Aqueous zinc ion battery electrolyte and preparation method and application thereof
By adding carboxylic acid derivative anhydride to the electrolyte of the aqueous zinc ion battery, the problems of zinc negative electrode dendrite growth and hydrogen evolution corrosion are solved, the specific capacity and cycle stability of the battery are improved, and more efficient electrochemical performance is achieved.
Patent Information
- Application Number
- CN202410899243.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
AI Technical Summary
Problems such as dendrite growth, hydrogen evolution corrosion and by-product formation of aqueous zinc ion batteries in zinc negative electrodes affect their circulation performance, energy density and power density, and the existing electrolytes have insufficient protection effect on zinc negative electrodes.
By adding carboxylic acid derivative acid anhydride as an additive to the electrolyte, the solvated structure of zinc is destroyed by its hydrolyzed properties, adsorbing it on the surface of the zinc negative electrode, adjusting the local pH value, inhibiting the generation of the passivation layer, and protecting the zinc negative electrode.
It significantly improves the specific capacity, rate performance and cycle stability of zinc ion batteries, inhibits dendrites growth and corrosion of zinc negative electrodes, and extends the service life of the battery.
Smart Images

Figure CN118888871A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energy storage materials, and specifically relates to an aqueous zinc ion battery electrolyte and a preparation method and application thereof. Background Art
[0002] With the continuous development of human social economy, the over-exploitation of fossil energy, energy shortage and environmental pollution have become the most serious problems facing mankind in the 21st century. It is urgent to find and develop new renewable clean energy (such as solar energy, wind energy, hydropower, tidal energy, hydrogen energy, etc.).
[0003] The most commercialized lithium-ion battery on the market has the advantages of high energy density, high open circuit voltage, high output power, no memory effect, and low self-discharge. However, it has certain safety hazards. For example, it will become unstable under conditions of overcharge, over-discharge, high temperature, or incompatible electrolyte, and may cause explosions, fires, and other problems. Compared with organic electrolytes, aqueous electrolytes are safe, green, efficient, and can operate in a wider temperature range (for example, traditional organic batteries can only operate under conditions below 60°C). Therefore, using aqueous electrolytes to replace organic electrolytes is one of the effective ways to solve the flammability, toxicity, and low safety of organic electrolytes. In addition, the ionic conductivity of aqueous electrolytes (1S cm -1 ) is much higher than the conductivity of organic electrolyte (~1-10mS cm -1 ), which is beneficial to improving the rate performance of electrode materials and can increase the response speed of large-scale energy storage devices during use.
[0004] Among many aqueous batteries, aqueous zinc-ion batteries have attracted attention due to their high energy density and power density, mainly because the zinc metal negative electrode has a high theoretical capacity (820 mAh g -1 ), low redox potential (-0.762 V compared to standard hydrogen electrode), high cost-effectiveness, and environmental friendliness, and are widely considered to be promising candidates. In recent years, a lot of research has been done on the electrochemical performance of cathode materials for aqueous zinc-ion batteries (ZIBs), and their specific capacity (250-350 mAh g -1 ) and life (≥1000 cycles) have made great progress.
[0005] However, the development of aqueous zinc-ion batteries still faces huge challenges. Dendrite growth, hydrogen corrosion, and byproduct formation of zinc negative electrodes have a great impact on the cycle performance, energy density, and power density of zinc-ion batteries. The emergence of electrolyte additives has played an unexpected role in inhibiting the side reactions of zinc negative electrodes. Zinc is an ideal negative electrode material for the new generation of rechargeable batteries. The exploration and design of harmless zinc negative electrode additives has become the key to the green development of aqueous zinc-ion batteries. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an aqueous zinc ion battery electrolyte. The electrolyte can protect the negative electrode by hydrolyzing the additive acid anhydride itself, and the product (carboxylic acid) after the decomposition of the acid anhydride and the acid anhydride itself are equivalent to the two additives acting together on the negative electrode.
[0007] The present invention also provides a method for preparing the aqueous zinc ion battery electrolyte.
[0008] The invention also proposes an application of an aqueous zinc ion battery electrolyte.
[0009] Specifically, the present invention also proposes an aqueous zinc ion battery.
[0010] According to one aspect of the present invention, an aqueous zinc ion battery electrolyte is provided. The electrolyte includes an additive, wherein the additive includes a carboxylic acid derivative anhydride.
