably 10 parts by mass or less relative to 100 parts by mass of the styrene butadiene copolymer. By making the amount of the oil-filling component 10 parts by mass or less, the wear resistance may be effectively improved. The amount of the oil-filling component may be more preferably 8 parts by mass or less, and further preferably 5 parts by mass or less.

[0026] The tire rubber composition of the present invention must contain 5% by mass or more of a butadiene copolymer in 100% by mass of the diene rubber in addition to the above-mentioned styrene butadiene copolymer. By containing the butadiene copolymer, in addition to the above-mentioned performance, the snow performance can be improved. The butadiene copolymer can be 5% by mass or more, preferably 8% by mass or more, and more preferably 10% by mass or more, in 100% by mass of the diene rubber. In addition, the butadiene copolymer can be mixed in 100% by mass of the diene rubber, preferably 65% ​​by mass or less, and more preferably 50% by mass or less. If the butadiene copolymer is less than 5% by mass, the effect of improving the snow performance cannot be fully obtained.

[0027] The tire rubber composition may contain other diene rubbers other than styrene-butadiene copolymer and butadiene copolymer. As other diene rubbers, styrene-butadiene copolymers with a Tg exceeding -55°C, natural rubber, isoprene rubber, butyl rubber, emulsion-polymerized styrene-butadiene rubber, halogenated butyl rubber, nitrile rubber, and modified rubbers to which functional groups are added to these rubbers can be exemplified. These other diene rubbers can be used alone or as any admixture. The content of other diene rubbers can be preferably 40% by mass or less, more preferably 0% by mass to 35% by mass, and further preferably 0% by mass to 25% by mass in 100% by mass of the diene rubber.

[0028] The tire rubber composition is mixed with 30 or more and less than 100 parts by mass of a white filler relative to 100 parts by mass of a diene rubber. By mixing the white filler, wet road performance and low rolling resistance can be excellent. If the white filler is less than 30 parts by mass, the wet road performance and / or low rolling resistance are insufficient. If the white filler is more than 100 parts by mass, the low rolling resistance is worsened. The white filler can be preferably mixed with 40 or more and less than 100 parts by mass, and more preferably mixed with 45 or more and less than 100 parts by mass.

[0029] The type of white filler is not particularly limited, and examples thereof include silicon dioxide, calcium carbonate, magnesium carbonate, talc, clay, aluminum oxide, aluminum hydroxide, titanium oxide, and calcium sulfate. They can be used alone or in combination of two or more. Among them, silicon dioxide is preferred, which can make wet road performance and low heat generation more excellent. As silicon dioxide, materials commonly used in tire rubber compositions can be used, such as wet-process silicon dioxide, dry-process silicon dioxide, or carbon-silicon dioxide (two-phase filler) in which silicon dioxide is supported on the surface of carbon black, and silicon dioxide surface-treated with compounds having reactivity or compatibility with both silicon dioxide and rubber, such as silane coupling agents or polysiloxanes, etc. Among them, wet-process silicon dioxide with hydrated silicic acid as the main component is preferred.

[0030] The tire rubber composition can be mixed with fillers other than the white filler to increase the strength of the rubber composition and ensure tire durability. Examples of other fillers include inorganic fillers such as carbon black, mica, alumina, and barium sulfate, and organic fillers such as cellulose, lecithin, lignin, and dendritic molecules.

[0031] Among them, by mixing carbon black, the strength of the rubber composition can be excellent. As carbon black, furnace black, acetylene black, thermal black, channel black, graphite and other carbon blacks can be mixed. Among them, furnace black is preferred, and as its specific example, SAF, ISAF, ISAF-HS, ISAF-LS, IISAF-HS, HAF, HAF-HS, HAF-LS, FEF and the like can be cited. These carbon blacks can be used alone or in combination of two or more. In addition, surface-treated carbon blacks in which these carbon blacks are chemically modified with various acid compounds can also be used.

