Preparation method of negative electrode of lithium ion battery and assembly method of lithium ion battery

By using the prelithiation reagent of phenanthrene tablets in organic solvents to process the silicon carbon negative electrode to form an SEI film, the problem of active Li+ consumption of silicon-based materials in lithium-ion batteries in the initial charge and discharge cycle is solved, and the initialization is improved Coulomb efficiency and cycle stability improve the performance of lithium-ion batteries.

CN118888697APending Publication Date: 2024-11-01HUBEI UNIV +1

Patent Information

Application Number
CN202410960731.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The formation and side reaction of the SEI film in the initial charge and discharge cycle of silicon-based materials in lithium-ion batteries lead to active Li+ consumption, resulting in low initial Coulomb efficiency, and the breaking of silicon particles leads to electrode grinding, and the electrolyte is consumed quickly, limiting the silicon-based materials. Application.

Method used

The prelithiation reagent prepared by phenanthrene lithium sheets in organic solvents was used to process the silicon carbon anode to form a SEI film, compensate for the irreversible capacity of the anode, improve the initial Coulomb efficiency and cycle stability of the anode, and reduce the prelithiation process. Active Li+ consumption in the electrolyte.

Benefits of technology

By prelithiation, the initial Coulomb efficiency and reversible capacity of the silicon carbon negative electrode are improved, the electrochemical performance is improved, the consumption of electrolyte is reduced, and the circulation stability of lithium-ion batteries is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888697A_ABST
    Figure CN118888697A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a lithium ion battery negative electrode and an assembly method of a lithium ion battery, and relates to the technical field of lithium ion batteries. According to the method, a silicon-carbon negative electrode is treated by adopting a pre-lithiation reagent composed of phenanthrene, lithium and an organic solvent, so that SEI film coating can be realized during pre-lithiation, and the formation of the SEI film can effectively compensate the irreversible capacity of the positive electrode, improve the ICE of the negative electrode and improve the electrochemical performance of the negative electrode and the cycling stability of the battery; the SEI film is formed in the pre-lithiation process, so that the consumption of active Li < + > in the electrolyte is reduced, the loss of the active Li < + > of the negative electrode in the initial several cycle processes is compensated, and the ICE and the reversible capacity of the silicon-carbon negative electrode are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a negative electrode of a lithium ion battery and a method for assembling a lithium ion battery. Background Art

[0002] Lithium-ion batteries (LIBs) are widely used in new energy vehicles, portable devices, power grids and other fields due to their high energy density, long cycle life, light weight and low environmental pollution. However, the energy density of lithium-ion batteries is far from meeting market needs. The development of high-energy-density electrode materials has attracted the attention of researchers as one of the important ways to improve the energy density of LIBs. Among them, silicon-based materials can be used as a substitute for the next generation of negative electrode materials due to their high specific capacity, large storage capacity, wide sources and environmental friendliness. However, in the initial charge and discharge cycle, the formation of the SEI film and the occurrence of related side reactions consume a certain amount of active Li + , resulting in low initial Coulomb efficiency (ICE) of silicon-based materials, and large volume changes in the subsequent charge and discharge process will cause the electrode to grind and the active material to lose contact with the current collector. In addition, the frequent breakage of silicon particles will cause the SEI film on its surface to break up repeatedly, leading to rapid consumption of the electrolyte and a rapid decrease in the capacity of the silicon-based anode. These problems, including low conductivity, limit the practical application of silicon-based materials.

[0003] Compared with electrochemical pre-lithiation and active material-assisted pre-lithiation, chemical pre-lithiation has attracted widespread attention due to its advantages such as low cost, simple operation, easy control of pre-lithiation degree and more uniform pre-lithiation. Chemical pre-lithiation uses lithium-containing compounds with strong reducing ability to spontaneously transfer Li+ to the anode material through redox reactions. This method can effectively compensate for the irreversible capacity of the anode, increase the ICE of the anode, and improve the electrochemical performance of the anode. At present, the most frequently used chemical pre-lithiation reagents are mainly aromatic lithium solutions (Li-Naph, Li-Bp and Li-FIr, etc.). In aromatic lithium solutions, the lithium radical anions of aromatics are a series of organic metal complexes with a reducing ability almost as strong as that of metallic lithium itself. According to existing literature reports, Luo et al. used a redox potential of ~0.19V (vs.Li / Li + ) lithium-naphthalene-2-methyltetrahydrofuran (Li-Naph / 2MT) solution effectively pre-lithiated the graphite anode in a few minutes, compensating for the irreversible loss of active lithium in the graphite anode during the initial charge and discharge process, and improving the ICE and energy density of the graphite anode.

