High-wettability composite diaphragm as well as preparation method and application thereof
By using a multifunctional coating of ordered mesoporous carbon, nanocellulose and ceramic powder in the lithium-ion battery separator, combined with ultra-high molecular weight polyethylene single-layer porous PE wet separator, the separator is solved in the high temperature environment. The problem of insufficient heat resistance and electrolyte wetting properties has achieved higher electrolyte utilization and heat shrinkage resistance, extending the service life of the battery and improving safety.
Patent Information
- Application Number
- CN202410960392.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium-ion battery separators have insufficient heat resistance and electrolyte wetting properties in high temperature environments, resulting in uneven battery current density and obvious temperature increase, which affects service life and safety.
Using a multifunctional coating layer composed of ordered mesoporous carbon, nanocellulose and ceramic powder, combined with ultra-high molecular weight polyethylene single-layer porous PE wet membrane, improves the wettability of the electrolyte through coating and hot pressing composite technology It also improves heat shrinkage resistance.
It significantly improves the electrolyte wetting and liquid retention rate of the lithium-ion battery separator during service, extends the battery's cycle life, reduces the risk of lithium-ion cell separation, and improves the battery's service life and safety.
Smart Images

Figure CN118888975A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium battery separators, and in particular relates to a high-wettability composite separator and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Compared with traditional secondary batteries, lithium-ion batteries have the advantages of high energy density, environmental friendliness, and long service life. They are currently widely used in digital electronic products, new energy vehicles, and energy storage. Lithium-ion batteries are mainly composed of positive electrode materials, negative electrode materials, separators, and electrolytes. Among them, the separator, as one of the four main materials of lithium-ion batteries, plays a role in isolating the short circuit between the positive and negative electrodes. At the same time, its microporous structure provides an effective channel for ions to form a complete charge and discharge circuit. The separators currently used in commercial applications are mainly made of PE and PP materials, and are coated with ceramic materials or high-temperature resistant organic materials to improve the high-temperature resistance and liquid retention performance of the separator substrate. However, the interface performance between the ceramic coating and the pole piece is poor, and when the pole piece and the separator are tightly attached, the electrolyte loss in the center of the battery is difficult to quickly infiltrate and replenish, resulting in local lithium precipitation, uneven battery current density, and significant temperature rise, which ultimately affects the service life and safety of the battery.
[0004] At present, modified diaphragm substrates are usually used to improve the wettability between the diaphragm and the electrolyte. For example, patent CN113725557A discloses a lithium-ion battery diaphragm support layer and a lithium-ion battery diaphragm, which ensure the heat resistance and tensile strength of the composite diaphragm by using organic fibers and inorganic fibers in combination. However, the thickness of the composite diaphragm material is relatively large, which is not conducive to the improvement of the energy density of the lithium-ion battery, and the pore size of the composite diaphragm is relatively large, and the self-discharge performance of the lithium-ion battery cannot be guaranteed. Patent CN114665227A discloses a highly wettable lithium-ion battery diaphragm and a preparation method thereof, which co-extrudes ethylene-vinyl acetate copolymer, polyolefin material and a compatibilizer to obtain a highly wettable diaphragm. However, since it is a multi-phase blended crystallization film, the heat resistance and mechanical strength will be affected to a certain extent.
[0005] Therefore, developing and designing a new type of highly electrolyte-wettable diaphragm is very important to improve the processing performance and performance of the battery. Summary of the invention
[0006] In order to address the deficiencies in the prior art, the purpose of the present invention is to provide a highly wettable composite diaphragm and a preparation method and application thereof. The present invention utilizes ordered mesoporous carbon, nanocellulose and ceramic powder to synergistically form a multifunctional coating layer, thereby improving the electrolyte wettability and liquid retention rate of the composite diaphragm during service, while also improving the heat shrinkage resistance to a certain extent.
[0007] In order to achieve the above object, the technical solution of the present invention is:
[0008] The first aspect of the present invention provides a high-wettability composite diaphragm, comprising a diaphragm substrate and a coating layer; the high-wettability composite diaphragm is a sandwich structure, and the coating layer is located between the diaphragm substrate;
[0009] The membrane substrate is a single-layer porous PE wet-process membrane, and the coating layer comprises ordered mesoporous carbon, polymethyl methacrylate microspheres, nanocellulose and ceramic powder.
[0010] In some embodiments of the present invention, the mass ratio of the ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder and nanocellulose is (1-10):(5-50):(100-300):(1-10).
[0011] In some embodiments of the present invention, the thickness of the diaphragm substrate is 3-10 μm, and the thickness of the coating layer is 0.5-5 μm.
