Lithium ion battery and electric device using same

By using a specific ratio of electrolyte and manganese-containing cathode active material in lithium-ion batteries, the problems of manganese ion dissolution and structural instability are solved, the cycle stability and low-temperature performance of the battery are improved, and the battery life is extended. , and maintain the normal operation of the battery in low temperature environments.

CN118867390AActive Publication Date: 2024-10-29EVE POWER CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202410939652.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Manganese-containing cathode active materials exhibit problems such as deterioration of power characteristics, attenuation of cycle life, and reduction in available capacity of lithium-ion batteries in low-temperature environments, mainly due to structural instability caused by Mn3+.

Method used

A manganese-containing cathode active material and a specific proportion of electrolyte are used. The electrolyte contains nitrile additives, ester additives and lithium salt additives. By adjusting the ratio of succinonitrile to vinylene carbonate and the lithium salt additives The type and proportion can inhibit the dissolution and migration of manganese ions, promote the formation of a stable SEI film, and reduce the interface impedance and adverse reactions of the electrolyte.

Benefits of technology

It effectively improves the cycle stability and low-temperature performance of lithium-ion batteries, extends the service life of the battery, ensures that the battery can operate normally in an environment of -40°C to 55°C, and optimizes the energy output and cycle efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004945021230000051
    Figure BDA0004945021230000051
  • Figure BDA0004945021230000061
    Figure BDA0004945021230000061
  • Figure BDA0004945021230000101
    Figure BDA0004945021230000101
Patent Text Reader

Abstract

The invention provides a lithium ion battery, which comprises a positive electrode, a negative electrode and an electrolyte, the positive electrode comprises a positive electrode active material containing a manganese element, the electrolyte comprises a lithium salt, a solvent and an additive, and the additive comprises a nitrile additive, an ester additive and a lithium salt additive; the nitrile additive comprises succinonitrile, the ester additive comprises vinylene carbonate, the mass ratio of the succinonitrile to the vinylene carbonate is (0.05-0.3): 1, and the content of the vinylene carbonate in the electrolyte is not more than 2wt%; the ester additive further comprises ethylene sulfate, fluoroethylene carbonate and 1, 3-propane sultone; the lithium salt additive comprises at least one of lithium difluorophosphate, lithium bis (oxalato) difluorophosphate and lithium bis (oxalato) borate. According to the lithium ion battery provided by the invention, manganese ions are effectively prevented from being dissolved out of the positive electrode active material by adopting the electrolyte meeting the conditions, and the low-temperature performance and the cycle output characteristic of the battery applying the electrolyte are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, in particular to a lithium ion battery and an electric device using the same. Background Art

[0002] Lithium-ion batteries are currently the battery system with the best comprehensive performance, with high specific energy, high cycle life, small size, light weight, no memory effect, no pollution, etc., and have rapidly developed into a new generation of energy storage power supply, used for power support in the fields of information technology, electric vehicles and hybrid vehicles, special aerospace, etc. With the widespread use of electronic products, the industry has put forward higher requirements for the battery performance of lithium-ion batteries.

[0003] Manganese-containing positive electrode active materials have the advantages of high theoretical specific capacity, high safety characteristics and low cost, and have become a hot topic in lithium-ion battery research. However, manganese-containing positive electrode active materials have problems such as poor power characteristics of lithium-ion batteries, reduced cycle life, and reduced available capacity under low-temperature conditions. 3+ The existence of the John-Teller effect can easily lead to structural instability of the positive electrode active material during the charge and discharge process, thus resulting in a shorter cycle life.

[0004] Based on the above-mentioned defects of the existing lithium-ion batteries, it is necessary to provide a lithium-ion battery which uses a positive electrode active material containing manganese elements and has good low-temperature performance and good cycle performance. Summary of the invention

[0005] The object of the present invention is to provide a lithium ion battery and an electrical device using the same, so as to enhance the cycle capacity retention rate and low temperature performance of the lithium ion battery and improve the battery output characteristics.

