Lithium ion battery and method for preventing cycle failure of lithium ion battery

By comprehensively considering the expansion rate of the negative electrode piece, binder content, powder OI value and electrode piece peeling strength during the preparation process of lithium-ion battery cells, it is ensured that K*M*L≥0.36, which solves the problem that cannot be effectively solved in the existing technology. Analyzing issues affected by multiple failure causes improves the cycle stability and safety performance of lithium-ion batteries.

CN118867408AActive Publication Date: 2024-10-29安徽得壹能源科技有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411065181.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-29
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing technology cannot effectively analyze the impact weight and primary and secondary relationship of multiple failure causes in lithium-ion battery cycle failure, resulting in the inability to accurately assess battery failure and propose targeted measures.

Method used

In the preparation process of lithium-ion battery cells, the expansion rate of the negative electrode piece, binder content, powder OI value and electrode piece peeling strength are comprehensively considered to ensure that K*M*L ≥ 0.36, and optimization of appropriate process parameters is required to improve Battery stability.

Benefits of technology

It effectively avoids cell failure caused by pole piece processing, detects and solves problems in advance, and improves the safe performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867408A_ABST
    Figure CN118867408A_ABST
Patent Text Reader

Abstract

The invention provides a lithium ion battery and a method for preventing cycle failure of the lithium ion battery, and relates to the technical field of cycle failure of the lithium ion battery, and the method comprises the following steps: assembling a soft package battery cell, the lithium ion battery comprising a negative pole piece, a positive pole piece, an isolating membrane and an electrolyte; wherein the preparation process of the negative pole piece comprises the following steps: coating the surface of a negative current collector with negative slurry comprising a negative active material, a conductive agent and a binder, and drying to form a negative active material layer, thereby obtaining the negative pole piece; the soft package battery core needs to meet the condition that K * M * L is larger than or equal to 0.36, K is the expansion rate of the battery core, M is the strength of the graphite pole piece, and L is the compensation coefficient. According to the invention, the expansion rate of the negative pole piece, the content of the binder, the OI value of the powder, the peel strength of the pole piece and the temperature during coating are comprehensively considered, so that the lithium ion battery does not easily lose efficacy in the cycle process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of lithium ion battery cycle failure, and in particular to a lithium ion battery and a method for preventing lithium ion battery cycle failure. Background Art

[0002] The statements in this section merely provide background information related to the present disclosure and do not necessarily constitute prior art.

[0003] Lithium battery failures are mainly divided into two categories: one is performance failure and the other is safety failure. Performance failure (cycle failure) refers to the performance of lithium batteries failing to meet the use requirements, mainly including capacity attenuation, diving, poor performance, poor consistency, large K value, poor high and low temperature performance, etc.; safety failure refers to the failure of lithium batteries with certain safety risks due to improper use or abuse, mainly including thermal runaway, flatulence, leakage, lithium precipitation, short circuit, expansion deformation, etc.

[0004] Failure analysis is a technical and management activity to determine product failure modes, analyze failure causes, and predict or prevent failure phenomena. In other words, failure analysis is to find the root cause of failure from defective products, summarize all the strange phenomena that occur in the life of defective products, and then apply these experiences to new products.

[0005] Failure phenomena and failure causes are not simply one-to-one correspondences. The same failure phenomenon may be caused by different failure causes. Existing methods all use a single failure cause to describe and analyze whether a lithium battery has failed. There is a lack of quantitative analysis to analyze the influence weights and primary and secondary relationships of multiple failure causes at a certain stage. It is impossible to accurately evaluate failed batteries and propose reasonable measures in a targeted manner. Summary of the invention

[0006] In order to solve the above problems, the present disclosure proposes a lithium ion battery and a method for preventing the cycle failure of the lithium ion battery. In the preparation process of the battery cell, the expansion rate of the negative electrode plate, the binder content, the OI value of the powder, the peel strength of the plate and the temperature during coating are comprehensively considered to prevent the lithium ion battery from failing easily during the cycle.

