Bio-based diaphragm slurry, lithium battery diaphragm and lithium battery thereof

By using bio-based separator slurry and high specific surface area inorganic ceramic particles, combined with binders and crosslinkers with high glass transition temperature, a high heat resistance coating is formed, and the liquid absorption and liquid retention performance of lithium battery separator is solved. The problem of insufficient thermal properties improves the circulation and safety performance of the battery.

CN118888974AInactive Publication Date: 2024-11-01ANHUI LIKE NEW MATERIAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410909473.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium battery separators have shortcomings in improving liquid-absorbing and liquid retention and heat resistance, which affects the high performance and safety performance of the battery.

Method used

Using bio-based separator slurry, including bio-based particles, inorganic ceramic particles, binders and crosslinkers, a high heat-resistant coating is formed through specific slurry and coating processes, to improve the liquid absorption and retention rate of the separator and Ion conductivity.

Benefits of technology

It significantly improves the circulation and power performance of lithium-ion batteries, improves the thermal runaway safety performance of the battery, and improves the overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888974A_ABST
    Figure CN118888974A_ABST
Patent Text Reader

Abstract

The invention discloses bio-based diaphragm slurry, a lithium battery diaphragm and a lithium battery thereof. The bio-based diaphragm slurry comprises the following components in parts by mass: 1-10 parts of bio-based particles; 20-40 parts by mass of inorganic ceramic particles; 5-10 parts by mass of a binder; 0.1 to 0.5 part by mass of a cross-linking agent; and 50-70 parts by mass of a solvent. According to the diaphragm slurry provided by the invention, the bio-based high-heat-resistance nano-particles with a bio-based functional group furan ring structure are used, and the bio-based high-heat-resistance nano-particles have a conjugated pi electron system structure and can have relatively good affinity with an electrolyte in a battery, and meanwhile, a high-specific-surface type is selected; the nano inorganic particles with better liquid absorption and retention capabilities are uniformly mixed to form a compact coating, gaps of the inorganic particles can be better filled with the bio-based heat-resistant nano particles, and a better heat-resistant structural layer is jointly formed by using a binder with higher glass transition temperature; and meanwhile, a slurry mixing and coating process is matched, so that the formed coating structure has better strength under the function of the cross-linking agent, and the diaphragm has higher heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a bio-based diaphragm slurry, a lithium battery diaphragm and a lithium battery thereof. Background Art

[0002] In recent years, with the large-scale application of lithium-ion batteries, fast charging, long cycle life and high safety performance have gradually become the performance demand trend of the lithium battery market. As an important component in battery design, the diaphragm has a very important impact on the performance of the battery, and the performance requirements of the diaphragm are gradually increasing.

[0003] In the current battery design, polyolefin materials with low cost and mature technology are mostly used as the base membrane, and functional coating design is used to further improve the performance of the diaphragm. However, this will increase the impedance of the diaphragm, reduce the ionic conductivity, and make the diaphragm's liquid absorption and retention performance and heat resistance performance not greatly improved, thus affecting the high performance of the battery. Summary of the invention

[0004] To this end, the present invention provides a bio-based diaphragm slurry, a lithium battery diaphragm and a lithium battery thereof. The diaphragm slurry has simple slurry mixing and coating processes, the diaphragm has a high liquid absorption and retention rate and ionic conductivity, the diaphragm has good high-temperature heat resistance and a high membrane rupture temperature, which can effectively improve the battery cycle and power performance, improve the battery thermal runaway and other safety performance, and greatly improve the comprehensive performance of lithium-ion batteries.

[0005] The invention protects a bio-based diaphragm slurry, which comprises: 1-10 parts by mass of bio-based particles; 20-40 parts by mass of inorganic ceramic particles; 5-10 parts by mass of a binder; 0.1-0.5 parts by mass of a cross-linking agent; and 50-70 parts by mass of a solvent.

[0006] Preferably, the bio-based particles include one or more of furan-based polyamide, furan-based polyimide, and furan polyester, with a particle size range of 0.01-0.1 μm and a thermal decomposition temperature of >400°C.

[0007] Preferably, the inorganic ceramic particles are one or more of alumina, boehmite, silicon dioxide, magnesium oxide, lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide, and lithium lanthanum titanium oxide; the particle size range is 0.1-1 μm, and the specific surface area is >10 m 2 / g.

[0008] Preferably, the adhesive is one or more of polyimide, polyamide, polyacrylate, and polyacrylic acid, and has a glass transition temperature greater than 180° C.; and the solvent is deionized water.

[0009] Preferably, the cross-linking agent is aziridine-modified isocyanate.