[0006] According to one aspect of the present invention, a lithium ion battery is provided, comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode active material containing a manganese element, the electrolyte comprises a lithium salt, a solvent and an additive, the additive comprising a nitrile additive, an ester additive and a lithium salt additive; the nitrile additive comprises succinonitrile (SN); the ester additive comprises vinylene carbonate (VC), the mass of succinonitrile: the mass of vinylene carbonate = 0.05-0.3:1, and the content of vinyl carbonate in the electrolyte does not exceed 2wt%; the ester additive further comprises vinyl sulfate (DTD), fluoroethylene carbonate (FEC) and 1,3-propane sultone (PS); the lithium salt additive comprises at least one of lithium difluorophosphate (LiPO2F2), lithium bis(oxalatodifluorophosphate) (LiDFOP) and lithium bis(oxalatoborate) (LiBOB). For example, the mass ratio of succinonitrile to vinylene carbonate is 0.05:1, 0.10:1, 0.15:1, 0.20:1, 0.25:1, 0.30:1, and the content of vinylene carbonate in the electrolyte is 0.5wt%, 1wt%, 1.5wt%, 2wt%.

[0007] The lithium-ion battery provided by the present invention effectively inhibits the dissolution of manganese ions from the positive electrode active material by using an electrolyte that meets the above conditions, thereby improving the low temperature performance and cycle output characteristics of the battery using the electrolyte. First, during the operation of the battery, the above electrolyte can effectively reduce the manganese ions dissolved from the positive electrode, slow down the damage to the positive electrode structure, improve the cycle stability of the battery, and extend its service life. Secondly, the SEI film is composed of electrolyte decomposition products, so the composition of the electrolyte has a greater impact on the performance indicators of the SEI film. When an additive that meets the above requirements is selected, the electrolyte can promote the formation of a structurally stable SEI film on the surface of the negative electrode, reduce the interface impedance, reduce the adverse reactions between the electrolyte and the positive and negative electrodes, maintain the stability of the battery interface, help maintain the electrochemical performance of the battery in a low temperature environment, and improve the energy output and cycle efficiency of the battery. In addition, by regulating the ratio of succinonitrile and vinylene carbonate in the electrolyte, the dissolution of manganese ions can be effectively inhibited, thereby reducing the content of manganese ions in the electrolyte, effectively reducing the manganese ions migrating to the surface of the negative electrode, and inhibiting the manganese ions from being reduced to manganese metal at the negative electrode to form manganese deposition, thereby reducing the probability of manganese deposition piercing the SEI film, further maintaining the stability of the electrolyte interface, and optimizing the cycle stability of the battery in a low temperature environment. In particular, the lithium-ion battery can maintain normal operation in an environment of -40°C to 55°C.

[0008] Preferably, based on the total weight of the electrolyte, the content of the ester additive is 3-4 wt %, for example, the content of the ester additive is 3 wt %, 3.5 wt %, or 4 wt %.

[0009] Preferably, based on the total weight of the electrolyte, the content of the lithium salt additive is 1-3 wt %, for example, the content of the lithium salt additive is 1 wt %, 1.5 wt %, 2 wt %, 2.5 wt %, or 3 wt %.

[0010] Preferably, the mass ratio of nitrile additives, ester additives and lithium salt additives is 0.01-1.5:2.5-5:1.5-2.5. For example, the mass ratio of nitrile additives, ester additives and lithium salt additives is 0.01:2.5:1.5, 0.5:3.5:1.8, 0.3:3.8:2, 1:4.5:2.5, 1.5:5:2.5. By comprehensively regulating the content of nitrile additives, ester additives and lithium salt additives in the electrolyte, the stability of the electrolyte interface can be improved, the chemical reaction inside the battery can be made more stable, and the cycle performance and kinetic performance of the battery can be improved while ensuring the good low temperature performance of the battery.

[0011] More preferably, the mass ratio of the nitrile additive, the ester additive and the lithium salt additive is 0.3:3.8:2.

[0012] Preferably, in the ester additive, the mass ratio of vinylene carbonate, vinyl sulfate, fluoroethylene carbonate and 1,3-propane sultone is 1-3: 0.2-0.7: 0.1-0.5: 0.5-1.5. Preferably, the mass ratio of vinylene carbonate, vinyl sulfate, fluoroethylene carbonate and 1,3-propane sultone is 1: 0.7: 0.1: 1.5, 2: 0.5: 0.3: 1, 3: 0.2: 0.5: 0.5. When the mass ratio of the ester additive falls within the above-mentioned mass ratio range, it can not only promote the formation of the SEI film in the first cycle, but also the formed SEI film has good structural stability and flexibility, which is beneficial to reduce the possibility of SEI film rupture caused by volume expansion of the negative electrode material or deposition of manganese ions on the negative electrode surface during lithium ion deintercalation and extraction, inhibit the side reaction of the electrolyte, effectively reduce the loss of active lithium, and reduce the polarization resistance growth rate of the battery containing it during the cyclic charge and discharge process, thereby improving the electrochemical performance of the battery.