[0007] According to some embodiments, the present disclosure adopts the following technical solutions:

[0008] A method for preventing cyclic failure of lithium-ion batteries comprises: in the process of preparing battery cells, comprehensively considering the expansion rate of negative electrode plates, binder content, powder OI value, battery cell expansion rate and graphite plate strength, so that they satisfy the following relationship: K*M*L≥0.36; wherein, K=∈*b*OI; ∈ is the plate expansion rate, b is the binder content, OI is the powder OI value, ∈ is the plate expansion rate, the smaller ∈ is, the more stable the plate is; the larger ∈ is, the more unstable the plate is; K is the battery cell expansion rate, M is the graphite plate strength, and L is the compensation coefficient.

[0009] Furthermore, M=n*t; n is the peeling strength of the negative electrode sheet, and t is the maximum temperature of a single side during negative electrode coating.

[0010] Furthermore, the value of ∈ is 3% to 8%, the value of b is 2.5% to 3.5%, and the value of OI is 2 to 10.

[0011] Furthermore, the value of n is ≥8N / m, the value of t is ≥60°C, and the value of L is 0.5-2.

[0012] According to some embodiments, the present disclosure adopts the following technical solutions:

[0013] A lithium ion battery comprises: a battery cell that satisfies: K*M*L≥0.36; wherein, K=∈*b*OI; ∈ is the expansion rate of the pole piece, b is the binder content, OI is the OI value of the powder, ∈ is the expansion rate of the pole piece, the smaller ∈ is, the more stable the pole piece is; the larger ∈ is, the more unstable the pole piece is; K is the battery cell expansion rate, M is the strength of the graphite pole piece, and L is the compensation coefficient.

[0014] Furthermore, the lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet, a separator and an electrolyte;

[0015] The negative electrode sheet preparation process is as follows: a negative electrode slurry including a negative electrode active material, a conductive agent and a binder is coated on the surface of a negative electrode current collector, and a negative electrode active material layer is formed after drying to obtain a negative electrode sheet.

[0016] Furthermore, the negative electrode active material includes at least one of artificial graphite, natural graphite, silicon-carbon material, hard carbon and soft carbon.

[0017] Furthermore, the particle size D50 of the negative electrode active material powder is 10 to 20 μm, the specific surface area of ​​the negative electrode active material powder is 1 to 3 m2 / g, and the compaction density of the negative electrode plate is 1.5 g / cm3 to 1.7 g / cm3.

[0018] Furthermore, the preparation of the lithium-ion battery includes the following steps: preparing a slurry by mixing graphite, a conductive agent, a binder and water through a slurry mixing process, applying the slurry to a current collector, and baking the slurry to prepare a negative electrode sheet; preparing a slurry by mixing lithium iron phosphate, a conductive agent, a binder and NMP through a slurry mixing process, applying the slurry to a current collector, and baking the slurry to prepare a positive electrode sheet.

[0019] Furthermore, the battery cell is finally manufactured through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, liquid injection, chemical formation and capacity division processes.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] A lithium ion battery and a method for preventing cyclic failure of a lithium ion battery disclosed herein, in the process of preparing a battery cell, the expansion rate of a negative electrode plate, the binder content, the OI value of a powder, the peel strength of the plate and the temperature during coating are comprehensively considered, and a quantitative analysis method is adopted. When K*M*L≥0.36 is satisfied, the lithium ion battery will not fail easily during the cycle process.

[0022] The present invention discloses a lithium-ion battery and a method for preventing cycle failure of a lithium-ion battery. The method can avoid cell failure caused by electrode processing, thereby discovering problems in the trial production process, discovering problems in advance and solving problems, thereby improving the safe use performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings constituting a part of the present disclosure are used to provide a further understanding of the present disclosure. The illustrative embodiments of the present disclosure and their descriptions are used to explain the present disclosure and do not constitute an improper limitation on the present disclosure.

