Injection hydrogel as well as preparation method and application thereof
Through a double crosslinked hydrogel composed of carboxymethyl chitosan, oxidized dextran and tea polyphenol, the problem of low maintenance of submucosal injection materials and tumor induction is solved, and high viscosity, injectability and anti-aging are achieved Tumor effect reduces surgical complications and tumor risk.
Patent Information
- Application Number
- CN202410979856.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-01
AI Technical Summary
Existing submucosal injection materials maintain insufficient submucosal pad height during surgery, resulting in prolonged surgical time and increased risk of anesthesia, and may damage surrounding tissues or induce tumor growth. Moreover, high-viscosity materials have large injection resistance and strong unevenness, which cannot be effective. Prevent perforation complications.
A double crosslinked hydrogel composed of carboxymethyl chitosan, oxidized dextran and tea polyphenols is used as the submucosal pad material, and hydrogen bonds are formed by reacting carboxymethyl chitosan with the Schiff base of oxidized dextran The Internet, tea polyphenols provide antioxidant and antibacterial effects, forming a hydrogel with high viscosity and good injectability.
This hydrogel can provide long-lasting submucosal pad height during ESD and TEM surgery, reduce the risk of electric and thermal damage, significantly improve biocompatibility and antibacterial ability, reduce tumor cell proliferation and migration, enhance hemostasis performance, and reduce surgical complications , such as perforation and wound infection.
Smart Images

Figure CN118873759A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of submucosal injection materials, and in particular to an injectable hydrogel, a preparation method and application thereof. Background Art
[0002] The use of submucosal injection materials SIM to form a submucosal barrier is an effective method to reduce the complications of ESD and TEM for rectal benign tumors and precancerous lesions. SIM can elevate the lesion through a thick liquid pad, separate the lesion from the muscle layer, thereby reducing the risk of thermal injury and perforation bleeding, and is more conducive to the overall resection of the lesion. In recent years, normal saline is the most commonly used SIM submucosal pad material, but because normal saline is a small molecule substance with low viscosity and fast diffusion, the barrier function will weaken rapidly and can only be maintained for a short time of about 3 minutes, so multiple injections are always required. This will cause some other potential risks of surgery, such as prolonged operation time, corresponding increase in the dose of anesthetic drugs, and increased risk of anesthesia. Substitutes for submucosal liquid pads with high osmotic pressure or high viscosity, such as hyaluronic acid, hypertonic glucose, and hydrogel, have also been used. However, the effect of high-concentration glucose solution in maintaining the height of the submucosal pad is not ideal. The height of the submucosal pad will quickly drop to less than 50% within 30 minutes, and its hyperosmoticity will cause severe damage to the surrounding tissues. Hyaluronic acid has become popular as a submucosal liquid pad material due to its long duration, relatively high overall resection success rate, and low incidence of perforation complications. However, hyaluronic acid is expensive and may induce tumor growth factors to promote the proliferation of tumor cells around the wound, and the comprehensiveness of tumor removal has been questioned. Sodium alginate is no longer recommended because of its high viscosity, high injection resistance, uneven thickness of the submucosal liquid pad, and unexplained mucosal contraction.
[0003] Therefore, there is an urgent need to develop a submucosal injection material that has excellent biocompatibility, hemostatic effect, antibacterial ability, adhesion, and injectability, and can maintain a lasting submucosal pad height for surgery without damaging surrounding tissues and having a certain anti-tumor effect. Summary of the invention
[0004] In order to solve the above technical problems, the present invention discloses an injectable hydrogel, a preparation method and an application thereof. The injectable hydrogel has great potential and can become a biomaterial to assist ESD and TEM surgeries, further reducing the complications of ESD and TEM surgeries.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] The first aspect of the present invention provides an injectable hydrogel comprising carboxymethyl chitosan, oxidized dextran and tea polyphenols.
[0007] Optionally, the mass ratio of carboxymethyl chitosan:oxidized dextran:tea polyphenols is 2.15-25:1-4:0.5-2.
[0008] The second aspect of the present invention provides a method for preparing an injectable hydrogel, comprising the following steps:
[0009] S1, synthetic oxidized dextran
[0010] Dissolve dextran and sodium periodate in double distilled water and stir in the dark; add ethylene glycol and stir in the dark to terminate the oxidation reaction; dialyze and then freeze-dry the purified original solution to obtain white sponge-like oxidized dextran;
[0011] S2. Preparation of injectable hydrogel
[0012] The tea polyphenols are dissolved in a carboxymethyl chitosan solution to prepare a mixture of the tea polyphenols and the carboxymethyl chitosan; the white spongy oxidized dextran is dissolved to prepare an oxidized dextran solution; the mixture of the tea polyphenols and the carboxymethyl chitosan is mixed with the oxidized dextran solution to obtain an injectable hydrogel.
[0013] In step S1, dextran and sodium periodate are dissolved in double distilled water, stirred in the dark, and ethylene glycol is added. The reason for stirring in the dark is that sodium periodate can oxidize the vicinal diol group in ethylene glycol to ketone. The reaction mechanism is to generate a double bond at the meta position by capturing the α-hydrogen of the vicinal diol and simultaneously obtain an oxygen atom. At this time, the intermediate product is very sensitive to light and is prone to a series of side reactions under the action of light, affecting the normal progress of the reaction. Therefore, in order to avoid the interference of light with the reaction, sodium periodate should be used in a dark environment when oxidizing the vicinal diol.
[0014] Optionally, in step S1, the molar ratio of oxidized dextran to sodium periodate is 3:1 to 1:3.
[0015] Optionally, in step S1, the molar numbers of ethylene glycol and sodium periodate are the same.
[0016] Optionally, in step S1, the dialysis time is 72 to 96 hours, the dialysis fluid is double distilled water, and during the dialysis process, the dialysis fluid is replaced every four hours.