[0013] Preferably, the lithium salt additive includes lithium difluorophosphate, lithium bis(oxalato)difluorophosphate and lithium bis(oxalato)borate.

[0014] Preferably, in the lithium salt additive, the mass ratio of lithium difluorophosphate, lithium difluorophosphate bisoxalate and lithium dioxalate borate is 0.5-1.0: 0.5-1.5: 0.1-0.5. Preferably, the mass ratio of lithium difluorophosphate, lithium difluorophosphate bisoxalate and lithium dioxalate borate is 0.5.0: 1.5: 0.5, 0.7: 1: 0.3, 0.5: 0.5: 0.1. When the mass ratio of lithium salt additives falls within the above mass ratio range, it can improve the transport performance of lithium ions in the SEI film, which is beneficial to the lithium deintercalation of the negative electrode, and can reduce the interfacial impedance of the SEI film, slowing down the aging of the SEI film during the battery cycle. In addition, the lithium salt additive can participate in the film formation process of the positive electrode and the negative electrode, and can effectively improve the film formation performance and thermal stability of the positive electrode and the negative electrode.

[0015] More preferably, in the lithium salt additive, the mass ratio of lithium difluorophosphate, lithium bis(oxalatodifluorophosphate) and lithium bis(oxalatoborate) is 0.7:1:0.3.

[0016] Preferably, the content of the additive is 5-8wt% based on the total mass of the electrolyte. For example, the content of the additive is 5wt%, 6wt%, 7wt%, 8wt%. When the amount of the additive added to the electrolyte is within the above range, the prepared lithium-ion battery has excellent low-temperature output performance and cycle performance, and can still maintain an excellent battery capacity retention rate in a low-temperature use environment.

[0017] Preferably, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI); the concentration of the lithium salt in the electrolyte is 0.5 to 1.5 mol / L. For example, the concentration of the lithium salt in the electrolyte is 0.5 mol / L, 1 mol / L, and 1.5 mol / L. By selecting the above-mentioned mixed lithium salt and regulating the concentration of the lithium salt in the electrolyte, on the one hand, the number of free lithium ions in the electrolyte can be increased, the migration efficiency of lithium ions can be promoted, and the current transmission speed can be increased. On the other hand, the electrolyte prepared by combining the lithium salt with the above-mentioned additives has good thermal stability and low viscosity characteristics. The electrolyte has good wettability to the positive and negative electrodes, which is beneficial to improving the battery kinetics, further reducing the internal resistance of the battery, and improving the output performance of the battery.

[0018] More preferably, the concentration of the lithium salt in the electrolyte is 1 mol / L.

[0019] Preferably, the lithium salt includes lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI).

[0020] Preferably, in the lithium salt, the mass ratio of lithium hexafluorophosphate to lithium bisfluorosulfonyl imide is 0.8-1.2:0.8-1.2. For example, the mass ratio of lithium hexafluorophosphate to lithium bisfluorosulfonyl imide is 0.8:1.2, 0.9:1.1, 1:1, 1.1:0.9, 1.2:0.8. By optimizing the mass ratio of lithium hexafluorophosphate to lithium bisfluorosulfonyl imide in the above manner, the conductivity of the electrolyte can be improved, the transmission efficiency of lithium ions can be improved, thereby improving the lithium precipitation phenomenon of the negative electrode, improving the battery output characteristics, and extending the battery life.

[0021] More preferably, in the lithium salt, the mass ratio of lithium hexafluorophosphate to lithium bis(fluorosulfonyl)imide is 1:1.

[0022] Preferably, the solvent includes at least one of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC).