[0024] Figure 1 A schematic diagram of a trial-produced battery cell according to an embodiment of the present disclosure;

[0025] Figure 2 This is a photo of the fully charged battery cell disassembled after 500 cycles of the embodiment of the present disclosure;

[0026] Figure 3 This is a photo of the fully charged battery cell disassembled after 500 cycles of Comparative Example 4 in the disclosed embodiment;

[0027] Figure 4 This is a photo of the fully charged battery cell disassembled after 500 cycles in Comparative Example 6 of the disclosed embodiment.

[0028] Figure 5 The battery curves of all groups of the embodiments of the present disclosure after 500 cycles. DETAILED DESCRIPTION

[0029] The present disclosure is further described below in conjunction with the accompanying drawings and embodiments.

[0030] It should be noted that the following detailed descriptions are all illustrative and are intended to provide further explanation of the present disclosure. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present disclosure belongs.

[0031] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present disclosure. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0032] Example 1

[0033] In one embodiment of the present disclosure, a method for preventing cyclic failure of lithium-ion batteries is provided. During the preparation of the battery cell, the expansion rate of the negative electrode plate, the binder content, the OI value of the powder, the stripping strength of the plate and the temperature during coating are comprehensively considered so that the battery cell satisfies: K*M*L≥0.36, wherein K is the battery cell expansion rate, M is the graphite plate strength, and L is the compensation coefficient.

[0034] Among them, K = ∈ * b * OI; ∈ is the expansion rate of the electrode, b is the binder content, and OI is the OI value of the powder. The three factors that affect the K value must meet: ∈ is 3% to 8%, b is 2.5% to 3.5%, and OI is 2 to 10; L must meet the value of 0.5 to 2.

[0035] After the battery cell fails, through the analysis of the reasons for the battery cell failure, the above parameters in the trial production process will affect the battery cell quality and thus lead to battery cell failure.

[0036] As an embodiment, ∈ is the electrode expansion rate. The smaller ∈ is, the more stable the electrode is, which is conducive to the insertion and extraction of lithium ions and can prevent the battery from being too thick. The larger ∈ is, the more unstable the electrode is, which is not conducive to the battery cell cycle and will cause the battery to fail.

[0037] As an embodiment, M=n*t; n is the peel strength of the negative electrode sheet, t is the highest temperature of a single side during negative electrode coating. The value of n is ≥8N / m, the value of t is ≥60°C, and the value of L is 0.5-2.

[0038] Wherein, b is the binder content. Too much binder will reduce the proportion of active materials and make the pole piece brittle. Too little binder will lead to low peeling strength of the pole piece, or even die cutting loss, increase side reactions, and increase the short circuit rate of the battery.

[0039] OI is the OI value of the powder, VOI = C004 / C110, where C004 is the peak area of ​​the 004 characteristic diffraction peak in the X-ray diffraction spectrum of the negative electrode active material powder, and C110 is the peak area of ​​the 110 characteristic diffraction peak in the X-ray diffraction spectrum of the negative electrode active material powder. The larger the OI value, the worse the kinetic performance, which will reduce the charging rate of the material and the battery, and it is easy to precipitate lithium under high rate conditions, affecting safety performance. The smaller the OI value, the better the isotropy of the material and the better the kinetic performance, but there are shortcomings such as poor adhesion and high temperature performance deviation.

[0040] n is the peel strength of the negative electrode sheet. The greater the peel strength of the electrode sheet, the better the bonding between the binder and the material, the better the bonding between the slurry and the current collector, and the greater the peel strength, which is beneficial to battery cycling.

[0041] t is the maximum temperature of a single side during negative electrode coating. When the coating temperature is low, it may cause a wet film on the electrode, roller sticking, or even stratification of the coating (upper layer dried, lower layer wet), leading to failure of cyclic powder removal; when the coating temperature is too high, it may cause cracking of the coated electrode.

[0042] As an example, the pole piece expansion rate, binder content, powder OI value, pole piece peel strength, and coating temperature may have a significant impact on the performance of the battery, leading to battery failure.