[0017] Optionally, in step S2, the concentration of the carboxymethyl chitosan solution is 2% to 3%.
[0018] Optionally, in step S2, the volume ratio of the mixture of tea polyphenols and carboxymethyl chitosan to the oxidized dextran solution is 2:1 to 1:2, and the concentration of the oxidized dextran solution is 20% to 30%.
[0019] The third aspect of the present invention provides a use of an injectable hydrogel.
[0020] In an alternative embodiment, the injectable hydrogel is used to prepare submucosal injection materials for colorectal mucosal dissection.
[0021] The beneficial effect of the present invention is that the present invention uses carboxymethyl chitosan, oxidized dextran and tea polyphenols to develop a double cross-linked hydrogel as a submucosal pad injection material. Compared with traditional submucosal pad injections such as physiological saline and hypertonic glucose, the SIM can provide a lasting submucosal pad height for surgery, elevate the diseased tissue, and avoid electrical and thermal damage. The SIM has excellent biocompatibility through cell experiments and hemolysis experiments. In in vivo experiments, the SIM can quickly control liver bleeding in rats and has excellent antibacterial ability. In the process of co-culturing with colon cancer cells, the effect of the SIM on inhibiting tumor proliferation and migration was also tested, and an additional physical barrier can be added for the wound metastasis of cancer cells in patients with early rectal cancer and precancerous lesions. Thanks to the excellent antioxidant capacity of tea polyphenols, oxygen free radicals in the wound site can be removed, excessive aggregation of inflammatory cells can be reduced, and rapid healing of the wound can be assisted. The double cross-linked antibacterial and anti-tumor hydrogel submucosal pad injection material has great potential and can become a biomaterial to assist ESD and TEM surgery, further reducing the complications of ESD and TEM surgery. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A is the synthesis mechanism of ODex and the gelation mechanism of OCT hydrogel;
[0023] Figure 1 B is the H NMR spectrum of Dex and ODex;
[0024] Figure 1 C is the gelation process of OCT hydrogel;
[0025] Figure 1 D is the gelation time of OCT hydrogel;
[0026] Figure 1 E is the microstructure of OCT hydrogel;
[0027] Figure 1 F is the actual picture of the swelling of OCT hydrogel;
[0028] Figure 1 G is the surface area swelling ratio of OCT hydrogel;
[0029] Figure 1 H is the rheological property of OCT hydrogel;
[0030] Figure 2 A shows the injectability of OCT hydrogel and simulated injection under the pig intestinal mucosa;
[0031] Figure 2B is the height duration of OCT hydrogel under the mucosa;
[0032] Figure 2 C is a schematic diagram of the burst pressure experiment;
[0033] Figure 2 D is the maximum burst pressure of OCT hydrogel;
[0034] Figure 2 E is a schematic diagram of the OCT hydrogel shear adhesion experiment;
[0035] Figure 2 F is the maximum shear adhesion force of OCT hydrogel;
[0036] Figure 2 G is a photo of pig skin with various twists and folds, but OCT hydrogel can still adhere tightly to the pig skin;
[0037] Figure 2 H is a macroscopic self-healing photo of OCT3 hydrogel;
[0038] Figure 2 I is the OCT hydrogel rheological self-healing performance test;
[0039] Figure 3 A is the cumulative release rate of TP in OCT hydrogels of each group;
[0040] Figure 3 B is the survival rate of cancer cells in each group co-cultured with OCT hydrogel and human ileocecal cancer cells HCT-8 for 1-3 days;
[0041] Figure 3 C is the live / dead fluorescence staining image of human ileocecal cancer cells HCT-8 after co-culture with each group of OCT hydrogel for 24 hours;
[0042] Figure 3 D is for Figure 3 The survival rate of human ileocecal cancer cell HCT-8 in C was quantitatively analyzed;
[0043] Figure 3 E is a representative image of HCT-8 migration in the scratch healing assay at different times, scale bar = 100 μm;
[0044] Figure 3 F is for Figure 3 Quantitative statistics of the migration and healing range of human ileocecal cancer cell HCT-8 in E;
[0045] Figure 3 G is the amount of reactive oxygen species produced after co-culture of human ileocecal cancer cells HCT-8 with each group of OCT hydrogels;
[0046] Figure 4A is the hemolysis rate of each OCT hydrogel group;
[0047] Figure 4 B shows the cell growth of each group of OCT hydrogels co-cultured with mouse fibroblasts L929 for 1 to 5 days;
[0048] Figure 4 C is a HE-stained smear of the heart, liver, spleen, lung, and kidney organs 14 days after the OCT hydrogel was buried subcutaneously in mice;
[0049] Figure 4 D is the colony picture and quantitative data of Staphylococcus aureus and Escherichia coli surviving on the culture dish after co-culture with OCT hydrogel;
[0050] Figure 5 To observe the optimal images of the hemostatic effect of OCT hydrogel on the mouse liver bleeding model, the blood loss and hemostasis time were quantified. DETAILED DESCRIPTION
[0051] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0052] Example 1
[0053] A method for preparing an injectable hydrogel comprises the following steps:
[0054] S1. Synthesis of ODex
[0055] Dex and NaIO4 were dissolved in double distilled water at a molar ratio of 1:1 (theoretical oxidation degree was 100%) and stirred in the dark for 24 hours; then, ethylene glycol in the same mole as NaIO4 was added and stirred in the dark for 2 hours to terminate the oxidation reaction; then, the reaction mixture was dialyzed with double distilled water for 3 days, during which the dialyzate was replaced every four hours; finally, the purified original solution was freeze-dried to obtain a white sponge-like ODex;
[0056] S2. Preparation of ODex / CMCS / TP (OCT) hydrogel
[0057] Tea polyphenols were dissolved in 2.5% CMCS solution at a ratio of 1:10000, 1:1000 and 1:100 (mass / volume) to prepare mixtures of tea polyphenols and carboxymethyl chitosan with concentrations of 0.01%, 0.1% and 1%, respectively, which were recorded as CT1 / CT2 / CT3; and the 2.5% CMCS solution without tea polyphenols was named CT0. Equal volumes of CT0 / CT1 / CT2 / CT3 were mixed with 20% ODex solution to prepare OCT0 / OCT1 / OCT2 / OCT3 hydrogels, respectively.