[0012] The second aspect of the present invention provides a method for preparing the highly wettable composite membrane, comprising the following steps:
[0013] The ultra-high molecular weight polyethylene and paraffin oil are melt-blended and extruded into a sheet, cooled and shaped, pores are formed, and stretched and shaped to obtain a diaphragm substrate;
[0014] Ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder and nanocellulose are mixed, water is added, stirred, and a stabilizer solution is added to obtain a coating slurry;
[0015] The coating slurry is coated on one side of the diaphragm substrate and dried, and the coated diaphragm substrate and the uncoated diaphragm substrate are hot-pressed and composited, with the coating slurry located between the diaphragm substrates, to obtain a highly wettable composite diaphragm.
[0016] In some embodiments of the present invention, the molecular weight of the ultra-high molecular weight polyethylene is 500,000-1.5 million, preferably 1 million.
[0017] In some embodiments of the present invention, the mass ratio of ultra-high molecular weight polyethylene to paraffin oil is (1-5):(5-10), preferably 3:7.
[0018] In some embodiments of the present invention, the pore-forming is performed by extraction with dichloromethane.
[0019] In some embodiments of the present invention, the thickness of the diaphragm substrate is controlled to be 3-10 μm.
[0020] In some embodiments of the present invention, the particle size of the polymethyl methacrylate (PMMA) microspheres is 0.5-5 μm, preferably 2 μm. The PMMA microspheres are used as glue points to bond two diaphragm substrates into a whole to obtain a composite diaphragm.
[0021] In some embodiments of the present invention, the particle size of the ceramic powder is 0.3-0.6 μm, preferably 0.4 μm, and the ceramic powder includes but is not limited to boehmite powder.
[0022] In some embodiments of the present invention, the mass ratio of the ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder, nanocellulose and water is (1-10):(5-50):(100-300):(1-10):(300-800).
[0023] In some embodiments of the present invention, the stabilizer comprises sodium carboxymethylcellulose (CMC);
[0024] In the stabilizer solution, the mass ratio of stabilizer to water is (1-10):100, preferably 5:100.
[0025] CMC is dissolved in water and stirred to obtain a colloid, which is added to the slurry as a thickener or stabilizer to improve the stability of the slurry.
[0026] In some embodiments of the present invention, the mass ratio of the stabilizer to the ceramic powder is (0.5-1.5):(10-30), preferably 1:20.
[0027] In some embodiments of the present invention, during the preparation of the coating slurry, a stabilizer is mixed with water and stirred to obtain a stabilizer solution; ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder and nanocellulose are mixed, water and a dispersant are added, and after stirring, the stabilizer solution is added, and after stirring again, a binder and a surfactant are added, and stirred to obtain a coating slurry.
[0028] Preferably, in the process of preparing the coating slurry, the stabilizer is mixed with water, and a high-speed stirrer is used to mix and stir to obtain a stabilizer solution, and the stirring time is 30 to 90 minutes; the ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder and nanocellulose are dry-blended and mixed for 30 to 60 minutes; water and dispersant are added, and the resulting slurry is stirred for 60 to 240 minutes using a planetary stirrer; the stabilizer solution is added and stirred for 15-60 minutes; then a polyacrylate binder and a surfactant are added and stirred for 30 to 60 minutes to obtain a coating slurry.
[0029] In some embodiments of the present invention, the dispersant includes but is not limited to ammonium polyacrylate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium hexametaphosphate or octylphenol polyoxyethylene ether.
[0030] In some embodiments of the present invention, the adhesive is a polyacrylate adhesive.
[0031] In some embodiments of the present invention, the surfactant includes but is not limited to at least one of a silane coupling agent, an alkylphenol polyoxyethylene ether, a fatty alcohol polyoxyethylene ether, a fatty acid polyoxyethylene ether and a polyether-modified polysiloxane.
[0032] In some embodiments of the present invention, the mass ratio of the ceramic powder, surfactant, binder and dispersant is (100-1600):(0.01-0.1):(10-80):(0.5-5).
[0033] In some embodiments of the present invention, a micro-gravure roller is used to coat one side of the diaphragm substrate, and the coating thickness is controlled between 0.5 and 5 μm. After coating, an oven may be used for drying.
[0034] In some embodiments of the present invention, the drying temperature is 50-90°C.
[0035] In some embodiments of the present invention, the hot pressing compounding has a hot pressing temperature of 60 to 110° C. and a hot pressing pressure of 0.1 to 5 MPa.
[0036] The third aspect of the present invention provides a use of the highly wettable composite separator in a battery.
[0037] A fourth aspect of the present invention provides a lithium battery, wherein the separator of the lithium battery adopts the highly wettable composite separator.