[0004] In view of this, it is necessary to design an improved method for preparing a negative electrode of a lithium ion battery and an assembly method of a lithium ion battery to solve the above problems. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a negative electrode of a lithium ion battery and a method for assembling a lithium ion battery.

[0006] To achieve the above-mentioned purpose of the invention, on the one hand, the present invention provides a method for preparing a negative electrode for a lithium ion battery, which is carried out as follows: immersing a silicon-carbon negative electrode in a pre-lithiation reagent to obtain the negative electrode for the lithium ion battery; wherein the pre-lithiation reagent is prepared by dissolving phenanthrene and lithium sheets in an organic solvent, and the concentrations of lithium ions and phenanthrene in the pre-lithiation reagent are both 1 mol / L.

[0007] Preferably, the immersion time of the silicon-carbon negative electrode in the pre-lithiation reagent is 0-120 min.

[0008] Preferably, the organic solvent is 2-methyltetrahydrofuran.

[0009] Preferably, the silicon-carbon negative electrode is prepared as follows: the active material, SuperP and polyacrylic acid are dispersed in water to form a slurry, and the slurry is evenly coated on a copper foil, vacuum dried, and then punched into sheets to obtain a silicon-carbon negative electrode. Preferably, the active material is a commercial silicon / carbon material, and the mass ratio of the active material, the SuperP and the polyacrylic acid is 7:2:1.

[0010] On the other hand, the present invention provides a method for assembling a lithium ion battery, which is as follows: a lithium sheet is used as a counter electrode, a polypropylene film is used as a diaphragm, and a mixed solution containing lithium hexafluorophosphate is used as an electrolyte, and the lithium ion battery negative electrode is assembled together to form a lithium ion battery.

[0011] Preferably, the mixed solution is a mixture of ethylene carbonate, diethyl carbonate, ethyl methyl carbonate and fluoroethylene carbonate, the volume ratio of the ethylene carbonate, the diethyl carbonate and the ethyl methyl carbonate is 1:1:1, and the volume of the fluoroethylene carbonate is 10% of the total volume of the ethylene carbonate, the diethyl carbonate and the ethyl methyl carbonate.

[0012] Preferably, the concentration of lithium hexafluorophosphate in the electrolyte is 1 mol / L.

[0013] The beneficial effects of the present invention are:

[0014] The preparation method of the negative electrode of a lithium ion battery provided by the present invention can realize SEI film coating during pre-lithiation by treating the silicon-carbon negative electrode with a pre-lithiation reagent composed of phenanthrene, lithium and an organic solvent (2-methyltetrahydrofuran). The formation of the SEI film can effectively compensate for the irreversible capacity of the anode, increase the ICE of the negative electrode, improve the electrochemical performance of the negative electrode, and the cycle stability of the battery; by forming the SEI film during the pre-lithiation process, the active Li in the electrolyte is reduced.+ consumption, compensating for the active Li + loss, improving the ICE and reversible capacity of the silicon-carbon negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a SEM image of the negative electrode of the lithium ion battery prepared in Example 1 of the present invention;

[0016] Figure 2 TEM image of the negative electrode of the lithium ion battery prepared in Example 1 of the present invention;

[0017] Figure 3 This is a SEM image of the silicon-carbon negative electrode used in Example 1 of the present invention;

[0018] Figure 4 TEM image of the silicon-carbon negative electrode used in Example 1 of the present invention;

[0019] Figure 5 is the redox potential of Li-phe / 2-MTHF used in Example 1 of the present invention;