[0023] Preferably, the solvent includes ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC). By selecting the above-mentioned composite organic solvent as the solvent in the electrolyte, not only can the compatibility between the additives, lithium salts and solvents in the electrolyte be improved, but it is also conducive to forming an electrolyte system with high dielectric constant, low viscosity and low melting point. In particular, when the mass ratio of nitrile additives, ester additives and lithium salt additives in the electrolyte falls within the range of 0.01-1.5:2.5-5:1.5-2.5, the SEI film formed has a low solubility in the above-mentioned composite organic solvent and can exist stably, and the above-mentioned composite organic solvent is difficult to pass through the SEI film, which is conducive to preventing the co-embedding of the solvent, thereby avoiding the damage of the solvent to the negative electrode material due to co-embedding and improving the service life of the battery.

[0024] Preferably, in the solvent, the mass ratio of ethylene carbonate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 0.8-1.2: 0.8-1.2: 2.5-3.5: 1.6-1.8. For example, the mass ratio of ethylene carbonate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 0.8: 1.2: 2.5: 1.6, 1: 1: 3: 1.7, 1.2: 0.8: 3.5: 1.8.

[0025] More preferably, in the solvent, the mass ratio of ethylene carbonate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:3:1.6 to 1.8. For example, the mass ratio of ethylene carbonate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:3:1.6, 1:1:3:1.7, 1:1:3:1.8.

[0026] Preferably, the positive electrode active material includes lithium iron manganese phosphate. Lithium iron manganese phosphate is a lithium-ion secondary battery with a very broad application prospect, and lithium iron phosphate has the advantages of high energy density, abundant raw material resources, low cost, environmental friendliness, and high safety. Under normal circumstances, the John-Teller effect will occur in lithium iron manganese phosphate during the battery cell cycle, which increases the amount of manganese ions dissolved in the electrolyte and affects the battery cycle capacity. By selecting the above-mentioned electrolyte and the lithium iron manganese phosphate positive electrode active material, the dissolution of manganese ions can be effectively inhibited, thereby reducing the content of manganese ions in the electrolyte, and improving the low temperature performance and cycle performance of the battery while meeting the high energy density of the battery.

[0027] Preferably, the active material of the negative electrode includes at least one of graphite and silicon carbon.

[0028] Preferably, the active material of the negative electrode includes graphite.

[0029] Preferably, the lithium-ion battery further comprises a separator disposed between the positive electrode and the negative electrode, and the separator comprises at least one of polypropylene, polyvinylidene fluoride, polytetrafluoroethylene, polyacrylonitrile and polyethylene.

[0030] Preferably, the membrane comprises polyethylene.

[0031] According to another aspect of the present invention, there is provided an electrical device comprising the above-mentioned lithium-ion battery. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0033] Example 1

[0034] This embodiment provides a lithium-ion battery, including a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte.

[0035] (1) Electrolyte:

[0036] The composition of the electrolyte is shown in Table 1:

[0037] Table 1. Raw material composition of the electrolyte used to prepare the battery provided in Example 1

[0038]

[0039]

[0040] Note: The ratios in Table 1 are mass ratios, such as "lithium hexafluorophosphate: lithium bis(fluorosulfonyl)imide = 1:1", which means the mass ratio of lithium hexafluorophosphate to lithium bis(fluorosulfonyl)imide is 1:1; and so on, such as "ethylene carbonate: propylene carbonate: dimethyl carbonate: ethyl methyl carbonate = 1:1:3:1.67", which means the mass ratio of ethylene carbonate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:1:3:1.67, and they are mixed as organic solvents.

[0041] Prepare the raw materials according to the above raw material composition, and prepare the electrolyte according to the following steps: under the environment of temperature 20-25°C, humidity ≤1%, oxygen content ≤1ppm, and water content ≤0.1ppm, first mix the solvent evenly, then add lithium salt and additives to the solvent, and mix evenly to obtain the electrolyte.

[0042] (2) Lithium-ion battery:

[0043] Lithium iron manganese phosphate is used as the positive electrode active material, graphite is used as the negative electrode active material, and PE+OBS separator is used as the separator. The positive electrode, separator and negative electrode are stacked in order, and a battery cell is obtained through a stacking process. The battery cell is placed in an outer packaging shell, dried, and electrolyte is injected at an electrolyte injection coefficient of 4.4g / Ah. After vacuum packaging, standing, formation, and capacity division processes, a lithium-ion battery is obtained.

[0044] Example 2

[0045] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, the feeding amount of succinonitrile and the solvent is adjusted so that the mass ratio of succinonitrile to vinylene carbonate is 0.3:1. The rest of the raw material ratios and the preparation method are strictly consistent with those in Example 1.