[0010] Preferably, the slurry further comprises: 2-5 parts by mass of a dispersant; and 0.1-0.5 parts by mass of a wetting agent.

[0011] Preferably, the dispersant is one or more of polyester ammonium salts, quaternary ammonium salts, polyurethanes, and polyesters; the wetting agent is one or more of polyethers, fatty alcohols, and fatty acid esters.

[0012] The present invention also protects a lithium battery separator, which is obtained by coating the above-mentioned bio-based separator slurry on at least one side of the base film and then drying it. The coating process is a uniform coating process such as gravure roller coating and extrusion, and the thickness of the coating is ≤2μm.

[0013] The present invention also protects a lithium battery, comprising: a positive electrode, a negative electrode and a battery separator, wherein the battery separator adopts the above-mentioned separator.

[0014] The diaphragm slurry proposed in the present invention uses bio-based high heat-resistant nanoparticles with a furan ring structure with a bio-based functional group, has a structure of a conjugated π electron system, and can have good affinity with the electrolyte in the battery. At the same time, high specific surface area type and nano inorganic particles with better liquid absorption and retention capabilities are selected and evenly mixed with each other to form a dense coating. The bio-based heat-resistant nanoparticles can better fill the gaps between the inorganic particles, and a binder with a higher glass transition temperature is used to form a better heat-resistant structural layer together; at the same time, the slurry coating process is matched, and the formed coating structure has better strength under the function of the cross-linking agent, and the diaphragm has higher heat resistance. The battery using this functional diaphragm can effectively improve the battery cycle and power performance, improve the safety performance of the battery such as thermal runaway, and greatly improve the comprehensive performance of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a schematic diagram of the internal structure of the bio-based diaphragm obtained in Example 1;

[0016] Figure 2 This is the SEM image of the bio-based diaphragm prepared in Example 1. DETAILED DESCRIPTION

[0017] In order to facilitate the understanding of the present invention, a more comprehensive description will be given below in conjunction with specific embodiments and accompanying drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The technical scheme of the present invention is described more clearly and completely below in conjunction with specific embodiments and comparative examples.

[0019] Example 1

[0020] 1. Select furan-based polyamide particles with a particle size of 0.05 μm, alumina ceramic powder with a particle size of 0.1 μm and a specific surface area of ​​12, polyester ammonium salt dispersant and deionized water, and use a high-speed disperser with a rotation of 2000 rpm and a revolution of 20 rpm to stir for 30 minutes to form a primary mixture in a mass ratio of 5%: 30%: 2%: 55%;

[0021] 2. Use a sand mill to fully mix the slurry. The sand mill is 600rpm and sand mills for 3 weeks to form a slurry;

[0022] 3. Select polyether wetting agent, polyimide binder, and aziridine modified isocyanate cross-linking agent, add them into the slurry in the mass ratio of 0.5%:7%:0.5%, use a disperser to rotate at 400 rpm and revolve at 20 rpm, and stir for 30 minutes to obtain the finished slurry.

[0023] A 9 μm PE base film was selected and coated with a 1 μm coating on both sides using a gravure roller coating process to obtain a coated diaphragm. Figure 1 As shown, its SEM image is as follows Figure 2 shown.

[0024] Comparative Example 1

[0025] 1. Select alumina ceramic powder with a particle size of 0.1μm and a specific surface area of ​​12, polyester ammonium salt dispersant and deionized water in a mass ratio of 35%:2%:55%, use a high-speed disperser with a rotation of 2000rpm and a revolution of 20rpm, and stir for 30 minutes to form a primary mixture;

[0026] 2. Use a sand mill to fully mix the slurry. The sand mill is 600rpm and sand mills for 3 weeks to form a slurry;

[0027] 3. Select polyether wetting agent, polyimide binder, and aziridine modified isocyanate cross-linking agent, add them into the slurry in the mass ratio of 0.5%:7%:0.5%, use a disperser to rotate at 400 rpm and revolve at 20 rpm, and stir for 30 minutes to obtain the finished slurry.

[0028] A 9 μm PE base film was selected and coated with a 1 μm coating on both sides using a gravure roller coating process to obtain a coated diaphragm.

[0029] The difference between this comparative example and Example 1 is that no bio-based particles are added to the initial mixture.

[0030] The same battery cell materials and manufacturing process were selected to manufacture the separators in Example 1 and Comparative Example 1 into 55Ah square wound lithium iron phosphate batteries, and the battery performance was tested.