[0032] When using silica as a white filler, it is preferred to use a silane coupling agent. By mixing a silane coupling agent, the dispersibility of silica relative to diene rubber can be improved. Regarding the type of silane coupling agent, as long as it can be used for the rubber composition mixed with silica, there is no particular restriction, and examples can be given, such as bis-(3-triethoxysilylpropyl) tetrasulfide, bis(3-triethoxysilylpropyl) disulfide, 3-trimethoxysilylpropylbenzothiazole tetrasulfide, γ-mercaptopropyltriethoxysilane, 3-octanoylthiopropyltriethoxysilane and other sulfur-containing silane coupling agents. Among them, in particular, substances with tetrasulfide bonds in the molecule can be used. The mixing amount of the silane coupling agent can be preferably 3% by mass to 20% by mass, and more preferably 5% by mass to 15% by mass relative to the mixing amount of silica. If the amount of the silane coupling agent blended exceeds 20% by mass of the amount of silica blended, the silane coupling agents condense with each other, and desired hardness and strength cannot be obtained in the rubber composition.

[0033] The tire rubber composition can adjust the temperature dependence of its dynamic viscoelasticity by mixing a specific thermoplastic resin. The specific thermoplastic resin is mixed with 15 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass of the diene rubber, preferably 20 parts by mass or more and 75 parts by mass or less, and more preferably 25 parts by mass or more and 60 parts by mass or less. If the thermoplastic resin is less than 15 parts by mass, the purpose of the present invention such as excellent wear resistance and wet road performance, good low rolling resistance and low temperature dependence cannot be achieved. In addition, if the specific thermoplastic resin exceeds 75 parts by mass, the wear resistance may be reduced.

[0034] The following relationship is satisfied between a specific thermoplastic resin and a diene rubber. That is, in a mixture obtained by mixing the above-mentioned diene rubber and thermoplastic resin in a mass ratio of 1:1, the difference Tga-Tgm between the theoretical value Tga of the glass transition temperature of the mixture calculated from the glass transition temperatures of the diene rubber and the thermoplastic resin and the measured value Tgm of the glass transition temperature of the mixture is 10°C or less. By making the difference Tga-Tgm below 10°C, the wear resistance and wet road performance are excellent, and the rolling resistance can be made small, and the temperature dependence is small. The difference Tga-Tgm can be preferably below 7°C, and more preferably below 5°C. It can be considered that if the difference Tga-Tgm is below 10°C, the diene rubber and the thermoplastic resin are in a compatible relationship, and by mixing the thermoplastic resin in a relatively large amount, the tensile strength at break of the rubber composition is large, which helps to improve the viscoelastic properties such as tanδ. In the present invention, the theoretical value Tga of the glass transition temperature of the mixture can be calculated as a weighted average value from the glass transition temperatures and mass ratios of the diene rubber and the thermoplastic resin. In addition, the glass transition temperatures of the diene rubber and the thermoplastic resin, and the glass transition temperature Tgm of the mixture are measured by measuring a thermogram by differential scanning calorimetry (DSC) at a temperature increase rate of 20°C / min, and are measured as the temperature of the midpoint of the transition region. In addition, when there are multiple transition regions in the thermogram, the midpoint in the largest transition region is set as the glass transition temperature Tgm of the mixture.

[0035] The so-called thermoplastic resin is a resin that is usually mixed with a tire rubber composition, has a molecular weight of about several hundred to several thousand, and has the function of imparting adhesion to the tire rubber composition. As a thermoplastic resin, it is preferably a resin containing at least one selected from terpene, modified terpene, rosin, rosin ester, C5 component, and C9 component. For example, natural resins such as terpene resins, modified terpene resins, rosin resins, and rosin ester resins, and synthetic resins such as petroleum resins containing C5 components and C9 components, coal resins, phenolic resins, and xylene resins can be cited.

[0036] Examples of the terpene resin include α-pinene resin, β-pinene resin, limonene resin, hydrogenated limonene resin, dipentene resin, terpene phenol resin, terpene styrene resin, aromatic modified terpene resin, hydrogenated terpene resin, etc. Examples of the rosin resin include gum rosin, tall oil rosin, wood distilled rosin, hydrogenated rosin, disproportionated rosin, polymerized rosin, modified rosins such as maleic rosin and fumaric rosin, ester derivatives of these rosins such as glycerol ester, pentaerythritol ester, methyl ester and triethylene glycol ester, and rosin-modified phenolic resins.