[0046] Example 3

[0047] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, an equal mass of lithium difluorophosphate is used to replace the lithium salt additive in Example 1, that is, this embodiment uses a single lithium salt additive. The rest of the raw material ratios and preparation methods are strictly consistent with Example 1.

[0048] Example 4

[0049] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, an equal mass of lithium bis(oxalyl)difluorophosphate is used to replace the lithium salt additive in Example 1, that is, this embodiment uses a single lithium salt additive. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0050] Example 5

[0051] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, an equal mass of lithium bis(oxalato)borate is used to replace the lithium salt additive in Example 1, that is, this embodiment uses a single lithium salt additive. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0052] Example 6

[0053] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, a mixed lithium salt additive of lithium difluorophosphate and lithium bis(oxalate) difluorophosphate with the same mass is used to replace the lithium salt additive in Example 1, and the mass ratio of lithium difluorophosphate to lithium bis(oxalate) difluorophosphate is 0.7:1. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0054] Example 7

[0055] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, a mixed lithium salt additive of lithium difluorophosphate and lithium dioxalate borate of equal mass is used to replace the lithium salt additive in Example 1, and the mass ratio of lithium difluorophosphate to lithium dioxalate borate is 0.7:0.3. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0056] Example 8

[0057] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, a mixed lithium salt additive of lithium bis(oxalate difluorophosphate) and lithium bis(oxalate borate) of equal mass is used to replace the lithium salt additive in Example 1, and the mass ratio of lithium bis(oxalate difluorophosphate) to lithium bis(oxalate borate) is 1:0.3. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0058] Example 9

[0059] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, lithium hexafluorophosphate of equal mass is used to replace the lithium bis(fluorosulfonyl)imide in Example 1. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0060] Example 10

[0061] This embodiment refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this embodiment and Example 1 is that in the process of preparing the electrolyte, an equal mass of lithium bis(fluorosulfonyl)imide is used to replace the lithium hexafluorophosphate in Example 1. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0062] Comparative Example 1

[0063] This comparative example refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this comparative example and Example 1 is that in the process of preparing the electrolyte, an equal mass of solvent is used to replace the fluoroethylene carbonate in Example 1. The rest of the raw material ratios and preparation methods are strictly consistent with Example 1.

[0064] Comparative Example 2

[0065] This comparative example refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this comparative example and Example 1 is that in the process of preparing the electrolyte, the feeding amounts of ethylene carbonate, succinonitrile and solvent are adjusted so that the content of ethylene carbonate in the electrolyte is 3wt%, and the mass ratio of succinonitrile to ethylene carbonate is consistent with that in Example 1. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0066] Comparative Example 3

[0067] This comparative example refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this comparative example and Example 1 is that in the process of preparing the electrolyte, an equal mass of lithium tetrafluoroborate is used to replace the lithium salt additive in Example 1. The rest of the raw material ratios and preparation methods are strictly consistent with Example 1.

[0068] Comparative Example 4

[0069] This comparative example refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this comparative example and Example 1 is that in the process of preparing the electrolyte, the content of succinonitrile and vinylene carbonate in the electrolyte is adjusted so that the mass ratio of succinonitrile to vinylene carbonate is 0.03:1. The rest of the raw material ratios and preparation methods are strictly consistent with Example 1.

[0070] Comparative Example 5

[0071] This comparative example refers to the preparation method provided in Example 1 to prepare a lithium ion battery. The difference between this comparative example and Example 1 is that in the process of preparing the electrolyte, the content of succinonitrile and vinylene carbonate in the electrolyte is adjusted so that the mass ratio of succinonitrile to vinylene carbonate is 0.4:1. The rest of the raw material ratios and preparation methods are strictly consistent with Example 1.

[0072] Test Case

[0073] Test objects: the lithium-ion batteries provided in Examples 1 to 11 and the lithium-ion batteries provided in Comparative Examples 1 to 5.