[0011] Carboxylic acid derivatives are compounds produced by replacing the hydroxyl group in the carboxylic acid molecule with other atoms or atomic groups such as halogens and amino groups, including acyl halides, anhydrides, esters, amides, etc. These four carboxylic acid derivatives can be hydrolyzed, among which acyl halides and anhydrides are easy to hydrolyze, while the hydrolysis of esters and amides requires the addition of acids or bases as catalysts, and also requires heating. After the hydrolysis of acyl halides, hydrogen halides (HCl, HF, HBr) are generated, all of which are strong acids, while acid anhydrides can generate carboxylic acids after hydrolysis.
[0012] When the anhydride is hydrolyzed, part of it will destroy the Zn 2+ The solvated structure can also be adsorbed on the surface of the zinc negative electrode to induce uniform deposition of zinc; a part of it forms carboxylic acid in the zinc salt solution to regulate the local OH caused by the hydrogen evolution reaction. - The problem of pH increase caused by the increase in concentration is solved, thereby inhibiting the formation of the passivation layer and ensuring the active nucleation sites of Zn.
[0013] In some experimental modes of the present invention, the acid anhydride includes at least one of acetic anhydride, propionic anhydride, succinic anhydride, maleic anhydride, benzoic anhydride, and phthalic anhydride.
[0014] In some preferred experimental modes of the present invention, the acid anhydride is succinic anhydride and maleic anhydride, and succinic anhydride is more preferred. Succinic anhydride is easier to hydrolyze and has better protection performance for the negative electrode when used as an electrolyte additive.
[0015] In some experimental modes of the present invention, the electrolyte further comprises a soluble zinc salt and a solvent.
[0016] In some experimental modes of the present invention, the zinc salt includes zinc sulfate and or zinc trifluoromethanesulfonate. Preferably, the zinc salt is zinc sulfate.
[0017] In some experimental modes of the present invention, the solvent includes water. Preferably, the solvent is deionized water or pure water.
[0018] In some experimental modes of the present invention, in the electrolyte, the molar ratio of the acid anhydride to the zinc salt is 1:(10-100).
[0019] In some preferred experimental modes of the present invention, the molar ratio of the anhydride to the zinc salt is 1:(25-75), for example, the molar ratio of the anhydride to the zinc salt can be about 1:25, about 1:40, about 1:50, about 1:60 or about 1:75; more preferably about 1:50.
[0020] In some experimental methods of the present invention, in the electrolyte, the concentration of zinc salt is 1-3 mol / L, for example, about 1 mol / L, about 1.5 mol / L, about 2 mol / L, about 2.5 mol / L or about 3 mol / L; preferably, the concentration of zinc salt is about 2 mol / L.
[0021] Another aspect of the present invention provides a method for preparing an aqueous zinc ion battery electrolyte, comprising the following steps:
[0022] The aqueous zinc ion battery electrolyte is obtained by mixing the zinc salt, the acid anhydride and the solvent and dispersing and dissolving them.
[0023] The raw materials used in the present invention are widely available, environmentally friendly, safe and pollution-free, and have good application prospects for zinc ion batteries. The present invention adopts a normal temperature stirring method to form an electrolyte containing a carboxylic acid derivative anhydride, and the preparation process is extremely simple, shortening the preparation time, reducing the synthesis path, reducing the cost, and being applicable to mass production.
[0024] In some embodiments of the present invention, the operating temperature is room temperature. Preferably, the operating temperature is 10°C-40°C, such as about 25°C or about 30°C.
[0025] In some experimental methods of the present invention, in order to accelerate dissolution, the stirring dissolution step includes stirring dispersion and ultrasound. Preferably, the stirring time is more than 24 hours; the ultrasound time is more than 1 hour; more preferably, the stirring time is 24-48 hours, such as about 36 hours; the ultrasound time is 1-3 hours, such as about 2 hours.
[0026] In some preferred experimental methods of the present invention, the zinc salt is first mixed with a solvent, dispersed and dissolved to obtain a zinc salt solution; then the acid anhydride is mixed with the zinc salt solution, dispersed and dissolved to obtain the aqueous zinc ion battery electrolyte.
[0027] Another aspect of the present invention provides the use of the above aqueous zinc ion battery electrolyte in an aqueous zinc ion battery.
[0028] Another aspect of the present invention provides an aqueous zinc ion battery, which includes a positive electrode, a negative electrode, a separator and the aqueous zinc ion battery electrolyte.