[0058] All the above solvents are PBS.
[0059] Example 2 Characterization of OCT hydrogel
[0060] 2.1OCT gelation time test
[0061] The gel time was determined by the vial tilting method. The OCT precursor solution was mixed and added to the vial, and the vial was tilted to observe the fluidity of the liquid. The gel time was the time when the liquid in the vial stopped flowing.
[0062] 2.2 Microstructure of OCT hydrogel
[0063] In order to observe the morphology of the samples, each group of OCT hydrogels was freeze-dried for 3 days using a freeze dryer. The dried samples were cut along the cross section and bonded to the sample stage with conductive glue. They were then sprayed with gold to increase conductivity and imaged using a scanning electron microscope at an accelerating voltage of 10 kV.
[0064] 2.3 Swelling rate test of OCT hydrogel
[0065] First, the hydrogel samples were prepared using the same cylindrical mold, and then the surface area of the samples was measured and marked as S0, and then the samples were immersed in PBS (pH 7.4, 37°C). At specific time intervals, the hydrogels were taken out of the solution and their surface areas were measured and recorded as St. The surface area swelling rate of the hydrogel was calculated as follows:
[0066]
[0067] 2.4 Rheological testing of OCT hydrogel
[0068] 500 μL of OCT0 / OCT1 / OCT2 / OCT3 hydrogel was injected into the center of the 40 mm parallel plate using a vortex mixer. After the hydrogel performance stabilized, the excess hydrogel was removed and the sample was sealed with dimethyl silicone oil to prevent water evaporation; then, the test data was set to amplitude γ = 1% and angular frequency ω = 0.1-100 rad s-1 Conduct rheological studies.
[0069] ODex was synthesized by oxidation reaction of Dex with NaIO4, and reacted with CMCS via Schiff base to form hydrogel-based SIM. Meanwhile, the amino groups of CMCS formed hydrogen bonds with the hydroxyl groups of TP, thus successfully synthesizing a double cross-linked network of OCT hydrogel ( Figure 1 A) NaIO4 catalyzes the oxidation of vicinal diols in Dex to obtain Dex derivatives with two -CHO. 1 H NMR test found that ODex and Dex showed a hemiacetal peak at 4.8-6.0 ppm, confirming that the hydroxyl group of Dex was successfully aldehyded ( Figure 1 B) Figure 1 As shown in C, the TP solution and the CMCS solution are first mixed, and before they are gelled through hydrogen bonding, an equal volume of ODex is added to the total of the first two, and OCT hydrogel is quickly formed at room temperature. Physiological saline has been used for submucosal injection to assist in raising mucosal lesions, but because of the rapid diffusion of its small molecules, the height of the submucosal pad will decrease rapidly, increasing the difficulty of surgery and the risk of perforation and bleeding. Therefore, SIM has strict requirements on the submucosal pad height and diffusion. ODex and CMCS can quickly undergo Schiff base reaction to form a hydrogel. On the basis of this study, the hydrogen bond network is introduced to further accelerate the gelation speed and enhance the performance of the hydrogel. By testing the gelation time, it was found that with the increase of TP content, the gelation time was significantly accelerated. The gelation time of OCT3 was shortened by about 50% (0.05%) compared with the OCT0 group without TP. Figure 1 D). The shortening of gelation time is helpful to avoid the diffusion of solution and uneven gelation when injected into the submucosal layer, which affects the height of lesion lifting. Although the gelation time of the OCT hydrogel SIM is slightly prolonged due to the addition of TP during submucosal injection, its gelation time can still meet the requirements of SIM. As a submucosal pad, it can fully lift the lesion mucosa, facilitate the peeling of the lesion mucosa during ESD and TEM surgery, avoid surgical level errors, and facilitate the operation.
[0070] The microstructural differences of each group of OCT hydrogel were observed by scanning electron microscopy at magnifications of 100 times and 300 times, respectively. Figure 1 All groups shown in E exhibited a stable, uniform and interconnected three-dimensional pore structure. With the increase of TP content, the cross-linked network of OCT hydrogel became denser and its three-dimensional structure became more stable. At the same time, because the cross-linking density of the hydrogel in the OCT3 group was dense, its contact area swelling rate was the lowest in the contact area swelling rate results, avoiding excessive swelling that caused the inability to adhere firmly to the original position, and it could play a long-term physical barrier role, preventing bacteria from entering the blood from the surgical wound, thereby further reducing the risk of postoperative perforation of the surgical wound ( Figure 1 F / G). The same dynamic rheological properties are also shown in the oscillatory rheological test. The frequency sweep measurement results of the hydrogel are expressed as storage modulus (G') and loss modulus (G") ( Figure 1 H). For all OCT hydrogel groups, G' was always higher than G", which proved that the hydrogel had been cross-linked and gelled and showed solid properties. OCT3 group had a denser three-dimensional structure, and its G' and G" were slightly higher than those of the other three groups. The structure was more stable and the viscosity was higher, which could meet the long-term stability required for the submucosal pad. The above characterization tests fully confirmed that OCT hydrogel SIM could meet the requirements of ESD and TEM surgery and assist in surgical operations.
[0071] Example 3 Injectability, Adhesion and Self-Healing of OCT Hydrogel
[0072] 3.1 Test of injectability of OCT hydrogel
[0073] To test the injectability of OCT hydrogel, two precursor solutions of OCT hydrogel were respectively loaded into a double-barreled mixing syringe and the word PCT was written on it for demonstration.