[0074] Test items and test methods:

[0075] (1) Discharge capacity retention rate at different temperatures: The battery of the test object is charged to 4.25V at 1 / 3C constant current and constant voltage at 25℃, and the cut-off current is 0.05C. After standing for 30 minutes, it is discharged to 2.5V at 1 / 3C. The released capacity is recorded as the initial capacity C0. Then it is charged at 1 / 3C0 constant current and constant voltage (cut-off current 0.05C0) to make SOC reach 100%. After the battery is left at different temperatures (represented by T, including -20℃, 0℃, 25℃, and 40℃) for 4 hours, it is discharged to 2.5V at 1 / 3C0 at the corresponding shelf temperature (-20℃, 0℃ discharge to 2.0V), and the discharge capacity C1 is recorded, and the discharge capacity retention rate is calculated. The specific calculation formula is: discharge capacity retention rate = (C1 / C0)*100%.

[0076] (2) Negative electrode manganese deposition: The test object was charged to 4.25V at 1 / 3C constant current and constant voltage at 25°C, with a cut-off current of 0.05C. After standing for 30 minutes, it was discharged to 2.0V at 1 / 3C, and then the negative electrode plate was disassembled and taken out, soaked in dimethyl carbonate and dried, weighed to calculate the weight of the negative electrode active material, and the negative electrode manganese content was measured by inductively coupled plasma atomic emission spectrometry, which was recorded as the initial negative electrode manganese deposition. Then the test object was charged and discharged at 1C at 25°C, with a voltage range of 2.5 to 4.25V, and the charge and discharge cycle was repeated 500 times. After 500 cycles, the battery cell was removed and discharged to 2.0V, and then the negative electrode plate was disassembled and taken out, soaked in dimethyl carbonate and dried, weighed to calculate the weight of the negative electrode active material, and the negative electrode manganese content was measured by inductively coupled plasma atomic emission spectrometry.

[0077] Test results: The composition of the electrolyte provided by the test subjects is shown in Table 2, and the test results are shown in Table 3.

[0078] Table 2. Composition of the electrolyte provided by each test subject

[0079]

[0080] Table 3. Performance test results of this test case

[0081]

[0082]

[0083] Result analysis:

[0084] By comparing the test results of Examples 1 to 11 with those of Comparative Examples 1 to 5 in Table 2, it can be found that the comprehensive performance of the batteries provided by Examples 1 to 11 is better than that of the batteries provided by Comparative Examples 1 to 5. Among them, in the batteries provided by Examples 1 to 11, the electrolyte provided by Example 1 can effectively reduce the negative electrode manganese deposition and has a high discharge capacity retention rate at low temperature. At -20°C, the capacity retention rate is 86.1%. The battery using the electrolyte has better low-temperature cycle characteristics.

[0085] By comparing the comprehensive performance of Example 1 with that of Comparative Example 1, it can be found that compared with the battery of Comparative Example 1, the battery provided by Example 1 has a higher discharge capacity retention rate in a low temperature environment, which shows that when the electrolyte system simultaneously uses vinyl sulfate (DTD), fluoroethylene carbonate (FEC) and 1,3-propane sultone (PS), it can promote the formation of a structurally stable SEI film on the surface of the negative electrode, reduce the interface impedance, reduce the adverse reactions between the electrolyte and the positive electrode and the negative electrode, maintain the stability of the battery interface, and help improve the electrochemical performance of the battery in a low temperature environment, and improve the energy output and cycle efficiency of the battery.

[0086] By comparing the comprehensive performance of Example 1 with that of Comparative Example 2, it can be found that compared with the battery of Comparative Example 2, the battery provided by Example 1 has a higher discharge capacity retention rate and a lower negative electrode manganese deposition amount under low temperature conditions, which indicates that when the content of ethylene carbonate in the electrolyte does not exceed 2wt%, the electrolyte can effectively reduce the manganese ions dissolved from the positive electrode.

[0087] Comparing the comprehensive performance of Example 1, Examples 3 to 8 with Comparative Example 3, it can be found that compared with the battery of Comparative Example 3, the batteries provided by Example 1 and Examples 3 to 8 have a lower amount of negative electrode manganese deposition, which shows that when the lithium salt additive uses at least one of lithium difluorophosphate, lithium difluorophosphate bisoxalate, and lithium dioxalate borate, the manganese ion concentration in the electrolyte system can be effectively reduced. Further, by comparing the low-temperature cycle performance of Example 1 and Examples 3 to 8, it can be found that compared with Examples 3 to 5 using only a single lithium salt additive, the batteries provided by Examples 1 and Examples 6 to 8 using composite lithium salt additives have better discharge capacity under low temperature conditions, among which the battery of Example 1 using three lithium salt additives has the best comprehensive performance. Match in any ratio. This shows that the use of composite lithium salt additives including lithium difluorophosphate, lithium difluorophosphate bisoxalate, and lithium dioxalate borate can play a synergistic effect in lithium-ion batteries.