[0038] The beneficial effects of the present invention are:
[0039] The present invention provides a highly wettable composite diaphragm. The present invention first uses PE particles and paraffin oil to blend and extrude casting sheets, then uses dichloromethane to extract and form pores, and finally stretches and shapes to obtain a single-layer porous PE wet-process diaphragm (i.e., the diaphragm substrate). Ordered mesoporous carbon, nanocellulose and small-particle ceramic particles are used for blending and coating. Then, it is thermally compounded with the diaphragm substrate after pore formation to form a highly wettable composite diaphragm material. Among them, the accumulation of small-particle ceramic materials plays a heat-resistant role, the porous structure on the ordered mesoporous carbon is conducive to the storage of electrolyte and plays a liquid retention role, and the nanocellulose has rich hydroxyl groups, which is conducive to the diffusion and infiltration of the electrolyte, and plays an accelerated transmission and infiltration effect. The three work synergistically to form a multifunctional coating layer, and a highly wettable diaphragm material is obtained by coating and hot pressing compounding, thereby improving the electrolyte wettability and liquid retention rate of the diaphragm during service, and its heat shrinkage resistance is also improved to a certain extent. On the one hand, during the battery assembly process, the diaphragm substrate absorbs the electrolyte to the intermediate coating to retain the liquid. Because the PE base film has small pores and the inorganic particle gaps are large, most of the electrolyte will be retained in the intermediate coating, and the electrolyte is stored between the positive and negative electrodes, which improves the utilization rate of the electrolyte. On the other hand, ordinary commercial diaphragms coated with ceramic on one side are prone to curling and shrinking toward the base film surface, while ordinary commercial diaphragms coated with ceramic on both sides have poor interface performance with the electrode, which easily leads to the problem of short cycle life. The high-wettability composite diaphragm provided by the present invention does not have the difference between the AB surface, and the synergistic use of nanocellulose and ceramics plays a skeleton support role, which improves its resistance to heat shrinkage. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0041] Figure 1 This is a structural diagram of the highly wettable composite diaphragm obtained in Examples 1 and 2 of the present invention, wherein: 1-diaphragm substrate, 2-ordered mesoporous carbon, 3-PMMA microspheres, 4-nanocellulose, and 5-ceramic particles. DETAILED DESCRIPTION
[0042] The present invention provides a high-wettability composite diaphragm and a preparation method and application thereof, for solving
[0043] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0044] Unless otherwise specified, the reagents or raw materials used in the following examples and comparative examples are all conventional commercially available products and can be purchased.
[0045] Example 1
[0046] A method for preparing a highly wettable composite diaphragm comprises the following steps:
[0047] 1. Preparation of diaphragm substrate: Ultra-high molecular weight polyethylene (molecular weight 1 million) and paraffin oil are melt-blended and extruded into sheets at a mass ratio of 3:7, cooled and shaped, extracted and pore-formed by dichloromethane, and then stretched and shaped to obtain the diaphragm substrate, wherein the thickness of the diaphragm substrate is controlled at 5 μm.
[0048] 2. Preparation of coating slurry: Take sodium carboxymethyl cellulose powder and add it to deionized water (CMC: deionized water = 5:100, mass ratio), use a high-speed mixer to mix and stir to obtain sodium carboxymethyl cellulose solution, and stir for 60 minutes. Dry blend the ordered mesoporous carbon, PMMA microspheres with a particle size of 2μm, boehmite powder with a particle size of 0.4μm, and nanocellulose for 45 minutes, then add deionized water and sodium dodecylbenzene sulfonate to prepare the slurry, stir it with a planetary stirrer for 120 minutes, add sodium carboxymethyl cellulose solution, and stir for 30 minutes. Then add polyacrylate binder and silane coupling agent and stir for 40 minutes to obtain coating slurry. Among them, the mass ratio of ordered mesoporous carbon, PMMA microspheres, boehmite powder, nanocellulose and deionized water is 2:10:100:5:250, the mass ratio of silane coupling agent, polyacrylate binder and sodium dodecylbenzene sulfonate is 0.03:12:0.7, and the mass ratio of boehmite powder to polyacrylate binder is 10:0.7.
[0049] 3. Preparation of coated diaphragm: The slurry prepared in step 2 is coated on one side of the diaphragm substrate in step 1 using a micro-gravure roller, and the coating thickness is controlled at 2 μm. After coating, it is dried in an oven, and the drying temperature is controlled at 70°C.
[0050] 4. Preparation of composite diaphragm: The diaphragm substrate prepared in step 1 and the diaphragm substrate coated in step 3 are composited by hot pressing at a temperature of 90° C. and a pressure of 1 MPa to obtain a highly wettable composite diaphragm.
[0051] The structure of the highly wettable composite membrane obtained in this embodiment is as follows: Figure 1 As shown, it is a sandwich structure, and the coating layer is arranged between the diaphragm substrates 1. The coating layer includes ordered mesoporous carbon 2, PMMA microspheres 3 (i.e., glue dots between the diaphragm substrates 1, used to fix the upper and lower diaphragm substrates 1), nanocellulose 4 and ceramic particles 5.