[0074] During ESD and TEM surgeries, SIM is required to be injectable and to gel in a short time to avoid submucosal diffusion and to easily elevate the lesion site for easier surgical operation. Figure 2 A It can be observed that the font "PCT" is written with a syringe, and the font is round and non-dispersed, which proves that the precursor solution of OCT hydrogel quickly gels when leaving the needle of the double-barreled syringe; it can be inferred that its precursor solution will not spread under the mucosa, and the lesion can be accurately lifted. This embodiment uses porcine large intestine to simulate ESD and TEM surgery. After injecting OCT hydrogel under the intestinal mucosa, the intestinal mucosa is separated from the intestinal muscle layer and is obviously lifted, which is very conducive to the operation.
[0075] 3.2 OCT hydrogel in vitro submucosal injection liquid pad height test
[0076] NS2mL and OCT0 / OCT1 / OCT2 / OCT3 were injected into the submucosal mucosa of pig colorectal tissue in vitro to evaluate the maintenance durability and operability of the submucosal pad height. At the specified intervals, the height changes of the submucosal liquid pad in each group were measured with a vernier caliper. All experiments were repeated 3 times.
[0077] Compared with the SIM medium (normal saline) commonly used in clinical practice, the mucosal elevation height decreases rapidly with the diffusion of normal saline; while the OCT hydrogel group can maintain the mucosal elevation height during a long surgical period, facilitating surgical operations ( Figure 2 B).
[0078] 3.3 OCT hydrogel in vitro adhesion strength test
[0079] The pig skin was fixed on a measuring device with a syringe pump containing PBS solution. After making a 5 mm long incision on the pig skin, 800 μL of OCT hydrogel pre-solution was injected into the incision. After keeping warm at 37°C for 15 minutes, one end of the tube connected to the PBS syringe pump was sealed. The syringe pump was pushed at a uniform rate to gradually increase the pressure on the pig skin wound surface, and the maximum burst pressure was recorded as the rupture pressure of the hydrogel when liquid flowed out of the incision. All tests were repeated 3 times.
[0080] Shear adhesion test: OCT hydrogel was used to bond two square pig skin surfaces (2 cm × 2 cm), and the two ends of the pig skin were fixed to the testing machine respectively. The maximum tensile force was recorded as the separation of the pig skin. All tests were repeated 3 times.
[0081] Adhesion test: The hydrogel was injected onto the surface of pig skin and pig intestine using a vortex mixer, and the pig skin and pig intestine were twisted and stretched to evaluate the adhesion and stretching ability of the hydrogel.
[0082] To further study the adhesion properties of the hydrogel after absorbing water, a piece of pig skin (10 cm × 2 cm) was prepared, and the hydrogel (2 cm × 1 cm) was synthesized in situ at the center of the inner surface of the pig skin. All hydrogels were placed at 37 ° C for 10 minutes until the mixture completely formed a hydrogel. The pig skin coated with hydrogel was curled in various ways and observed in a fast water flow to see if the hydrogel broke or fell off.
[0083] The normal rectal pressure is 76±23 mm Hg, and the maximum rectal pressure can reach 239±99 mm Hg. After ESD and TEM surgery, the intestinal mucosa is absent, which will cause the defect site to have a weak structure, which may lead to postoperative rectal perforation. Therefore, this embodiment cuts a 2 mm notch in the pig rectum and uses Figure 2 C's device simulated and tested the burst pressure of OCT hydrogel. Figure 2 D The results show that as the TP content increases, the burst pressure decreases accordingly. Despite this, the burst pressure of the OCT3 hydrogel group with the lowest burst pressure can still reach 245±83.63mm Hg, which can completely prevent the occurrence of perforation complications at the ESD and TEM surgical sites. In addition, the burst pressure of the OCT hydrogel far exceeds the normal blood pressure of 120mm Hg, and can also prevent intraoperative and postoperative bleeding. The shear adhesion test also showed similar results. As the TP content increases, the shear adhesion of the OCT hydrogel decreases ( Figure 2E and 2F). However, even when the pig skin was curled and flushed by high-speed water flow, the OCT3 hydrogel could still firmly adhere to the pig skin surface, further confirming the adhesion of the OCT3 hydrogel ( Figure 2 G).
[0084] 3.4 Self-healing performance test of OCT hydrogel
[0085] The self-healing properties of OCT hydrogels were evaluated by macroscopic and microscopic observation methods. From a macroscopic perspective, OCT3 hydrogels of different colors treated with red and blue dyes were injected into an "M"-shaped mold. After the hydrogels were gelled, they were taken out and cut into two halves. The OCT3 hydrogel pieces of different colors were put together and left for 2 hours. The self-healing properties of the OCT3 hydrogels were observed under an optical microscope and photographed.
[0086] The self-healing ability of OCT hydrogel was further evaluated by rheological methods. The precursor solution of OCT3 hydrogel was injected into the center of 40mm parallel plates through a vortex mixer, and the spacing distance was adjusted to 1.0mm. After the hydrogel was stabilized, the sample was sealed with dimethyl silicone oil to prevent water evaporation. Then a strain amplitude sweep was performed to record the storage modulus and loss modulus data. Then another hydrogel disk was used to perform an alternating strain sweep test at a fixed angular frequency (10rad / s) to test its self-healing behavior. The amplitude oscillation strain was switched from a small strain (y=1.0%, each interval of 6.2s) to a large strain (y=10%, each interval of 6.2s) and cycled 3 times.