[0043] In the design disclosed herein, the negative electrode sheet expansion rate, binder content, powder OI value, sheet peel strength, and coating temperature are comprehensively considered. When K*M*L≥0.36 is satisfied, the lithium-ion battery will not fail easily during the cycle process.

[0044] In some embodiments, the particle size D50 of the negative electrode active material powder is 10-20 μm, the specific surface area is 1-3 m2 / g, and the compaction density of the negative electrode plate is 1.5 g / cm3 to 1.7 g / cm3. . For the particle size D50, if it is too small, the compaction density will be reduced. If the particle size is too large, the compaction density will increase, and the impedance of the material will be too large, affecting the rate performance. For the specific surface area, if it is too small, there are fewer active points, which reduces the diffusion coefficient of lithium ions. If it is too large, the compaction density is reduced, which is beneficial to the rate and cycle performance, but it will reduce the high temperature performance. For the compaction density, if it is too low, the pole piece is too thick, which affects the diffusion coefficient of the material and reduces the energy density. If the compaction density is too high, a "crushed to death" phenomenon may occur, resulting in lithium precipitation.

[0045] Example 2

[0046] In one embodiment of the present disclosure, a lithium-ion battery is provided, wherein the lithium-ion battery is assembled into a soft-pack battery cell, and the lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet, a separator, and an electrolyte;

[0047] The negative electrode sheet preparation process is as follows: a negative electrode slurry including a negative electrode active material, a conductive agent and a binder is coated on the surface of a negative electrode current collector, and a negative electrode active material layer is formed after drying to obtain a negative electrode sheet.

[0048] As an embodiment, the particle size D50 of the negative electrode active material powder is 10-20 μm, the specific surface area of ​​the negative electrode active material powder is 1-3 m2 / g, and the compaction density of the negative electrode plate is 1.5 g / cm3-1.7 g / cm3.

[0049] As an embodiment, the negative electrode active material includes at least one of artificial graphite, natural graphite, silicon-carbon material, hard carbon and soft carbon.

[0050] As an embodiment, a method for preparing a lithium-ion battery is provided, comprising the following steps: preparing a slurry of graphite, a conductive agent, a binder and water through a slurry mixing process, applying the slurry to a current collector, and baking the slurry to form a negative electrode sheet; preparing a slurry of lithium iron phosphate, a conductive agent, a binder and NMP through a slurry mixing process, applying the slurry to a current collector, and baking the slurry to form a positive electrode sheet.

[0051] Finally, the battery cell is made through rolling, slitting, die-cutting, lamination, hot pressing, welding, packaging, liquid injection, formation and capacity division processes.

[0052] Specifically, Figure 1 As shown, the specification of the soft-package lithium-ion battery in this embodiment is 3Ah;

[0053] As an embodiment, a preparation of a lithium ion battery includes the following steps:

[0054] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0055] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 5% was selected, the powder OI value was 5, the binder content was 3%, the peeling force was 18N / m, and the single-side baking temperature was 60°C during coating. During the trial production process, other influencing factors were about 1.5;

[0056] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0057] As an embodiment, the specification of the soft-package lithium-ion battery in this embodiment is 3Ah; compared with the above embodiment, the difference is that the parameters are changed;

[0058] A lithium ion battery comprises the following steps:

[0059] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0060] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 8% was selected, the powder OI value was 2, the binder content was 2.5%, the peeling force was 8N / m, and the single-side baking temperature was 60°C during coating. During the trial production process, other influencing factors were about 1.5;

[0061] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0062] As an embodiment, the specification of the soft-package lithium-ion battery in this embodiment is 3Ah; compared with the above embodiment, the difference is that the parameters are changed;

[0063] A lithium ion battery comprises the following steps:

[0064] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0065] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 3% was selected, the powder OI value was 10, the binder content was 3.5%, the peeling force was 25N / m, and the single-side baking temperature was 60°C during coating. During the trial production process, other influencing factors were about 1.5;