[0029] In some experimental methods of the present invention, the negative electrode includes a zinc sheet; the positive electrode includes a vanadium-based positive electrode material, for example, the positive electrode is a carbon cloth covered with a vanadium-based positive electrode material; and the separator includes glass fiber.
[0030] The vanadium-based positive electrode material may be at least one of vanadium dioxide, vanadium pentoxide or vanadium trioxide.
[0031] The present invention has the following beneficial effects:
[0032] The present invention prepares a self-adjusting pH value electrolyte as an electrolyte for an aqueous zinc ion battery by using a carboxylic acid derivative anhydride additive, which is beneficial to Zn 2+ Migration and accelerated reaction kinetics. In addition, carboxylic acid derivatives are compounds produced by replacing the hydroxyl group in the carboxylic acid molecule with other atoms or atomic groups such as halogens and amino groups, including acyl halides, anhydrides, esters, amides, etc. All four carboxylic acid derivatives can be hydrolyzed. Acyl halides and carboxylic acid derivative anhydrides are easy to hydrolyze, while the hydrolysis of esters and amides requires acid or base as a catalyst, and heating is also required. The hydrolysis of acyl halides will produce hydrogen halides (HCl, HF, HBr), all of which are strong acids. The hydrolysis of carboxylic acid derivative anhydrides will produce carboxylic acids.
[0033] When the carboxylic acid anhydride is hydrolyzed, part of it will destroy the Zn 2+ The solvated structure can also be adsorbed on the surface of the zinc negative electrode to induce uniform deposition of zinc; a part of it forms carboxylic acid in the zinc salt solution to regulate the local OH caused by the hydrogen evolution reaction. - The problem of pH increase caused by the increase in concentration is solved, thereby inhibiting the formation of the passivation layer and ensuring the active nucleation sites of Zn.
[0034] The modified electrolyte of the aqueous zinc ion battery provided by the invention has high specific capacity, good rate performance and cycle stability when used in the aqueous zinc ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The present invention is further described below with reference to the accompanying drawings and experimental examples, wherein:
[0036] Figure 1 The zinc batteries prepared in Experimental Examples 1-3 and Comparative Example 1 were -2 At a current density of 1 mAh cm -2SEM image of the zinc sheet surface after 200 cycles of charge and discharge at a fixed capacity;
[0037] Figure 2 Hydrogen evolution and Tafel curves measured for the electrolytic cells prepared in Experimental Examples 1-4 and Comparative Example 1;
[0038] Figure 3 The zinc battery prepared in Experimental Example 1 and Comparative Example 1 was tested at 4 mA cm -2 At a current density of 1 mAh cm -2 Long cycle data of charge and discharge of the capacity;
[0039] Figure 4 The zinc batteries prepared in Experimental Example 1 and Comparative Example 1 were subjected to different current densities (1, 2, 5, 8, 10, 12, 15 mA cm -2 ) at 1 mAh cm -2 The fixed capacity is used to perform charge and discharge rate data;
[0040] Figure 5 The zinc batteries prepared in Experimental Example 4 and Comparative Example 1 were subjected to different current densities (1, 2, 5, 8, 10, 12, 15 mA cm -2 ) at 1 mAh cm -2 The rate data of charging and discharging at a fixed capacity;
[0041] Figure 6 The full cells prepared in Experimental Example 1, Experimental Example 4 and Comparative Example 1 were 6Ag -1 The specific capacity data was measured at a current density of . DETAILED DESCRIPTION
[0043] The following will clearly and completely describe the concept of the present invention and the technical effects produced by the experimental examples, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the experimental examples described are only part of the experimental examples of the present invention, not all of the experimental examples. Based on the experimental examples of the present invention, other experimental examples obtained by technicians in this field without creative work are all within the scope of protection of the present invention.
[0044] As used herein, when used in connection with a numerical value, the term "about" is intended to include a set or range of numerical values. For example, "about" means a numerical range of ±10%, ±5%, ±2%, ±1%, ±0.5%, ±0.2% or ±0.1% of the numerical value. In one experimental scheme, the term "about" refers to a numerical range of 5% more or less than a specific value. In another experimental scheme, the term "about" refers to a numerical range of 2% more or less than a specific value. In another experimental scheme, the term "about" refers to a numerical range of 1% more or less than a specific value.