[0037] Examples of petroleum-based resins include aromatic hydrocarbon resins or saturated or unsaturated aliphatic hydrocarbon resins, such as C5 petroleum resins (aliphatic petroleum resins obtained by polymerizing fractions such as isoprene, 1,3-pentadiene, cyclopentadiene, methylbutene, and pentene), C9 petroleum resins (aromatic petroleum resins obtained by polymerizing fractions such as α-methylstyrene, o-vinyltoluene, m-vinyltoluene, and p-vinyltoluene), and C5C9 copolymer petroleum resins.

[0038] The glass transition temperature (Tg) of the thermoplastic resin may be preferably 40°C to 120°C, preferably 45°C to 115°C, and more preferably 50°C to 110°C. By setting the Tg of the thermoplastic resin to 40°C or more, wet road performance can be improved. In addition, by setting the Tg of the thermoplastic resin to 120°C or less, wear resistance can be improved. The glass transition temperature of the thermoplastic resin can be measured by the above method.

[0039] In the following description, the tire rubber composition of the present invention is referred to as rubber composition A, and a material having the same composition as rubber composition A except that all the thermoplastic resin contained in rubber composition A is replaced with oil is referred to as rubber composition B. In addition, the maximum value of the loss tangent of rubber composition A at -40°C to 60°C is referred to as tan δ MAXA The maximum value of the loss tangent of the rubber composition B at -40°C to 60°C is defined as tan δ MAXB In this case, tanδ is preferably MAXA and tanδ MAXB The relationship of the following formula (1) is satisfied.

[0040] tanδ MAXA / tanδ MAXB > 0.8 (1)

[0041] If the ratio of the maximum loss tangent to tanδ MAXA / tanδ MAXB When the tanδ of the rubber composition for tires of the present invention (rubber composition A) is greater than 0.8, the tensile strength at break of the rubber composition for tires of the present invention (rubber composition A) becomes greater, and the wear resistance of the tires becomes more excellent, which is preferred. Rubber composition B has a tendency to have a high compatibility between the diene rubber and the oil contained therein and a high tensile strength at break. It is estimated that the tanδ of the rubber composition A is MAXA is close to tanδ of rubber composition B MAXB When the value of tanδ is greater than tanδ, the viscoelastic behavior of the rubber composition is similar, the compatibility of the diene rubber and the thermoplastic resin is good, and the thermoplastic resin is inhibited from becoming the starting point of destruction, and the tensile strength at break increases. MAXA / tanδ MAXBIt may be more preferably greater than 0.85, and even more preferably greater than 0.9. MAXA and tanδ MAXB The dynamic viscoelasticity of the cured products of rubber compositions A and B can be measured using a viscoelasticity spectrometer under the conditions of a tensile strain rate of 10±2%, a frequency of 20 Hz, and a temperature of -40°C to 60°C. A viscoelasticity curve with the measured temperature as the horizontal axis and the loss tangent (tanδ) as the vertical axis is obtained, and the maximum values ​​(peak values) of tanδ are respectively set as tanδ MAXA and tanδ MAXB .

[0042] The tire rubber composition of the present invention may further contain oil. The blending amount of the oil may be preferably less than 25 parts by mass, more preferably less than 10 parts by mass, and further preferably 8 parts by mass relative to 100 parts by mass of the diene rubber. By suppressing the amount of oil in this way, it is beneficial to maintain good snow performance. If the blending amount of oil is more than 25 parts by mass, the time-dependent change of snow performance becomes large and it is difficult to maintain good snow performance.

[0043] In the rubber composition for tires, in addition to the above-mentioned components, various compounding agents generally used in rubber compositions for tires such as vulcanization or crosslinking agents, vulcanization accelerators, antioxidants, processing aids, liquid polymers, thermosetting resins, etc. can be mixed according to conventional methods. Such compounding agents can be mixed by a general method to form a rubber composition for vulcanization or crosslinking. The compounding amount of these compounding agents can be the general compounding amount in the past as long as it does not violate the purpose of the present invention. The rubber composition for tires can be modulated by mixing the above-mentioned components using a known rubber mixing machine such as a Banbury mixer, a kneading machine, a roller, etc.