[0087] As the intestines move, the hydrogel may suffer fatigue fracture, but due to the advantages of its dynamic Schiff base bonds and hydrogen bonds, the OCT hydrogel has the ability to self-repair. In order to further analyze the self-repair ability of OCT hydrogel, the cut hydrogels of different colors were spliced together for 120 minutes. The healed hydrogels can still maintain their integrity under the action of gravity, and the seams can be clearly observed through microscopic observation. The cracks disappeared and the dyes of different colors on both sides were stained ( Figure 2 H). Its self-healing performance was tested by using a rheometer, and the amplitude oscillation strain was switched from a small strain (y=1%, every 300s) to a large strain y=200%. The results showed that at a strain of 1%, G' was greater than G", and at a strain of 200%, G' was less than G", indicating that the OCT hydrogel was damaged. As the strain returned to 1%, G' returned to its previous level. After multiple cycles of testing, G' did not decrease significantly compared to before, confirming its excellent self-healing performance ( Figure 2 I).
[0088] Example 4 Test of OCT hydrogel inhibiting cancer cell proliferation and migration
[0089] 4.1 OCT hydrogel tea polyphenols release test
[0090] Prepare 400 μL of TP-loaded hydrogel and immerse it in 25 mL of PBS in a shaker at 37°C (~100 rpm). At specified time intervals, take 4 ml of the surrounding supernatant and measure the absorbance using a UV spectrophotometer. Analyze the TP content (R) in the dissolution sample with reference to the original standard curve. 2 >0.99).
[0091] Drug sustained release is one of the ways to maintain the drug's effective concentration for a relatively long time, achieve higher efficacy and no side effects. Figure 3 As shown in A, as the TP content increases, the release rate gradually accelerates. At 0.5 days, the release rates of OCT1 and OCT2 are similar, 43.45% and 42.82% respectively; while OCT3 can be quickly released up to 84.38%. OCT1 and OCT2 are close to complete release at 3.5 days, while OCT3 has been released on the third day.
[0092] 4.2 Test of the inhibitory ability of OCT hydrogel on human ileocecal cancer cells HCT-8.
[0093] Human ileocecal cancer cells HCT-8 were seeded in 96-well plates at a density of 5×10 3 Cells were incubated for 24 hours, and then 15 μL of hydrogel OCT0 / OCT1 / OCT2 / OCT3 was added and incubated for 1, 2, and 3 days. After incubation, the hydrogel was removed and 10 μL of CCK-8 and 100 μL of fresh culture medium were added to each well. Incubate at 37°C in a humidified incubator containing 5% CO2 for 2 hours. Then, 100 μL of culture medium in each well was transferred to a 96-well plate, and the OD value of each group was tested at 450nm using a microplate reader. The control group was without hydrogel.
[0094] The live / dead activity assay was used to evaluate the toxicity of the prepared OCT hydrogel to human ileocecal cancer cells HCT-8. HCT-8 cells were seeded in 6-well plates at a density of 3×10 5 cells, incubated for 24 h, then added 900 μL OCT0 / OCT1 / OCT2 / OCT3 hydrogels and continued incubation for 24 h. After incubation, the hydrogels were removed, washed once with PBS, and co-incubated with 2.5 μM calcein-AM and 2.5 μM ethylene dimer at 37°C for 20 min and observed under an inverted fluorescence microscope.
[0095] The effect of OCT hydrogel on the migration of human ileocecal cancer cells HCT-8 was tested by cell scratch assay. HCT-8 cells were plated at 3×10 5The cells were seeded in 6-well plates at a concentration of 10 cells / mL. After 24 h of incubation, scratches with a width of 400 μm were formed in each well, and then washed three times with PBS and incubated with each group of OCT hydrogels for 24 h. Digital images were captured using an inverted fluorescence microscope at 0, 12, and 24 h of incubation.
[0096] The OCT hydrogel had a significant inhibitory effect on the growth and migration of human ileocecal cancer cells HCT-8 by performing CCK-8 experiments, live-death experiments and cell scratch experiments. Figure 3 B The results of the CCK-8 experiment showed that from the first day to the third day, OCT hydrogel had a significant inhibitory effect on the proliferation of human ileocecal cancer cells HCT-8, and the OCT3 group had the most significant inhibitory effect on the growth of human ileocecal cancer cells HCT-8, mainly due to the rapid release of OCT3 drugs, which can quickly reach the effective concentration for inhibiting the proliferation and migration of cancer cells. The same results also appeared in the live-death experiment of human ileocecal cancer cells HCT-8 ( Figure 3 C). After quantification of the live-death experiment, it was found that the human ileocecal cancer cell HCT-8 in the control group had a higher activity, while a large number of human ileocecal cancer cells HCT-8 died after co-incubation with the OCT hydrogel extract, and the cell survival rate was below 21%. The survival rate of human ileocecal cancer cells HCT-8 in the OCT3 group was as low as 4.72±1.33% ( Figure 3 D).
[0097] The migration ability of cells determines the ability of tumor metastasis. In order to study the effect of OCT hydrogel in inhibiting cancer cell metastasis in vitro, this example uses the cell scratch method to investigate the effect of OCT hydrogel on the migration of human ileocecal cancer cells HCT-8. OCT hydrogel significantly inhibited the cell migration of human ileocecal cancer cells HCT-8, which was confirmed in the scratch experiment ( Figure 3 E). After quantification, it was found that the control group had healed 44.41±9.8% at 24h ( Figure 3 F). In comparison, the migration of human ileocecal cancer cells HCT-8 was significantly slow in each OCT hydrogel group, and the hydrogel group containing TP inhibited the migration of human ileocecal cancer cells HCT-8 more significantly.
[0098] This example tested the concentration of reactive oxygen species between the groups and found that the OCT hydrogel group had a significant inhibitory effect on the generation of reactive oxygen species in human ileocecal cancer cell HCT-8, and showed a TP concentration dependence ( Figure 3G). The proliferation and migration of cancer cells require a high level of reactive oxygen concentration. Therefore, the addition of TP can significantly inhibit the proliferation and migration of human ileocecal cancer cells HCT-8; and can synergistically inhibit the proliferation and migration of cancer cells with carboxymethyl chitosan to inhibit the expression of MMP-9, VEGF and E-selectin. The results showed that OCT3 hydrogel significantly inhibited the proliferation and migration of human ileocecal cancer cells HCT-8, showing great potential in inhibiting the proliferation and metastasis of cancer cells.