[0045] Unless otherwise specified, the test methods used in the experimental examples are all conventional methods; the materials and reagents used, unless otherwise specified, can be obtained from commercial sources. Unless otherwise specified, the same parameter in each experimental example has the same value. The experimental examples described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0046] Experimental Example 1
[0047] 1) Preparation of negative electrode materials
[0048] The zinc foil was cut into electrodes with a diameter of 12 mm using a slicer, and the electrodes were immersed in 1 mol / L dilute hydrochloric acid for ultrasonic cleaning for 1-2 seconds to remove the oxide film and impurities on the surface. The electrodes after ultrasonic cleaning were repeatedly cleaned with deionized water, dried in a natural environment, and used as negative electrodes for standby use.
[0049] 2) Preparation of succinic anhydride electrolyte
[0050] S1. At room temperature, 2 mol / L zinc sulfate was dissolved in 20 mL of deionized water, and the mixture was dispersed by stirring for 24 hours and ultrasonicated for 2 hours to obtain a uniform clear solution, i.e., a zinc sulfate aqueous solution.
[0051] S2. Add 0.04 mol / L succinic anhydride to the above-mentioned zinc sulfate aqueous solution, stir and disperse for 24 hours, and ultrasonicate for 2 hours to obtain a solution, that is, a succinic anhydride electrolyte.
[0052] 3) Battery assembly
[0053] For zinc batteries:
[0054] Use two identical zinc sheets as positive and negative electrodes. Place the gasket in the negative electrode shell, then place a cut zinc sheet on the gasket, put in a glass fiber diaphragm, use a pipette to drop 80uL of succinic anhydride electrolyte, and then place another zinc sheet on top of the diaphragm. Then put in a stainless steel gasket, then the spring, and finally buckle the positive electrode shell. Use a battery packaging machine to package the battery, and you will get an electrolyte-modified aqueous zinc ion symmetrical button battery, marked as GZn@GZn-50 symmetrical button battery.
[0055] Full Battery:
[0056] Use a zinc sheet as the negative electrode. Place a gasket in the negative electrode shell, then place a cut zinc sheet on the gasket, put in a glass fiber diaphragm, use a pipette to drop 80uL of succinic anhydride electrolyte, and then place a vanadium-based positive electrode material on top of the diaphragm. Then put in a stainless steel gasket, then a spring, and finally buckle the positive electrode shell. Use a battery packaging machine to package the battery, and you will get an aqueous zinc ion button battery modified with electrolyte, marked as GZn50@V button battery.
[0057] Experimental Example 2
[0058] Experimental Example 2 provides a method for preparing a succinic anhydride electrolyte. The raw materials and preparation method are the same as those in Experimental Example 1, except that the molar ratio of the added succinic anhydride to zinc sulfate is 1:10, and the obtained aqueous zinc ion symmetric button battery is marked as GZn@GZn-10 symmetric button battery.
[0059] Experimental Example 3
[0060] Experimental Example 3 provides a method for preparing a succinic anhydride electrolyte. The raw materials and preparation method are the same as those in Experimental Example 1, except that the molar ratio of the added succinic anhydride to zinc sulfate is 1:75, and the obtained aqueous zinc ion symmetric button battery is marked as GZn@GZn-75 symmetric button battery.
[0061] Experimental Example 4
[0062] Experimental Example 4 provides a method for preparing a maleic anhydride electrolyte. The raw materials and preparation method are the same as those of Experimental Example 1, except that the additive of the electrolyte is maleic anhydride, and the obtained aqueous zinc ion symmetric button battery is marked as SZn@SZn-50 symmetric button battery.
[0063] Comparative Example 1
[0064] 1) Preparation of negative electrode materials
[0065] The zinc foil was cut into electrodes with a diameter of 12 mm using a slicer, and the electrodes were immersed in 1 mol / L dilute hydrochloric acid for ultrasonic cleaning for 1-2 seconds to remove the oxide film and impurities on the surface. The electrodes after ultrasonic cleaning were repeatedly cleaned with deionized water, dried in a natural environment, and used as negative electrodes for standby use.
[0066] 2) Preparation of zinc sulfate electrolytic solution
[0067] At room temperature, 2 mol / L zinc sulfate was dissolved in 20 mL of deionized water, and the mixture was stirred and dispersed for 24 hours and ultrasonicated for 2 hours to obtain a uniform clear solution, that is, a zinc sulfate aqueous solution.