[0088] By comparing the comprehensive performance of Examples 1 to 2 with Comparative Examples 4 to 5, it can be found that as the mass ratio of succinonitrile to vinylene carbonate increases, the negative electrode manganese deposition amount and volume expansion rate measured by the battery show a downward trend, and the low-temperature discharge capacity retention rate of the battery shows an upward trend. When the mass ratio of succinonitrile to vinylene carbonate is 0.05 to 0.3:1, the content of manganese ions in the electrolyte can be effectively reduced, thereby reducing the side reactions between manganese ions and the electrolyte, and improving the cycle performance of the battery.

[0089] Comparing the comprehensive performance of Example 1 with that of Examples 9-10 in Table 2, it can be found that compared with Examples 9-10 using a single lithium salt, Example 1 using a compound lithium salt has a higher capacity retention rate. And during the experiment, it was found that

[0090] Compared with the electrolyte of Example 9 using LiPF6 as the lithium salt, the electrolyte provided in Example 1 has moderate viscosity and high lithium ion mobility, which is reflected in a higher capacity retention rate. Compared with the electrolyte of Example 10 using only LiFSI as the lithium salt, the electrolyte provided in Example 1 has a lower cost, and the aluminum foil is not easily corroded by the electrolyte, which is reflected in a longer battery cycle life.

[0091] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A lithium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode active material containing a manganese element, the electrolyte comprises a lithium salt, a solvent and an additive, and the additive comprises a nitrile additive, an ester additive and a lithium salt additive; The nitrile additive includes succinonitrile, and the ester additive includes vinylene carbonate, the mass of succinonitrile: the mass of vinylene carbonate = 0.05-0.3:1, and the content of vinyl carbonate in the electrolyte does not exceed 2wt%; The ester additives also include vinyl sulfate, fluoroethylene carbonate and 1,3-propane sultone; The lithium salt additive includes at least one of lithium difluorophosphate, lithium bis(oxalato)difluorophosphate, and lithium bis(oxalato)borate.

2. The lithium-ion battery according to claim 1, characterized in that: The mass ratio of the nitrile additive, the ester additive and the lithium salt additive is 0.01-1.5:2.5-5:1.5-2.

5.

3. The lithium ion battery according to claim 2, characterized in that: In the ester additive, the mass ratio of the vinylene carbonate, the vinyl sulfate, the fluoroethylene carbonate and the 1,3-propane sultone is 1-3: 0.2-0.7: 0.1-0.5: 0.5-1.

5.

4. The lithium-ion battery according to claim 1, characterized in that: The lithium salt additives include lithium difluorophosphate, lithium bis(oxalate)difluorophosphate and lithium bis(oxalate)borate.

5. The lithium ion battery according to claim 4, characterized in that: In the lithium salt additive, the mass ratio of the lithium difluorophosphate, the lithium bis(oxalato)difluorophosphate and the lithium bis(oxalato)borate is 0.5-1.0:0.5-1.5:0.1-0.

5.

6. The lithium ion battery according to claim 1, wherein: Based on the total mass of the electrolyte, the content of the additive is 5-8wt%.

7. The lithium ion battery according to claim 1, characterized in that: The lithium salt includes at least one of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide; and the concentration of the lithium salt in the electrolyte is 0.5 to 1.5 mol / L.

8. The lithium ion battery according to claim 1, characterized in that: The solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate and ethyl methyl carbonate.

9. The lithium ion battery according to any one of claims 1 to 8, characterized in that: The positive electrode active material includes lithium manganese iron phosphate.

10. An electrical device comprising the lithium-ion battery according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Non-aqueous electrolyte for high-voltage lithium ion batteries

    CN103268956A

  • Electrolyte solution for high-capacity lithium-ion battery, preparation method and lithium-ion battery

    CN104900916A

  • Low temperature lithium ion battery

    CN107482253A

  • Lithium ion battery and preparation method

    CN109713298A

  • Lithium ion battery electrolyte suitable for NCM811 and SiO-C material system and preparation method

    CN110600804A