[0099] Advanced colorectal adenomas can be cured by removing the diseased mucosa through ESD and TEM surgery. However, when ESD and TEM surgery is performed for early colorectal cancer in the T1 stage, although the probability is extremely low, there is still a possibility of residual tumor cells or implanted metastasis. The OCT hydrogel SIM has a significant ability to inhibit the proliferation and migration of tumor cells, and can reduce the possibility of proliferation and metastasis of residual or implanted cancer cells. Therefore, the OCT hydrogel is used as a submucosal pad material to reduce the chance of recurrence after ESD and TEM surgery for early colorectal cancer in the T1 stage, and further consolidate the treatment effect.
[0100] Example 5 Biocompatibility and antibacterial ability of OCT hydrogel
[0101] 5.1 Blood compatibility test of OCT hydrogel
[0102] The hemolytic activity of the hydrogel was determined according to the direct contact method of ISO 10993-5. Rat anticoagulated whole blood that complies with relevant legal and institutional guidelines was selected for hemolysis assessment. 100uL of the prepared hydrogel OCT0 / OCT1 / OCT2 / OCT3 samples were stored in 1mL PBS solution; 1ml of anticoagulated blood was diluted with 5mL PBS; the diluted blood was dropped into the hydrogel suspension, double distilled water (positive control, hemolysis 100%) and PBS solution (negative control, hemolysis 0%) respectively; each group was placed in a 37°C incubator for 1h, centrifuged at 1500rpm / min for 5min; the absorbance of the supernatant was recorded at 540nm using an enzyme reader. The OD value of the OCT hydrogel is recorded as OD hydrogel The OD value of the positive control was recorded as OD positive The OD value of the negative control was recorded as OD negative The hemolysis rate (Hemolysis, %) was calculated as follows:
[0103]
[0104] 5.2 Cytocompatibility testing of OCT hydrogel
[0105] Cell proliferation (CCK-8): The hydrogel extract was used to analyze the effects of OCT0 / OCT1 / OCT2 / OCT3 on the behavior of mouse L929 fibroblasts. Briefly, the OCT0 / OCT1 / OCT2 / OCT3 precursor solution was exposed to ultraviolet light for 30 minutes to sterilize it, and then a sterile OCT hydrogel was formed under a sterile operating environment; then 100μL of OCT0 / OCT1 / OCT2 / OCT3 hydrogel was soaked in 8mL of DMEM culture medium at 37°C for 12 hours; the culture medium after soaking in each OCT hydrogel group was collected, filtered with a 0.22μM membrane filter, and sterilized again; the obtained solution was set as OCT0 / OCT1 / OCT2 / OCT3 hydrogel extract. In order to observe the proliferation of cells, L929 cells were cultured at 5×10 3 The cells were inoculated at a density of 100 μL / well in a 96-well plate, and first cultured with untreated DMEM medium (prepared with DMEM basal medium, fetal bovine serum and penicillin / streptomycin solution in a volume ratio of 90:10:1) for 24 h (37°C, 5% CO2). After L929 cells adhered to the wall, they were cultured with each group of OCT hydrogel extracts for 1, 3, and 5 days. The samples were collected and incubated with 100 μL of fresh DMEM solution containing 10% CCK-8 at 37°C for 1 h, and the absorbance of each group at 450 nm was measured with an ELISA reader.
[0106] 5.3 In vivo compatibility experiment of OCT hydrogel
[0107] In this embodiment, 0.5 mL of sterilized OCT0 / OCT1 / OCT2 / OCT3 precursor solution was injected into the same part of the back of the mouse subcutaneously. The mice were given appropriate diet and water. After 14 days, the five organs of the mouse, heart, liver, spleen, lung, and kidney, were fixed in 4% formaldehyde solution. In order to analyze the inflammatory response in vivo, hematoxylin and eosin (H&E) staining was performed on the five organ tissues of heart, liver, spleen, lung, and kidney according to the product instructions. Images were obtained under a microscope.
[0108] This example uses blood compatibility, cell compatibility and pathological HE staining to evaluate the biocompatibility of OCT hydrogel. The hemolysis results show that the hemolysis rates of OCT0, OCT1, OCT2 and OCT3 are 0.63±0.23%, 0.57±0.19%, 0.76±0.37% and 0.94±0.17%, respectively. All values are lower than the material hemolysis rate standard (2%) specified by the International Organization for Standardization (ISO) 10993-413, indicating that OCT hydrogel has excellent blood compatibility ( Figure 4 A).
[0109] In terms of cell compatibility, mouse fibroblast L929 cells were selected as template cells. Different groups of OCT hydrogel extracts were co-cultured with mouse fibroblast L929 cells, and the cytotoxicity of OCT hydrogel was evaluated using CCK-8. Figure 4 B), the results showed that L929 fibroblasts in each group proliferated significantly. After 1 day of incubation, there was no statistical difference between the groups. On the 3rd and 5th days, the cells in the OCT1 group had the best growth state, and there was no significant difference between the OCT0 hydrogel group and the control group, confirming that ODex and CS hydrogels had no obvious cytotoxicity. On the 5th day, TP in all groups had been released, and the OD values of the OCT2 and OCT3 hydrogel groups were lower than those of the control group, but the cell survival rate was still above 88% ( Figure 4 B) The results showed that TP was slightly toxic in terms of adhesion and proliferation of mouse fibroblast L929 cells.