[0068] 2) Assemble the battery
[0069] For zinc batteries:
[0070] Use two identical zinc sheets as positive and negative electrodes. Place the gasket in the negative electrode shell, then place a cut zinc sheet on the gasket, put in a glass fiber diaphragm, use a pipette to drop 80uL of zinc sulfate electrolyte, and then place another zinc sheet on top of the diaphragm. Then put in a stainless steel gasket, then the spring, and finally buckle the positive electrode shell. Use a battery packaging machine to package the battery, and you will get an aqueous zinc ion symmetrical button battery, marked as a Zn@Zn symmetrical button battery.
[0071] Full Battery:
[0072] Use a zinc sheet as the negative electrode. Place a gasket in the negative electrode shell, then place a cut zinc sheet on the gasket, put in a glass fiber diaphragm, use a pipette to drop 80uL of zinc sulfate electrolyte, and then place a vanadium-based positive electrode material on top of the diaphragm. Then put in a stainless steel gasket, then a spring, and finally buckle the positive electrode shell. Use a battery packaging machine to package the battery, and you will get an aqueous zinc ion button battery, marked as a Zn@V button battery.
[0073] Performance Testing and Characterization
[0074] The aqueous zinc ion symmetric button cells assembled with the electrolytes prepared in the above experimental examples and comparative examples, the full cells composed of vanadium-based materials, and the electrolytic cells composed of the three-electrode method (working electrode: zinc sheet; reference electrode: silver chloride; counter electrode: carbon rod) were used for morphological characterization and electrochemical performance testing. The following performance tests and characterizations were all carried out at room temperature.
[0075] Figure 1 In the figure, (a) shows the appearance of the zinc sheet of the zinc battery prepared in comparative example 1 after 200 cycles of charge and discharge; (b) shows the appearance of the zinc sheet of the zinc battery prepared in experimental example 1 after 200 cycles of charge and discharge; (c) shows the appearance of the zinc sheet of the zinc battery prepared in experimental example 2 after 200 cycles of charge and discharge; (d) shows the appearance of the zinc sheet of the zinc battery prepared in experimental example 3 after 200 cycles of charge and discharge. Figure 1 It can be seen that the appearance of the zinc flakes in each experimental example is not much different, and compared with the comparative example 1 without additive modification, it can be found that the appearance of the zinc flakes in the experimental example is smoother. This shows that the zinc deposition in the experimental example is lateral growth, the deposition is more uniform, and the appearance is closer to the zinc flake before the cycle, which effectively inhibits the growth of zinc negative electrode dendrites.
[0076] Figure 2In the figure, (a) is the hydrogen evolution curve measured by the electrolytic cell prepared in Experimental Examples 1-4 and Comparative Example 1; (b) is the Tafel curve measured by the electrolytic cell prepared in Experimental Examples 1-4 and Comparative Example 1. As can be seen from Figure (a), Experimental Example 1 has a better ability to inhibit hydrogen production by corrosion of zinc sheets; as can be seen from Figure (b) and Table 1, the zinc sheet in Experimental Example 1 has the slowest corrosion rate, and the zinc sheet in Comparative Example 1 is most susceptible to corrosion. This shows that the anhydride additive of the present application not only induces uniform deposition of zinc after being adsorbed on the surface of the zinc negative electrode, but also isolates large-area contact with water, thereby inhibiting hydrogen production by corrosion.
[0077] Figure 3 The zinc battery prepared in Experimental Example 1 and Comparative Example 1 was tested at 4 mA cm -2 The current density is below 1 mAh cm -2 Long cycle data of charging and discharging the capacity of the battery. Figure 3 It can be found that the potential polarization of the zinc sheet in Experimental Example 1 is generally lower than that in Comparative Example 1, and relative to Comparative Example 1, the charge and discharge curve of Experimental Example 1 is stable without a chaotic curve, which proves that Experimental Example 1 has good cycle stability.