[0044] The tire rubber composition is suitable for forming the tread and sidewall of winter tires and all-season tires that are assumed to run on snowy roads, and is particularly suitable for forming the tread of these tires. The winter tires and all-season tires obtained thereby can well demonstrate snow performance, wet road performance, and wear resistance.

[0045] Hereinafter, the present invention will be further described by way of examples, but the scope of the present invention is not limited to these examples.

[0046] Example

[0047] When preparing 17 kinds of rubber compositions for tires (standard example 1, examples 1 to 8, comparative examples 1 to 8) having the common additive formula shown in Table 3 and composed of the blends shown in Tables 1 and 2, the components other than sulfur and vulcanization accelerator were weighed respectively, and after mixing for 5 minutes in a 1.7-liter closed Banbury mixer, the masterbatch was released outside the mixer and cooled to room temperature. The masterbatch was supplied to the Banbury mixer, sulfur and vulcanization accelerator were added and mixed to obtain a rubber composition for tires. Regarding comparative example 8 in Table 1, since SBR4 is an oil-extended product with 25 parts by mass, the blending amount excluding the oil-extending component is recorded in the brackets at the lower level. The additive formula in Table 3 is recorded in parts by mass relative to 100 parts by mass of the diene rubber recorded in Tables 1 and 2. In addition, the tire rubber compositions of the above-mentioned Examples 1 to 8 and Comparative Examples 1 to 8 were respectively designated as rubber composition A, and a material having the same composition as each rubber composition A except that all the thermoplastic resins were replaced by oil was designated as rubber composition B, and the same preparation was performed as above. Furthermore, in a mixture obtained by mixing the diene rubber and the thermoplastic resin constituting the tire rubber composition of each Example and Comparative Example in a mass ratio of 1:1, the glass transition temperature (Tgm) was measured by the above-mentioned method, and the theoretical value Tga of the glass transition temperature was calculated, and the difference Tga-Tgm from the measured value Tgm of the glass transition temperature was calculated and recorded in Tables 1 and 2. In addition, in Tables 1 and 2, tanδ of each rubber composition A is shown. MAXA Tanδ of each rubber composition B MAXB Ratio tanδ MAXA / tanδ MAXB About tanδ MAXA and tanδ MAXB The dynamic viscoelasticity of the cured products of the rubber compositions A and B was measured using a viscoelasticity spectrometer under the conditions of a tensile strain rate of 10±2%, a frequency of 20 Hz, and a temperature of -40°C to 60°C. The viscoelasticity curve was obtained with the measured temperature as the horizontal axis and the loss tangent (tanδ) as the vertical axis. The maximum values ​​(peak values) of tanδ were taken as tanδ, respectively. MAXA and tanδ MAXB And find out.

[0048] The tire rubber compositions obtained above were vulcanized in a mold of a predetermined shape at 160° C. for 20 minutes to prepare evaluation samples. The evaluation samples obtained were used to measure wear resistance, wet performance, and snow performance by the following methods.

[0049] Wear resistance

[0050] The evaluation samples of the obtained tire rubber composition were measured for wear amount using a Lamborn wear tester (manufactured by Iwamoto Seisakusho Co., Ltd.) in accordance with JIS K6264 under the conditions of a load of 15.0 kg (147.1 N) and a sliding rate of 25%. The reciprocals of the obtained results were calculated and recorded in the "wear resistance" column of Tables 1 and 2 as an index with the reciprocal of the wear amount of Standard Example 1 being 100. The larger the wear resistance index, the better the wear resistance.

[0051] Wet road performance

[0052] The above-mentioned 17 kinds of rubber compositions for tires (standard example 1, comparative examples 1 to 8, and embodiments 1 to 8) were used for the crown to manufacture pneumatic tires (test tires) with a tire size of 195 / 55R15. These test tires were assembled on wheels with a rim size of 15 inches, installed on test vehicles with an air pressure of 230 kPa, and the braking distance from ABS braking at a speed of 40 km / h until the vehicle stopped was measured on a test track consisting of a wet road surface. Regarding the evaluation results, the reciprocal of the measured value is used as an index value with standard example 1 set to 100 and recorded in the "wet road performance" column of Tables 1 and 2. The larger the index value, the shorter the braking distance and the better the wet road performance.