[0110] In order to further test the biocompatibility of OCT hydrogel, in this example, each group of OCT3 hydrogel was buried under the skin of mice for 14 days, and then the heart, liver, spleen, lung, kidney and other organs of each group of mice were taken out for HE staining ( Figure 4 C). No obvious foreign body reaction such as edema, ulcers, and purulent secretions were found in the tissues surrounding the OCT3 hydrogel within 14 days. HE staining evaluation showed that there was no obvious inflammatory cell infiltration between the organs of the OCT3 group and the control group. The results were similar to those of the in vitro cell experiment, further confirming the excellent in vivo biocompatibility. The above results show that the OCT hydrogel has good blood compatibility, cell compatibility, and in vivo biocompatibility.
[0111] 5.4 OCT hydrogel antibacterial ability test
[0112] Preparation of culture medium:
[0113] (1) Liquid culture medium: Mix TSB / LB culture medium powder and deionized water in the mass-to-volume ratio specified in the instructions. Sterilize with high-pressure steam at 121°C for 20 min in an autoclave to obtain TSB liquid culture medium, which is then stored at 4°C for later use.
[0114] (2) Solid culture medium: Add 1.5% agar powder to TSB / LB liquid culture medium and sterilize it in an autoclave at 121°C for 20 min to obtain TSB solid culture medium. Cool it to 50-60°C and pour it into a bacterial culture dish in a clean bench. Wait for the culture medium to solidify before use.
[0115] Resuscitation of strains and isolation of single colonies: Take out the frozen Staphylococcus aureus and Escherichia coli from the -80℃ refrigerator and transfer them to a constant temperature water bath to thaw rapidly at 37℃. Take a small amount of bacterial solution with a sterile metal inoculation loop and spread it on TSB solid culture medium according to the quarter-line method. Transfer the agar plate to a bacterial incubator and culture it at 37℃ and 5% CO2 for 24 hours.
[0116] Strain amplification: Use a sterile metal inoculation loop to separate a single colony from the agar plate, inoculate it into 5 mL of TSB liquid medium, and culture it at 37°C and 5% CO2 for 24 h.
[0117] Cryopreservation of bacterial strains: Mix the bacterial solution with 50% (v / v) glycerol at a volume ratio of 1:1, pipette 1.5 mL of the mixture into a bacterial cryopreservation tube, and store in a -80°C refrigerator.
[0118] Gram-positive bacteria S. aureus and Gram-negative bacteria E. coli were used to detect the antibacterial ability of OCT0 / OCT1 / OCT2 / OCT3 hydrogels. Briefly, the OCT hydrogel precursor solution was filtered through a 0.22 μM membrane filter to remove bacteria from the OC hydrogel precursor solution; then 2 mL of the OCT precursor solution was soaked in disinfected PBS for 30 min, and then 5 mL of bacterial suspension (4×10 CFU / mL) was added, and incubated at 37°C for 12 h in a relatively humid environment; 10 μL of the treated bacterial suspension was inoculated on an agar plate and incubated in a 37°C incubator for 24 h; finally, the CFUs on the agar plate were counted, the control group was recorded as CFUc, and the sample group was recorded as CFUoct, and the antibacterial rate (Antibacterial rate%) was calculated as follows:
[0119]
[0120] The colorectal microenvironment is composed of a large number of bacterial communities. Although intestinal preparation is performed during ESD and TEM surgeries, a sterile environment cannot be formed. During ESD and TEM surgeries, intestinal mucosal lesions will be removed, resulting in the destruction of the intestinal mucosal barrier, which may cause bacteria to enter the blood vessels through venous ruptures, causing bacteremia. At the same time, the surgical wound is prone to postoperative wound infection due to the lack of barrier protection. Therefore, we conducted in vitro antibacterial experiments to test whether the antibacterial ability of OCT hydrogel can meet the needs of ESD and TEM surgeries. The in vitro antibacterial experiment used the colony forming unit (CFU) counting method to evaluate the antibacterial ability of OCT hydrogel against Escherichia coli (Gram-negative bacteria) and Staphylococcus aureus (Gram-positive bacteria). Figure 4As shown in Figure D, the antibacterial ability of each OCT group against Staphylococcus aureus was close to 100%. The antibacterial rate of the OCT3 group against Escherichia coli was as high as 82.87%. In vitro antibacterial experiments showed that OCT hydrogel has excellent broad-spectrum antibacterial ability. It can provide a physical barrier to prevent bacteria from entering the blood and causing bacteremia when the intestine has a large number of complex flora, coupled with excellent broad-spectrum antibacterial ability. OCT hydrogel has the ability to protect the wound surface and further reduce the incidence of postoperative infection after TAES. The antibacterial effect of OCT hydrogel may be that the aldehyde group of ODex can react with the primary amino group on the bacterial membrane, and CMCS can bind to the negatively charged bacterial surface, synergistically destroy the bacterial membrane, causing the leakage of bacterial components, thereby killing bacteria.
[0121] Example 6 Hemostatic properties of OCT hydrogel
[0122] 6.1 OCT hydrogel in vivo animal hemostasis experiment
[0123] A mouse liver bleeding model was used to simulate human visceral bleeding. This model was used to evaluate the hemostatic ability of OCT hydrogel in vivo. After 8-week-old male SD rats (200-220g) were anesthetized by intraperitoneal injection of 1% w / v pentobarbital solution, the liver was exposed and the tissue fluid around the liver was carefully wiped; the liver was placed on a pre-weighed filter paper, and a 3mm long and 1mm deep incision was made on the surface of the liver with a scalpel; the OCT hydrogels in each group were immediately sprayed on the bleeding site as a hemostatic sealant using a vortex mixer; commercially available hemostatic products were used. As a positive control, mice without hemostasis intervention were used as negative controls. The hemostasis process was photographed at specific times of 0, 15, 30, 60, and 120 seconds. The bleeding weight of each group was weighed and the hemostasis time of each group was calculated.