[0066] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0067] Simulation comparison

[0068] Comparative Example 1: The specification of the soft-package lithium-ion battery in this comparative example 1 is 3Ah; compared with the embodiment, the difference is that the steps and parameters are changed;

[0069] A lithium ion battery comprises the following steps:

[0070] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0071] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 5% was selected, the powder OI value was 5, the binder content was 3%, the peeling force was 6N / m, and the single-side baking temperature was 60°C during coating. During the trial production process, other influencing factors were about 1.5;

[0072] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0073] Comparative Example 2: The specification of the soft-package lithium-ion battery in this comparative example 2 is 3Ah; compared with the embodiment, the difference is that the parameters are changed;

[0074] A lithium ion battery comprises the following steps:

[0075] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0076] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 10% was selected, the powder OI value was 5, the binder content was 3%, the peeling force was 18N / m, and the single-side baking temperature was 60°C during coating. During the trial production process, other influencing factors were about 1.5;

[0077] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0078] Comparative Example 3: The specification of the soft-package lithium-ion battery in this comparative example 3 is 3Ah; compared with the embodiment, the difference is that the parameters are changed;

[0079] A lithium ion battery comprises the following steps:

[0080] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0081] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 2% was selected, the powder OI value was 5, the binder content was 3%, the peeling force was 18N / m, and the single-side baking temperature was 60°C during coating. During the trial production process, other influencing factors were about 1.5;

[0082] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0083] Comparative Example 4: The specification of the soft-package lithium-ion battery in this comparative example 4 is 3Ah; compared with the embodiment, the difference is that the parameters are changed;

[0084] A lithium ion battery comprises the following steps:

[0085] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0086] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 5% was selected, the powder OI value was 5, the binder content was 2.3%, the peeling force was 18N / m, and the single-side baking temperature was 60°C during coating. During the trial production process, other influencing factors were about 1.5;

[0087] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0088] Comparative Example 5: The specification of the soft-package lithium-ion battery in this comparative example 5 is 3Ah; compared with the embodiment, the difference is that the parameters are changed;

[0089] A lithium ion battery comprises the following steps:

[0090] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0091] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 5% was selected, the powder OI value was 5, the binder content was 4%, the peeling force was 18N / m, and the single-side baking temperature was 60°C during coating. During the trial production process, other influencing factors were about 1.5;

[0092] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0093] Comparative Example 6: The specification of the soft-package lithium-ion battery in this comparative example 6 is 3Ah; compared with the embodiment, the difference is that the parameters are changed;

[0094] A lithium ion battery comprises the following steps:

[0095] 1. Graphite, conductive agent, binder, water, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a negative electrode sheet; lithium iron phosphate, conductive agent, binder, NMP, etc. are made into slurry through a slurry mixing process, applied to the current collector, and baked to form a positive electrode sheet; then through rolling, slitting, die cutting, lamination, hot pressing, welding, packaging, injection, formation, capacity division and other processes, a battery cell is made;

[0096] 2. After the negative electrode was left to stand for 24 hours, a pole piece with a rebound rate of about 5% was selected, the powder OI value was 5, the binder content was 3%, the peeling force was 18N / m, and the single-side baking temperature was 55°C during coating. During the trial production process, other influencing factors were about 1.5;

[0097] 3. The obtained battery was subjected to a cycle test in a 25°C environment, and the cycle voltage was 2.5V-3.65V.

[0098] According to the batteries produced in the above examples and comparative examples, 3 batteries were randomly selected from each group for cycling, and the charge and discharge cycles were performed at 1C / 1C, with a voltage range of (2.5V-3.65). After 500 cycles, the battery with the best cycle was selected from all groups to observe the battery cycle curves, such as Figure 5 shown.

[0099] from Figure 5It can be seen that the battery cell meets: K*M*L≥0.36. The three factors affecting the K value must meet: ∈ is 3% to 8%, b is 2.5% to 3.5%, and OI is 2 to 10, the resulting battery has obvious advantages.