[0020] Figure 6 The initial discharge curve and initial charge and discharge capacity of the negative electrode of the lithium-ion battery prepared under different treatment times and the cycle performance diagram at a current density of 0.5A / g;

[0021] Figure 7 The dQ / dV curve of the silicon-carbon negative electrode prepared with a pre-lithiation time of 0-30min during the first discharge cycle;

[0022] Figure 8 The XPS graphs of the negative electrode of lithium-ion battery prepared at pre-lithiation time of 0 and 5 min respectively;

[0023] Fig. 9 are the initial coulombic efficiency and open circuit voltage of the negative electrode material obtained when the pre-lithiation time is 0 and 5 min respectively;

[0024] Fig.10 The CV curves of the negative electrode of the lithium-ion battery prepared at the pre-lithiation time of 0 and 5 min at a scan rate of 0.1 mV / s. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0026] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0027] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0028] On the one hand, the present invention provides a method for preparing a negative electrode for a lithium ion battery, and the preparation method is as follows: immersing a silicon-carbon negative electrode in a pre-lithiation reagent to obtain a negative electrode for a lithium ion battery; wherein the pre-lithiation reagent is prepared by dissolving phenanthrene (phe) and a lithium sheet in an organic solvent, and the concentration of lithium in the pre-lithiation reagent is 1 mol / L, and the concentration of phenanthrene is 1 mol / L.

[0029] Conventional SiC anodes without pre-lithiation consume active Li in the electrolyte during the first few electrochemical cycles. + The SEI film is formed, which causes some active Li + The dead lithium makes the initial coulombic efficiency (ICE) of the silicon-carbon negative electrode low, and the active Li + The content determines its reversible capacity. After pre-lithiation of the silicon-carbon negative electrode, the active Li in the electrolyte can be reduced by forming a SEI film before the electrochemical cycle process. + consumption, compensating for the active Li + loss, improving the ICE and reversible capacity of the silicon-carbon negative electrode.

[0030] As an embodiment of the present invention, the immersion time of the silicon-carbon negative electrode in the pre-lithiation reagent is 0-120 min, preferably 0-30 min, and more preferably 5 min. Specifically, the silicon-carbon negative electrode is prepared according to the following method: the active material (commercial silicon / carbon material), SuperP and polyacrylic acid are dispersed in water according to a mass ratio of 7:2:1 to form a slurry, and then the slurry is evenly coated on a copper foil, vacuum dried, and stamped into sheets to obtain a silicon-carbon negative electrode; wherein the added mass ratio of conductive carbon black and polyacrylic acid is 7:2:1, the vacuum drying temperature is 80°C, and the time is 12h.

[0031] As an embodiment of the present invention, the organic solvent is 2-methyltetrahydrofuran (2-MTHF).

[0032] The aromatic lithium solution commonly used in the pre-lithiation process consists of two parts: a complex of polycyclic aromatic hydrocarbon ions, lithium ions and solvents. The polycyclic aromatic hydrocarbons are a large planar π-conjugated molecule that can combine with electrons to form an ionic structure, which plays a role in stabilizing the structure and can adjust its affinity, thereby adjusting the reducing ability of the solution. The solvent is often an ether, such as ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF) and 2-methyltetrahydrofuran (2-MTHF), but cyclic ethers (THF) are more compatible with Li than polydentate ethers (DME) containing multiple ether groups. + 2-MTHF has a higher coordination number when coordinated, and its greater electron-donating property can shift the redox potential of the aromatic lithium solution negatively. Therefore, phenanthrene was selected as the polycyclic aromatic hydrocarbon and 2-MTHF as the solvent to prepare the pre-lithiation reagent.

[0033] On the other hand, the present invention also provides a method for assembling a lithium ion battery using the above-mentioned lithium ion battery negative electrode, and the specific steps are as follows: using a lithium sheet as a counter electrode, a polypropylene film as a diaphragm, and a mixed solution containing lithium hexafluorophosphate (LiPF6) as an electrolyte, and assembling them together with the lithium ion battery negative electrode into a lithium ion battery.