[0031] Example 2

[0032] 1. Select furan polyester particles with a particle size of 0.1 μm, lithium aluminum titanium phosphate ceramic powder with a particle size of 0.8 μm and a specific surface area of ​​15, polyurethane dispersant and deionized water in a mass ratio of 6%: 35%: 3%: 50%. Use a high-speed disperser to rotate at 2500 rpm and revolve at 30 rpm, and stir for 30 minutes to form a primary mixture;

[0033] 2. Use a sand mill to fully mix the slurry. The sand mill is 550rpm and sand mills for 4 cycles to form a slurry;

[0034] 3. Select fatty alcohol wetting agent, polyamide binder, and aziridine modified isocyanate crosslinking agent, and add them into the slurry in a mass ratio of 0.5%:5%:0.5%. Use a disperser to rotate at 350 rpm and revolve at 30 rpm, and stir for 30 minutes to obtain the finished slurry.

[0035] A 12 μm PE base film was selected and coated with a 2 μm coating on one side using a gravure roller coating process to obtain a coated diaphragm.

[0036] Comparative Example 2

[0037] 1. Select lithium aluminum titanium phosphate ceramic powder with a particle size of 0.8 μm and a specific surface area of ​​15, a polyurethane dispersant and deionized water in a mass ratio of 41%:3%:50% using a high-speed disperser with a rotation of 2500 rpm and a revolution of 30 rpm, and stir for 30 minutes to form a primary mixture;

[0038] 2. Use a sand mill to fully mix the slurry. The sand mill is 550rpm and sand mills for 4 cycles to form a slurry;

[0039] 3. Select fatty alcohol wetting agent and polyamide binder, add them into the slurry in the mass ratio of 1%:5%, use a disperser to rotate at 350rpm and revolve at 30rpm, stir for 30 minutes to obtain the finished slurry.

[0040] A 12 μm PE base film was selected and coated with a 2 μm coating on one side using a gravure roller coating process to obtain a coated diaphragm.

[0041] The same battery cell materials and manufacturing process were selected to manufacture the separators in Example 2 and Comparative Example 2 into nickel-cobalt-manganese ternary system 50Ah square wound batteries, and the battery performance was tested.

[0042] Example 3

[0043] 1. Select furanyl polyimide particles with a particle size of 0.06 μm, boehmite ceramic powder with a particle size of 0.4 μm and a specific surface area of ​​13, quaternary ammonium salt dispersant and deionized water in a mass ratio of 4%:28%:2%:60% using a high-speed disperser with a rotation of 1800 rpm and a revolution of 25 rpm, and stir for 30 minutes to form a primary mixture;

[0044] 2. Use a sand mill to fully mix the slurry. The sand mill is 500 rpm. Sand mill for 2 weeks to form a slurry;

[0045] 3. Select fatty acid ester wetting agent, polyacrylic acid binder, and aziridine modified isocyanate crosslinking agent, and add them into the slurry in a mass ratio of 0.2%:5.5%:0.3%. Use a disperser with a rotation of 300 rpm and a revolution of 25 rpm, and stir for 30 minutes to obtain the finished slurry.

[0046] A 7 μm PE base film was selected and coated with a 2 μm coating on one side using a gravure roller coating process to obtain a coated diaphragm.

[0047] Comparative Example 3

[0048] 1. Select boehmite ceramic powder with a particle size of 0.4 μm and a specific surface area of ​​13, a quaternary ammonium salt dispersant and deionized water in a mass ratio of 32%: 2%: 60%, use a high-speed disperser with a rotation of 1800 rpm and a revolution of 25 rpm, and stir for 30 minutes to form a primary mixture;

[0049] 2. Use a sand mill to fully mix the slurry. The sand mill is 500 rpm. Sand mill for 2 weeks to form a slurry;

[0050] 3. Select fatty acid ester wetting agent and polyacrylic acid binder, add them into the slurry in the mass ratio of 0.5%:5.5%, use a disperser to rotate at 300 rpm and revolve at 25 rpm, stir for 30 minutes to obtain the finished slurry.

[0051] A 7 μm PE base film was selected and coated with a 2 μm coating on one side using a gravure roller coating process to obtain a coated diaphragm.

[0052] The same battery cell materials and manufacturing process were selected to manufacture the separators in Example 1 and Comparative Example 1 into 15Ah cylindrical wound batteries of lithium iron phosphate system, and the battery performance was tested.

[0053] The diaphragms prepared in Examples 1-3 and Comparative Examples 1-3 were tested for liquid absorption rate, liquid retention rate, ionic conductivity, thermal shrinkage rate at 150°C for 1h, and membrane rupture temperature performance according to the following test conditions, and the prepared batteries were tested for internal resistance, discharge capacity ratio at 3C rate current, 45°C 0.5C cycle capacity retention rate, and thermal runaway performance according to the following test conditions.