[0053] Snow performance

[0054] The above-mentioned 17 kinds of rubber compositions for tires (standard example 1, comparative examples 1 to 8, and embodiments 1 to 8) were used for the crown to manufacture pneumatic tires (test tires) with a tire size of 195 / 55R15. These test tires were assembled on wheels with a rim size of 15 inches, installed on test vehicles with an air pressure of 230 kPa, and the braking distance from ABS braking at a speed of 40 km / h until the vehicle stopped was measured on a test track consisting of a compacted snow road surface. Regarding the evaluation results, the reciprocal of the measured value is used as an index value with standard example 1 set to 100 and recorded in the "Snow Performance" column of Tables 1 and 2. The larger the index value, the shorter the braking distance and the better the snow performance.

[0055] [Table 1]

[0056]

[0057] [Table 2]

[0058]

[0059] The types of raw materials used in Tables 1 and 2 are shown below.

[0060] NR: Natural rubber, TSR20 (glass transition temperature: -65°C)

[0061] SBR1: a terminal-modified solution-polymerized styrene-butadiene rubber having a polyorganosiloxane structure, Nipol NS612 manufactured by Zeon Co., Ltd. of Japan (glass transition temperature: -61°C, styrene content: 15% by mass, vinyl content: 31 mol%, non-oil-extended product)

[0062] SBR2: a terminal-modified solution-polymerized styrene-butadiene rubber having a polyorganosiloxane structure, Nipol NS616 manufactured by Zeon Co., Ltd. of Japan (glass transition temperature: -23°C, styrene content: 22% by mass, vinyl content: 67 mol%, non-oil-extended product)

[0063] SBR3: terminal-modified solution-polymerized styrene-butadiene rubber produced by batch polymerization, HPR850 manufactured by JSR Corporation (glass transition temperature: -25°C, styrene content: 27% by mass, vinyl content: 59 mol%, non-oil-extended product)

[0064] SBR4: Alkoxysilane-modified solution-polymerized styrene-butadiene rubber produced by continuous polymerization, M2520 manufactured by LG Corporation (glass transition temperature: -48°C, styrene content: 27% by mass, vinyl content: 27 mol%, oil-filling amount: 25 parts by mass)

[0065] BR: Butadiene rubber, Nipol BR1220 manufactured by Nippon Zeon Co., Ltd. (glass transition temperature: -105°C)

[0066] CB: Carbon black, Tokai Carbon Co., Ltd. Seat 7HM

[0067] Silica 1: Zeosil 1165MP manufactured by Solvey (nitrogen adsorption specific surface area: 159 m 2 / g)

[0068] Silica 2: ULTRASIL 9100GR manufactured by Evonic (nitrogen adsorption specific surface area: 220 m 2 / g)

[0069] Silica 3: Zeosil 115GR manufactured by Solvey (nitrogen adsorption specific surface area: 110 m 2 / g)

[0070] Resin 1: Aromatic modified terpene resin, HSR-7 manufactured by Yashara Chemical Co., Ltd. (glass transition temperature: 72°C)

[0071] Resin 2: Aromatic modified terpene resin, YS Resin TO-105 manufactured by Yashara Chemical Co., Ltd. (glass transition temperature: 57° C.)

[0072] Resin 3: Indene resin, FMR0150 manufactured by Mitsui Chemicals, Inc. (glass transition temperature: 89°C)

[0073] Resin 4: Phenol-modified terpene resin, Tamanol 803L manufactured by Arakawa Chemical Industries, Ltd. (glass transition temperature: 95°C)

[0074] Silane coupling agent 1: Sulfur-containing silane coupling agent, bis(3-triethoxysilylpropyl)tetrasulfide, Si69 manufactured by Evonik

[0075] Silane coupling agent 2: 3-octanoylthio-1-propyltriethoxysilane, NXT silane manufactured by Evonik Degussa

[0076] ・Oil: Esutech No. 4S manufactured by Showa Sikkim Oil Co., Ltd.