[0100] Although the above describes the specific implementation methods of the present disclosure in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the present disclosure. Technical personnel in the relevant field should understand that on the basis of the technical solution of the present disclosure, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present disclosure.

Claims

1. A method for preventing lithium-ion battery cycle failure, characterized in that: include: In the preparation process of battery cells, the expansion rate of the negative electrode plate, the binder content, the powder OI value, the cell expansion rate and the graphite plate strength are comprehensively considered so that they satisfy the following relationship: K*M*L≥0.36; wherein, K=∈*b*OI; ∈ is the plate expansion rate, b is the binder content, OI is the powder OI value, ∈ is the plate expansion rate, the smaller ∈ is, the more stable the plate is; the larger ∈ is, the more unstable the plate is; K is the cell expansion rate, M is the graphite plate strength, and L is the compensation coefficient.

2. A method for preventing lithium-ion battery cycle failure as claimed in claim 1, characterized in that: M = n*t; n is the peeling strength of the negative electrode sheet, and t is the maximum temperature of a single side during negative electrode coating.

3. A method for preventing lithium-ion battery cycle failure as claimed in claim 1, characterized in that: The value of ∈ is 3%~8%, the value of b is 2.5%~3.5%, and the value of OI is 2~10.

4. A method for preventing lithium-ion battery cycle failure as claimed in claim 1, characterized in that: The value of n is ≥8N / m, the value of t is ≥60℃, and the value of L is 0.5~2.

5. A lithium ion battery, characterized in that: The battery cell satisfies: K*M*L≥0.36; wherein, K=∈*b*OI; ∈ is the electrode expansion rate, b is the binder content, OI is the powder OI value, ∈ is the electrode expansion rate, the smaller ∈ is, the more stable the electrode is; the larger ∈ is, the more unstable the electrode is; K is the battery cell expansion rate, M is the graphite electrode strength, and L is the compensation coefficient.

6. A lithium ion battery as claimed in claim 5, characterized in that: The lithium-ion battery comprises a negative electrode sheet, a positive electrode sheet, a separator and an electrolyte; The negative electrode sheet preparation process is as follows: a negative electrode slurry including a negative electrode active material, a conductive agent and a binder is coated on the surface of a negative electrode current collector, and a negative electrode active material layer is formed after drying to obtain a negative electrode sheet.

7. A lithium ion battery as claimed in claim 6, characterized in that: The negative electrode active material includes at least one of artificial graphite, natural graphite, silicon-carbon material, hard carbon and soft carbon.

8. A lithium ion battery as claimed in claim 6, characterized in that: The particle size D50 of the negative electrode active material powder is 10 to 20 μm, the specific surface area of ​​the negative electrode active material powder is 1 to 3 m2 / g, and the compaction density of the negative electrode plate is 1.5 g / cm3 to 1.7 g / cm3.

9. A lithium ion battery as claimed in claim 5, characterized in that: The lithium ion battery preparation comprises the following steps: Graphite, a conductive agent, a binder and water are made into a slurry through a slurry mixing process, applied to a current collector, and baked to form a negative electrode sheet; lithium iron phosphate, a conductive agent, a binder and NMP are made into a slurry through a slurry mixing process, applied to a current collector, and baked to form a positive electrode sheet.

10. A lithium ion battery as claimed in claim 9, characterized in that: Finally, the battery cell is made through rolling, slitting, die-cutting, lamination, hot pressing, welding, packaging, liquid injection, formation and capacity division processes.

Citation Information

Patent Citations

  • Negative electrode material, negative electrode slurry, negative electrode plate and lithium ion battery

    CN111725509A

  • Negative electrode material and negative electrode plate containing negative electrode material

    CN114050264A

  • Long-circulation negative electrode slurry, negative electrode plate, preparation method of negative electrode plate and cylindrical battery

    CN116387456A

  • Negative plate and battery

    CN117352650A

  • Battery Cell, Battery and Electric Device

    US20240178461A1