[0054] 1. Liquid absorption rate and liquid retention rate test

[0055] The test diaphragm was cut into 3 pieces of 100mm*100mm each, weighed and marked as m1 respectively, and the diaphragm was clamped with two layers of dust-free cloth and rolled into a barrel shape, tied with a rope, and immersed in a plastic beaker filled with electrolyte for 1 hour; the electrolyte type was 1.0 mol / L lithium hexafluorophosphate, and the volume of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate was 1:1:1.

[0056] Take the diaphragm out of the beaker, quickly wipe the electrolyte on the surface of the diaphragm with absorbent paper, weigh it and record it as m2, put the wiped diaphragm in a fume hood for 1 hour, weigh it and record it as m3, the liquid absorption rate is calculated according to the formula (m2-m1) / m1*100%, and the liquid retention rate is calculated according to the formula (m3-m1) / m1*100%. Take the average of the three test results as the test value of liquid absorption rate and liquid retention rate.

[0057] 2. Ionic conductivity test

[0058] Cut the diaphragm and put it into an electrolyte with a volume ratio of 1:1:1 of 1.0 mol / L lithium hexafluorophosphate, ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate, and keep it sealed and soaked for 2 hours. Inject the electrolyte into the resistance test mold, first put in 1 layer of diaphragm, test its AC impedance resistance, then put in 1 layer, test its AC impedance resistance, until 4 layers are put in, and measure four AC impedance resistance values ​​respectively.

[0059] During the test, it is necessary to ensure that the electrolyte in the resistance test mold can completely immerse the placed diaphragm. Draw a curve with the number of diaphragm layers as the horizontal coordinate and the resistance as the vertical coordinate, and find the slope and linear fit of the curve. When the linear fit is greater than 0.99, the ionic conductivity is calculated according to the formula R=k*1 and σ=d / R*S. When the linear fit is less than 0.99, retesting is required. In the formula, R is the resistance of one layer of diaphragm (in ohms), k is the slope of the curve when the fit is greater than 0.99, σ is the ionic conductivity (in Siemens per centimeter), d is the thickness of one layer of diaphragm (in micrometers), and S is the diaphragm test area (in square centimeters).

[0060] 3. Thermal Shrinkage Test

[0061] Cut the test diaphragm into 3 pieces of 100mm*100mm, measure the longitudinal and transverse lengths of each diaphragm, and use a forced air thermostat with an accuracy of ±1℃. Place the stainless steel plate and two quantitative filter papers in the middle of the oven, put the diaphragm between the two filter papers, close the thermostat door and keep it at 150℃ for 1h.

[0062] After heating, take out the diaphragm, wait for the diaphragm to return to room temperature, measure the longitudinal and transverse lengths again, and calculate the shrinkage rate according to the formula ΔL = (L0-L1) / L0*100%. The average of the three test results is the thermal shrinkage rate of the diaphragm. In the formula, ΔL is the thermal shrinkage rate (unit %), L0 is the length before heating (unit millimeter), and L1 is the length after heating (unit millimeter).

[0063] 4. Film rupture temperature test

[0064] The diaphragm was cut into strips with a length of 30 cm and a width of 2 cm. A thermal mechanical analyzer was used to test the diaphragm at a tensile force of 0.03 N and a heating rate of 5°C / min from room temperature until the diaphragm broke. The diaphragm rupture temperature was recorded as the membrane rupture temperature.

[0065] 5. Internal resistance test

[0066] Use a resistance tester to test the trial-produced batteries after capacity division and record the internal resistance of the batteries.

[0067] 6. Discharge capacity ratio test at 3C rate current

[0068] At room temperature, use a 1C rate to charge at constant current to the termination voltage, then switch to constant voltage charging. Stop charging when the charging current drops to 0.05C. Then discharge at a 3C rate to the cut-off voltage. The discharge capacity ratio is calculated as the tested discharge capacity / initial capacity*100%.

[0069] The charge and discharge cut-off voltages of the diaphragm batteries of Examples 1 and 3 and Comparative Examples 1 and 3 are 3.65V and 3.2V, respectively. The charge and discharge cut-off voltages of the diaphragm batteries of Example 1 and Comparative Example 2 are 4.2V and 3.6V.