[0077] [Table 3]

[0078] Mixing amount Antioxidant mass parts 3 Wax mass 1 Sulfur mass 1.5 Vulcanization accelerator mass parts 2

[0079] The types of raw materials used in Table 3 are shown below.

[0080] Antiaging agent: VULANOX 4020 manufactured by LANXESS

[0081] Wax: OZOACE-0015A manufactured by NIPPON SEIRO

[0082] ·Sulfur: Tsurumi Chemical Industry Co., Ltd. Salfux 5

[0083] · Vulcanization accelerator: Noxela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0084] As is clear from Table 2, the tire rubber compositions of Examples 1 to 8 are excellent in wear resistance, wet performance, and snow performance, and these performances are improved in a well-balanced manner.

[0085] On the other hand, it is clear from Table 1 that the rubber composition for tires of Comparative Example 1 does not contain butadiene rubber, so the snow performance is reduced. The rubber composition for tires of Comparative Example 2 has a reduced wet performance due to a small amount of styrene-butadiene rubber mixed. The rubber composition for tires of Comparative Example 3 has a reduced wear resistance and wet performance due to a difference Tga-Tgm exceeding 10°C. The rubber composition for tires of Comparative Example 4 has a reduced wear resistance and snow performance due to an excessive amount of resin. The rubber composition for tires of Comparative Example 5 has a reduced snow performance due to a large amount of silica mixed. The rubber composition for tires of Comparative Example 6 has a reduced wet performance due to a small amount of silica mixed. The rubber composition for tires of Comparative Example 7 has a reduced wear resistance and snow performance due to a high glass transition temperature of styrene-butadiene rubber. The rubber composition for tires of Comparative Example 8 has a reduced wear resistance and snow performance due to a high glass transition temperature of styrene-butadiene rubber.

Claims

1. A rubber composition for a tire, characterized in that: A method of preparing a mixture of at least 30 parts by mass and less than 100 parts by mass of a white filler and at least 15 parts by mass and at most 80 parts by mass of a thermoplastic resin with respect to 100 parts by mass of a diene rubber comprising at least 55% by mass of a styrene-butadiene copolymer having a glass transition temperature of -55°C or less and at least 5% by mass of a butadiene copolymer, wherein the diene rubber and the thermoplastic resin are mixed in a mass ratio of 1:1, wherein a difference Tga-Tgm between a theoretical value Tga of the glass transition temperature of the mixture calculated from the glass transition temperatures of the diene rubber and the thermoplastic resin and a measured value Tgm of the glass transition temperature of the mixture is 10°C or less.

2. The tire rubber composition according to claim 1, characterized in that Less than 25 parts by mass of oil is blended with respect to 100 parts by mass of the diene rubber.

3. The tire rubber composition according to claim 1 or 2, characterized in that: The glass transition temperature of the styrene butadiene copolymer is below -64°C.

4. The tire rubber composition according to any one of claims 1 to 3, characterized in that At least one terminal of the styrene butadiene copolymer is modified with a functional group.

5. The tire rubber composition according to any one of claims 1 to 4, characterized in that The glass transition temperature of the thermoplastic resin is 40°C to 120°C.

6. The rubber composition for a tire according to any one of claims 1 to 5, characterized in that The thermoplastic resin is at least one selected from a resin containing at least one selected from terpene, modified terpene, rosin, rosin ester, C5 component, C9 component, and a resin in which at least a part of double bonds of these resins are hydrogenated.

7. The rubber composition for a tire according to any one of claims 1 to 6, characterized in that The amount of oil extension in the styrene-butadiene copolymer is 10 parts by mass or less based on 100 parts by mass of the styrene-butadiene copolymer.

8. The tire rubber composition according to any one of claims 1 to 7, characterized in that In relation to a rubber composition B having the same composition as the tire rubber composition except that all the thermoplastic resin is replaced with oil, the maximum value tanδ of the loss tangent at -40°C to 60°C of the tire rubber composition MAXA , and the maximum value of the loss tangent tanδ of the rubber composition B at -40°C to 60°C MAXB Satisfies the following formula (1), tanδ MAXA / tanδ MAXB > 0.8 (1)。 9 . A tire comprising a tread portion formed from the rubber composition for a tire according to claim 1 .