[0034] As an embodiment of the present invention, the mixed solution is a mixture of ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and fluoroethylene carbonate (FEC), ethylene carbonate is solid at room temperature, and is heated and melted into a liquid before use, the volume ratio of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate is 1:1:1, the concentration of lithium hexafluorophosphate in the electrolyte is 1mol / L, and the added volume of fluoroethylene carbonate is 10% of the total volume of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate. The electrolyte is prepared according to the following method: after heating ethylene carbonate, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate are uniformly mixed according to a volume ratio of 1:1:1, LiPF6 is added to ensure that the concentration of LiPF6 is 1mol / L, and then fluoroethylene carbonate is added, and the added volume of fluoroethylene carbonate is 10% of the total volume of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0035] The following is a further description of the method for preparing the negative electrode of a lithium ion battery and the method for assembling a lithium ion battery proposed by the present invention in conjunction with specific embodiments:

[0036] The sources of raw materials used in the embodiments of the present invention are as follows: ethylene carbonate, diethyl carbonate, ethyl methyl carbonate, and fluoroethylene carbonate were purchased from Nobond with analytical purity; dimethyltetrahydrofuran was purchased from Aladdin with analytical purity; polyacrylic acid was purchased from Aladdin; silicon-carbon materials were purchased from Shanghai Shanshan; battery accessories such as electrode shells were purchased from Cluder. Unless otherwise specified, other raw materials can be purchased on the market.

[0037] Example 1

[0038] This embodiment prepares a lithium ion battery negative electrode, and its specific preparation method is as follows:

[0039] 1.4258 g phe was dissolved in 8 mL of 2-MTHF, and 0.06 g of lithium sheet (excess) was added and stirred for 12 h to prepare a 1 M Li-phe / 2-MTHF pre-lithiation reagent; the silicon-carbon negative electrode was immersed in the above-mentioned pre-lithiation reagent for 5 min to pre-lithiate the silicon-carbon negative electrode, and was washed three times with 2-MTHF to remove the residual pre-lithiation reagent on the pre-lithiated silicon-carbon electrode, and dried under vacuum to obtain a lithium-ion battery negative electrode. The pre-lithiation treatment was carried out in a glove box.

[0040] Among them, the silicon-carbon negative electrode is prepared by the following method: commercial silicon / carbon material, Super P and polyacrylic acid are dispersed in deionized water at a mass ratio of 7:2:1 to prepare a slurry, and the slurry is evenly coated on a copper foil, vacuum dried at 80°C for 12 hours, and the copper foil coated with the dried material is punched into a 8mm disc to prepare a silicon-carbon negative electrode. It should be noted that the reagents and raw materials used in the present invention, unless otherwise specified, can be obtained by purchasing on the market.

[0041] The SEM image of the pre-lithiated silicon-carbon anode is shown in Figure 1 As shown in the figure, it can be seen that there are several fine films on the surface of the silicon-carbon negative electrode after pre-lithiation. The production of the film makes the cracks on the silicon-carbon negative electrode smaller, and the surface of the exposed electrode material inside is also covered with a layer of material, which may be produced by the reaction between the silicon-carbon negative electrode and the pre-lithiation reagent during the pre-lithiation process; TEM picture is shown in Figure 2 As shown in the figure, it can be seen that after pre-lithiation, the surface of the silicon-carbon negative electrode is covered with a layer of film. The SEM and TEM images of the silicon-carbon negative electrode that has not been pre-lithiated are shown in Figure 1. Figure 3 , Figure 4 As shown in the figure, it can be seen that the surface is smooth and has cracks with relatively wide width, through which the exposed silicon-carbon material and conductive carbon black can be observed.