[0070] 7. 45℃0.5C cycle capacity retention test

[0071] The battery was placed in a 45°C constant temperature box, charged at a constant current rate of 1C to the termination voltage, then switched to constant voltage charging, and charging was stopped when the charging current dropped to 0.05C. After leaving it for 30 minutes, it was discharged at a current rate of 0.5C. After leaving it for 30 minutes, it was charged again according to the above method, and then it was discharged at a current rate of 0.5C after leaving it for another 30 minutes. The above charge and discharge method was used for continuous cycle 500 times, and the capacity retention rate was calculated by testing the battery discharge capacity / initial capacity*100%.

[0072] The charge and discharge cut-off voltages of the diaphragm batteries of Examples 1 and 3 and Comparative Examples 1 and 3 are 3.65V and 3.2V, respectively. The charge and discharge cut-off voltages of the diaphragm batteries of Example 1 and Comparative Example 2 are 4.2V and 3.6V.

[0073] 8. Thermal runaway test

[0074] The battery was tested by step-by-step temperature increase starting from 50°C using an adiabatic accelerating calorimeter. After each temperature increase of 3°C, the battery was left to stand for observation for 1 hour and then continued to be heated to 300°C. At the end of the test, the battery status was recorded.

[0075] The test data is shown in Table 1 below. The test results show that the separators in Examples 1-3 all have relatively high liquid absorption rate, liquid retention rate, ionic conductivity and high temperature resistance. The separators in Comparative Examples 1-3 are conventional process separators with slightly poor comprehensive performance. The trial-produced batteries in Examples 1-3 have lower internal resistance and better high-rate discharge performance. At the same time, the batteries have better cycle life and higher thermal stability and safety performance, and the comprehensive performance of the batteries is good.

[0076] Table 1 Test results of separator and battery performance

[0077]

[0078]

[0079] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0080] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A bio-based diaphragm slurry, characterized in that: include: 1-10 parts by mass of bio-based particles; 20-40 parts by mass of inorganic ceramic particles; 5-10 parts by mass of a binder; 0.1-0.5 parts by mass of a cross-linking agent; 50-70 parts by mass of solvent.

2. The bio-based diaphragm slurry according to claim 1, characterized in that: The bio-based particles include one or more of furan-based polyamide, furan-based polyimide, and furan polyester, with a particle size range of 0.01-0.1 μm and a thermal decomposition temperature of more than 400° C.

3. The bio-based diaphragm slurry according to claim 1, characterized in that: The inorganic ceramic particles are one or more of alumina, boehmite, silicon dioxide, magnesium oxide, lithium aluminum titanium phosphate, lithium lanthanum zirconium oxide, and lithium lanthanum titanium oxide; the particle size range is 0.1-1 μm, and the specific surface area is >10 m 2 / g.

4. The bio-based diaphragm slurry according to claim 1, characterized in that: The adhesive is one or more of polyimide, polyamide, polyacrylate and polyacrylic acid, and the glass transition temperature is greater than 180° C.; the solvent is deionized water.

5. The bio-based diaphragm slurry according to claim 1, characterized in that: The cross-linking agent is aziridine modified isocyanate.

6. The bio-based diaphragm slurry according to claim 1, characterized in that: The slurry further comprises: 2-5 parts by mass of a dispersant; and 0.1-0.5 parts by mass of a wetting agent.

7. The bio-based diaphragm slurry according to claim 1, characterized in that: The dispersant is one or more of polyester ammonium salts, quaternary ammonium salts, polyurethanes, and polyesters; the wetting agent is one or more of polyethers, fatty alcohols, and fatty acid esters.

8. A lithium battery separator, characterized in that: The bio-based diaphragm slurry according to any one of claims 1 to 7 is applied to at least one side of a base film and then dried to obtain the diaphragm.

9. The lithium battery separator according to claim 8, characterized in that: The coating process is gravure roller coating or extrusion coating, and the coating thickness after coating is ≤2 μm.

10. A lithium battery, characterized in that: include: A positive electrode, a negative electrode and a battery separator, wherein the battery separator is the separator described in claim 8 or 9.

Citation Information

Patent Citations

  • Ceramic diaphragm for lithium ion battery and preparation method of ceramic diaphragm

    CN105514328A

  • Battery diaphragm coated with high-temperature resistant coating and preparation method thereof

    CN107895766A

  • High-temperature-resistant heat-shrinkable lithium battery diaphragm and preparation method thereof

    CN110993866A

  • Preparation and application of water-based coating slurry for improving diaphragm rupture temperature

    CN116387751A

  • Preparation method for coating bio-based furan polyamide film on lithium ion battery diaphragm

    CN117438738A

Cited By

  • Furyl polyamide lithium battery diaphragm and preparation method thereof

    CN120127335A