[0078] Figure 4 The zinc batteries prepared in Experimental Example 1 and Comparative Example 1 were subjected to different current densities (1, 2, 5, 8, 10, 12, 15 mA cm -2 ) at 1 mAh cm -2 The charge and discharge rate data at a fixed capacity. Figure 5 The zinc batteries prepared in Experimental Example 4 and Comparative Example 1 were subjected to different current densities (1, 2, 5, 8, 10, 12, 15 mA cm -2 ) at 1 mAh cm -2 The charge and discharge rate data of a fixed capacity. Figure 4-5 From Table 1, it can be found that the polarization potential of the modified electrolytes in Experimental Examples 1 and 4 is smaller than the polarization potential of the unmodified electrolyte in Comparative Example 1, and the nucleation overpotentials in Experimental Examples 1 and 4 are much smaller than the nucleation overpotential in Comparative Example 1, indicating that Experimental Examples 1 and 4 have better rate performance.
[0079] Figure 6 The full cells prepared in Experimental Example 1, Experimental Example 4 and Comparative Example 1 were -1 The specific capacity data is obtained under the following conditions. Figure 6 It can be found from Table 1 that the specific capacity of the full battery of Experimental Example 1 and Experimental Example 4 using the modified electrolyte is higher, and even after 350 cycles, the specific capacity is higher than that of Comparative Example 1 using the unmodified zinc sulfate electrolyte. It can be seen that the capacity retention rate of this experimental example has been improved, further verifying the modification effect of the anhydride additive.
[0080] Table 1 shows the relevant test data of long cycle, rate, capacity diagram and Tafel curve of the modified zinc sulfate electrolyte in Experimental Example 1 (succinic anhydride), Experimental Example 4 (maleic anhydride) and the blank zinc sulfate electrolyte in Comparative Example 1 under the assembly of zinc batteries, full batteries and electrolytic cells.
[0081] Table 1 Comparison of relevant properties in this experimental example and the comparative example
[0082]
[0083] From the comparison in the table, it can be found that the performance of Experimental Examples 1 and 4 is much better than the relevant performance of Comparative Example 1, among which the comprehensive performance of Experimental Example 1 is the best. By comparing Experimental Example 1, Experimental Example 4 and Comparative Example 1, it can be proved that the anhydride additives do have a good inhibitory effect on the dendrite growth, hydrogen evolution corrosion, and the formation of by-products of the zinc negative electrode. The aqueous zinc ion battery obtained by adding anhydride additives in this experimental example has a high specific capacity, good rate performance and cycle stability.
[0084] Obviously, the above experimental examples of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the experimental methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is not necessary and impossible to list all experimental methods here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. An aqueous zinc ion battery electrolyte, characterized in that The electrolyte includes an additive, and the additive includes an acid anhydride.
2. The aqueous zinc ion battery electrolyte according to claim 1, characterized in that The acid anhydride includes at least one of acetic anhydride, propionic anhydride, succinic anhydride, maleic anhydride, benzoic anhydride and phthalic anhydride.
3. The aqueous zinc ion battery electrolyte according to claim 1, characterized in that The electrolyte also includes a zinc salt and a solvent.
4. The aqueous zinc ion battery electrolyte according to claim 3, characterized in that The zinc salt includes zinc sulfate and / or zinc trifluoromethanesulfonate; and / or, the solvent includes water.
5. The aqueous zinc ion battery electrolyte according to claim 3 or 4, characterized in that In the electrolyte, the molar ratio of the acid anhydride to the zinc salt is 1:(10-100); and / or the concentration of the zinc salt is 1-3 mol / L.
6. The aqueous zinc ion battery electrolyte according to claim 5, characterized in that The molar ratio of the anhydride to the zinc salt is 1:(25-75).
7. A method for preparing an aqueous zinc ion battery electrolyte, characterized in that: The following steps are involved: The aqueous zinc ion battery electrolyte is obtained by mixing the zinc salt, the acid anhydride and the solvent and dispersing and dissolving them.
8. The preparation method according to claim 7, characterized in that: The operating temperature is 10° C.-40° C.; and / or, the dispersing and dissolving step comprises stirring dispersion and ultrasound, wherein the stirring time is 24-48 hours, and the ultrasound time is 1-3 hours.
9. An aqueous zinc ion battery, characterized in that: The invention comprises the aqueous zinc ion battery electrolyte described in any one of claims 1 to 6 or the aqueous zinc ion battery electrolyte prepared by the preparation method described in any one of claims 7 to 8.
10. The aqueous zinc ion battery according to claim 9, characterized in that: The aqueous zinc ion battery further comprises a positive electrode, a negative electrode and a diaphragm; the negative electrode comprises a zinc sheet; the positive electrode comprises a vanadium-based positive electrode material; and the diaphragm comprises glass fiber.