[0042] In order to verify the feasibility of using Li-phe / 2-MTHF pre-lithiation reagent to pre-lithiate silicon-carbon anode, the redox potential of Li-phe / 2-MTHF was measured by cyclic voltammetry (CV). Figure 5 As shown, Figure 5 As shown in a, the redox potential of the organic pre-lithiation reagent is 0.25 V (vs. Li / Li + ); Figure 5 b is the dQ / dV curve of the original silicon-carbon negative electrode in the first three cycles. The silicon-carbon material is at 0.04, 0.08 and 0.15V (vs. Li / Li + ) has three peaks corresponding to Li+ During the initial discharge process, the formation of the solid electrolyte interface (SEI) and other side reactions lead to a single peak in the dQ / dV curve, which is located at 0-0.1V (vs. Li / Li + ), in addition, it can be observed that at 0.5-0.6V (vs.Li / Li + ) range, the SEI film corresponding to the broad peak is formed, and the potential of the three is compared ( Figure 5 c) Li-phe / 2-MTHF uses its excellent redox properties to form SEI film. The unpre-lithiated silicon-carbon anode consumes part of the active Li in the initial electrochemical cycle. + To form the SEI film, the silicon-carbon negative electrode is pre-lithiated by Li-phe / 2-MTHF to form the SEI film in advance before the electrochemical cycle, thereby compensating for the active Li of the silicon-carbon material in the initial electrochemical cycle. + Consumption, increase active Li + content, thereby improving the reversible capacity of the silicon-carbon material in the cycle.

[0043] Furthermore, this embodiment also explores the performance difference of the negative electrode of the lithium ion battery prepared under different pre-lithiation treatment times. The pre-lithiation treatment time is 0, 1, 5, 10, 30, 60, and 120 minutes. The initial discharge curve and initial charge and discharge capacity of the negative electrode of the lithium ion battery prepared under different treatment times and the cycle performance at a current density of 0.5A / g are as follows: Figure 6 As shown in the figure, the dQ / dV curve of the silicon-carbon negative electrode prepared with a pre-lithiation time of 0-30min during the first cycle discharge process is as follows Figure 7 As shown in the figure, it can be seen that when the pre-lithiation time is 5 minutes, the performance of the prepared lithium-ion battery negative electrode is optimal.

[0044] Example 2

[0045] In this embodiment, the negative electrode of the lithium ion battery prepared in Example 1 is further assembled into a lithium ion battery. The specific assembly method is as follows:

[0046] After mixing ethylene carbonate, diethyl carbonate and ethyl methyl carbonate in a volume ratio of 1:1:1, a certain mass of lithium hexafluorophosphate was dissolved, and 10% of fluoroethylene carbonate was added to prepare a 1 mol / L lithium hexafluorophosphate electrolyte; then, a silicon-carbon anode and a pre-lithiated silicon-carbon anode (lithium-ion battery anode) were used as the anode, a lithium sheet was used as the counter electrode, and a Celgard2400 polypropylene film was used as the diaphragm. A half-cell of model CR2025 was assembled in a glove box filled with high-purity argon gas and oxygen and water content less than 0.1ppm. A constant current charge-discharge experiment of 0.01-3.0V was carried out on a Neware test system, and a cyclic voltammetry (CV) test with a scan rate of 0.1mV / s was carried out on an electrochemical workstation (CHI600E, Shanghai).

[0047] The XPS images of the negative electrode of the lithium-ion battery prepared at the pre-lithiation time of 0 and 5 min are as follows: Figure 8 a, After 5 min of pre-lithiation treatment, a Li 1s peak is generated in the material, and the peak intensities of O1s and Li 1s change, proving that the pre-lithiation process is effective in the negative electrode material; O 1s and Li 1s The figures are as follows Figure 8 b and 8c, Figure 8 Li in the negative electrode material after pre-lithiation for 5 min in b x SiO y The generation of Li(56.0eV), Li2CO3(55.3eV) and LiOR(54.5eV) peaks is attributed to the redox reaction between the pre-lithiation reagent and the silicon-carbon anode to form the SEI film. Figure 8 The changes in the peak intensities of O=CO (533.3 eV) and Si-O (532.2 eV) in c and the changes in the peak intensities of Li2CO3 (531.3 eV) and Li x SiO y The generation of the (531.4eV) peak also confirms the above conclusion; the initial coulombic efficiency (ICE) and open circuit voltage (OCP) of the negative electrode material prepared when the pre-lithiation time is 0 and 5min respectively are as follows Fig. 9 As shown in the figure, the CV curves of the negative electrode of the lithium-ion battery prepared when the pre-lithiation time is 0 and 5 min respectively at a scan rate of 0.1 mV / s are as follows Fig.10 As shown, the results show that the OCP of the silicon-carbon electrode treated with Li-phe / 2-MTHF pre-lithiation showed a downward trend. However, ICE, initial charge and discharge capacity and capacity during the cycle were significantly improved. When the pre-lithiation time was 5 minutes, ICE increased from 83% to 90%, but further increasing the pre-lithiation time did not significantly improve ICE. At this time, the initial charge and discharge capacity of the silicon-carbon electrode was the highest, which were 587.5 mA / g and 652.1 mA / g respectively, and the cycle performance was also the best.