[0124] ESD and TEM surgery involves the removal of the intestinal mucosa at the site of lesions, which inevitably leads to bleeding. In mild cases, this will contaminate the surgical experiment and prolong the operation time. In severe cases, it may develop into massive bleeding or hematoma in the intestinal wall followed by secondary perforation. Therefore, SIM is required to have excellent hemostatic ability to avoid the above complications. This example uses a mouse liver bleeding model to test the hemostatic ability of OCT hydrogel, and uses Commercial hemostatic gauze was used as a positive control. Figure 5 As can be seen in A, the control group without intervention had a lot of bleeding. The OCT hydrogel group and the control group all had significant hemostatic effects. After qualitative analysis of the hemostasis time and blood loss, it was found that the control group needed 154.33±6.66s to complete self-hemostasis. The hemostatic time of the hemostatic gauze group was reduced to 77.66±7.64s. The hemostatic gauze group was further shortened. The OCT3 hydrogel group was even shortened to 15.33±2.52s ( Figure 5 B) The statistical results of blood loss are the same as the time to hemostasis. Hemostatic gauze can reduce blood loss, but the OCT3 group further reduced blood loss compared with the BP sponge group, and the results were statistically significant. The results showed that OCT hydrogel has excellent hemostatic ability, which is mainly attributed to the following aspects: 1. The rapid gelation ability and strong adhesion of OCT hydrogel can quickly seal the bleeding site and reduce blood loss. 2. The aldehyde group of ODex can promote the aggregation of red blood cells, platelets, fibrin and coagulation factors, and cooperate with the positive charge of CMCS to activate the coagulation cascade reaction and accelerate the formation of blood clots.
[0125] The present invention uses covalent bonds and hydrogen bonds to synthesize a new type of OCT hydrogel SIM with excellent antibacterial ability, outstanding antitumor effect, and strong hemostatic performance. The OCT hydrogel SIM can be used as a submucosal pad material in ESD and TEM surgery for benign and malignant rectal tumors, elevating the lesion mucosa, separating the lesion from the muscle layer, avoiding rectal perforation, facilitating the complete resection of the lesion, and reducing thermal damage to surrounding tissues. The SIM material has the ability of rapid gelation and self-healing, and its excellent injectability and long-term maintenance of submucosal pad height can facilitate the operation during ESD and TEM surgery and speed up the surgical process. At the same time, thanks to the strong adhesion performance, excellent antibacterial ability and excellent hemostatic effect of OCT hydrogel, the incidence of postoperative complications of ESD and TEM, such as rectal perforation, wound infection and bleeding, can also be reduced; and in various experiments against human ileocecal cancer cells HCT-8 in vitro, OCT hydrogel has shown a significant ability to inhibit cancer cell proliferation and migration, and is used for ESD and TEM surgery for patients with early colorectal T1 cancer, reducing the incidence of wound cancer cell proliferation and metastasis. The OCT hydrogel submucosal injection material developed by the present invention is a very promising auxiliary application material in colorectal ESD and TEM surgery, and has a significant positive effect on optimizing surgical operability, reducing collateral damage to surrounding tissues, increasing the effect of disease treatment, and reducing the incidence of postoperative complications.
[0126] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. An injectable hydrogel, characterized in that: Including carboxymethyl chitosan, oxidized dextran and tea polyphenols.
2. An injectable hydrogel according to claim 1, characterized in that: The mass ratio of carboxymethyl chitosan: oxidized dextran: tea polyphenols is 2.15-25: 1-4: 0.5-2.
3. The method for preparing the injectable hydrogel according to any one of claims 1 to 2, characterized in that: The steps include: S1, synthetic oxidized dextran Dissolve dextran and sodium periodate in double distilled water and stir in the dark; add ethylene glycol and stir in the dark to terminate the oxidation reaction; dialyze and then freeze-dry the purified original solution to obtain white sponge-like oxidized dextran; S2. Preparation of injectable hydrogel The tea polyphenols are dissolved in a carboxymethyl chitosan solution to prepare a mixture of the tea polyphenols and the carboxymethyl chitosan; the white spongy oxidized dextran is dissolved to prepare an oxidized dextran solution; the mixture of the tea polyphenols and the carboxymethyl chitosan is mixed with the oxidized dextran solution to obtain an injectable hydrogel.
4. The method for preparing the injectable hydrogel according to claim 3, characterized in that: In step S1, the molar ratio of oxidized dextran to sodium periodate is 3:1 to 1:
3.
5. The method for preparing the injectable hydrogel according to claim 4, characterized in that: In step S1, the molar numbers of ethylene glycol and sodium periodate are the same.
6. The method for preparing the injectable hydrogel according to claim 5, characterized in that: In step S1, the dialysis time is 72 to 96 hours, the dialysis fluid is double distilled water, and the dialysis fluid is replaced every four hours during the dialysis process.
7. The method for preparing the injectable hydrogel according to claim 6, characterized in that: In step S2, the concentration of the carboxymethyl chitosan solution is 2% to 3%.
8. The method for preparing the injectable hydrogel according to claim 7, characterized in that: In step S2, the volume ratio of the mixture of tea polyphenols and carboxymethyl chitosan to the oxidized dextran solution is 2:1 to 1:2, and the concentration of the oxidized dextran solution is 20% to 30%.
9. Use of the injectable hydrogel according to any one of claims 1 to 2, or the injectable hydrogel prepared by the preparation method according to any one of claims 3 to 8, characterized in that: Used to prepare submucosal injection materials for colorectal mucosal dissection.
Citation Information
Patent Citations
Antibacterial compound hydrogel and preparation method thereof
CN111150880A
Tea polyphenol hydrogel as well as preparation method and application thereof
CN116808285A
Supramolecular hydrogel based on natural plant components as well as preparation and application of supramolecular hydrogel
CN117084970A
Dextran-chitosan based in-situ gelling hydrogels for biomedical applications
US20110076332A1
Cited By
Hydrogel as well as preparation method and application thereof
CN120643755A