[0048] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a negative electrode of a lithium ion battery, It is characterized in that The process is as follows: immersing the silicon-carbon negative electrode in a pre-lithiation reagent to obtain the lithium-ion battery negative electrode; wherein the pre-lithiation reagent is prepared by dissolving phenanthrene and lithium sheets in an organic solvent, and the concentrations of lithium ions and phenanthrene in the pre-lithiation reagent are both 1 mol / L.

2. The method for preparing a negative electrode for a lithium ion battery according to claim 1, It is characterized in that The immersion time of the silicon-carbon negative electrode in the pre-lithiation reagent is 0-120 minutes.

3. The method for preparing a negative electrode of a lithium ion battery according to claim 1, It is characterized in that The organic solvent is 2-methyltetrahydrofuran.

4. The method for preparing a negative electrode for a lithium ion battery according to claim 1, It is characterized in that The silicon-carbon negative electrode is prepared according to the following method: the active material, Super P and polyacrylic acid are dispersed in water to prepare slurry, and the slurry is evenly coated on a copper foil, vacuum dried, and then punched into sheets to prepare the silicon-carbon negative electrode.

5. The method for preparing a negative electrode for a lithium ion battery according to claim 3, It is characterized in that The active material is a commercial silicon / carbon material, and the added mass ratio of the active material, the Super P, and the polyacrylic acid is 7:2:

1.

6. A negative electrode for a lithium ion battery prepared by the preparation method according to any one of claims 1 to 5.

7. Application of a lithium ion battery negative electrode prepared by the preparation method according to any one of claims 1 to 5 in the field of lithium ion batteries.

8. A method for assembling a lithium-ion battery, It is characterized in that The assembly method is as follows: a lithium sheet is used as a counter electrode, a polypropylene film is used as a diaphragm, a mixed solution containing lithium hexafluorophosphate is used as an electrolyte, and the lithium ion battery negative electrode is assembled together to form a lithium ion battery.

9. The method for assembling a lithium-ion battery according to claim 8, It is characterized in that The mixed solution is a mixture of ethylene carbonate, diethyl carbonate, ethyl methyl carbonate and fluoroethylene carbonate, the volume ratio of the ethylene carbonate, the diethyl carbonate and the ethyl methyl carbonate is 1:1:1, and the volume of the fluoroethylene carbonate is 10% of the total volume of the ethylene carbonate, the diethyl carbonate and the ethyl methyl carbonate.

10. The method for assembling a lithium-ion battery according to claim 8, It is characterized in that The concentration of lithium hexafluorophosphate in the electrolyte is 1 mol / L.

Citation Information

Patent Citations

  • Lithium ion supplementing technology of lithium ion batteries

    CN108520978A

  • Lithium ion battery negative electrode and pre-lithiation method and application thereof

    CN110120496A

  • Lithium supplementing method of lithium ion battery negative electrode active material

    CN112234160A

  • Chemical pre-lithiation method for graphite electrode of lithium ion battery

    CN112490394A

  • Method for synthesizing high-performance lithium ion battery positive electrode material by using waste lithium ion battery

    CN113764762A

Cited By

  • Battery cell and preparation method therefor, battery device, and electric device

    WO2026045274A1

  • Lithium secondary battery, negative electrode active material and preparation method therefor, and electric device

    WO2026166257A1