[0052] Example 2
[0053] A method for preparing a highly wettable composite diaphragm comprises the following steps:
[0054] 1. Preparation of diaphragm substrate: Ultra-high molecular weight polyethylene (molecular weight 1 million) and paraffin oil are melt-blended and extruded into sheets at a mass ratio of 3:7, cooled and shaped, extracted and pore-formed by dichloromethane, and then stretched and shaped to obtain the diaphragm substrate, wherein the thickness of the diaphragm substrate is controlled at 5 μm.
[0055] 2. Preparation of coating slurry: Take sodium carboxymethyl cellulose powder and add it to deionized water (CMC: deionized water = 5:100, mass ratio), use a high-speed mixer to mix and stir to obtain sodium carboxymethyl cellulose solution, and stir for 60 minutes. Dry blend the ordered mesoporous carbon, PMMA microspheres with a particle size of 2 μm, boehmite powder with a particle size of 0.4 μm, and nanocellulose for 45 minutes, then add deionized water and sodium dodecyl sulfate to prepare the slurry, stir it with a planetary stirrer for 120 minutes, add sodium carboxymethyl cellulose solution, and stir for 30 minutes. Then add polyacrylate binder and alkylphenol polyoxyethylene ether and stir for 40 minutes to obtain coating slurry. Among them, the mass ratio of ordered mesoporous carbon, PMMA microspheres, boehmite powder, nanocellulose and deionized water is 2:10:100:5:250, the mass ratio of alkylphenol polyoxyethylene ether, polyacrylate binder and sodium dodecyl sulfate is 0.03:12:0.7, and the mass ratio of boehmite powder to polyacrylate binder is 10:0.7.
[0056] 3. Preparation of coated diaphragm: The slurry prepared in step 2 is coated on one side of the diaphragm substrate in step 1 using a micro-gravure roller, and the coating thickness is controlled at 3 μm. After coating, it is dried in an oven, and the drying temperature is controlled at 70°C.
[0057] 4. Preparation of composite diaphragm: The diaphragm substrate prepared in step 1 and the diaphragm substrate coated in step 3 are composited by hot pressing at a temperature of 90° C. and a pressure of 1 MPa to obtain a highly wettable composite diaphragm.
[0058] Example 3
[0059] A method for preparing a highly wettable composite diaphragm comprises the following steps:
[0060] 1. Preparation of diaphragm substrate: Ultra-high molecular weight polyethylene (molecular weight 1 million) and paraffin oil are melt-blended and extruded into sheets at a mass ratio of 3:7, cooled and shaped, extracted and pore-formed by dichloromethane, and then stretched and shaped to obtain the diaphragm substrate, wherein the thickness of the diaphragm substrate is controlled at 5 μm.
[0061] 2. Preparation of coating slurry: Take sodium carboxymethyl cellulose powder and add it to deionized water (CMC: deionized water = 5:100, mass ratio), use a high-speed mixer to mix and stir to obtain sodium carboxymethyl cellulose solution, and stir for 60 minutes. Dry blend the ordered mesoporous carbon, PMMA microspheres with a particle size of 2μm and boehmite powder with a particle size of 0.4μm for 45 minutes, then add deionized water and sodium dodecyl sulfate to prepare the slurry, stir it with a planetary stirrer for 120 minutes, add sodium carboxymethyl cellulose solution, and stir for 30 minutes. Then add polyacrylate binder and fatty alcohol polyoxyethylene ether and stir for 40 minutes to obtain coating slurry. Among them, the mass ratio of ordered mesoporous carbon, PMMA microspheres, boehmite powder, nanocellulose and deionized water is 2:10:100:5:250, the mass ratio of fatty alcohol polyoxyethylene ether, polyacrylate binder and sodium dodecyl sulfate is 0.03:12:0.7, and the mass ratio of boehmite powder to polyacrylate binder is 10:0.7.
[0062] 3. Preparation of coated diaphragm: The slurry prepared in step 2 is coated on one side of the diaphragm substrate in step 1 using a micro-gravure roller, and the coating thickness is controlled at 2 μm. After coating, it is dried in an oven, and the drying temperature is controlled at 70°C.
[0063] 4. Preparation of composite diaphragm: The diaphragm substrate prepared in step 1 and the diaphragm substrate coated in step 3 are composited by hot pressing at a temperature of 90° C. and a pressure of 1 MPa to obtain a highly wettable composite diaphragm.
[0064] Example 4
[0065] A method for preparing a highly wettable composite diaphragm comprises the following steps:
[0066] 1. Preparation of diaphragm substrate: Ultra-high molecular weight polyethylene (molecular weight 1 million) and paraffin oil are melt-blended and extruded into sheets at a mass ratio of 3:7, cooled and shaped, extracted and pore-formed by dichloromethane, and then stretched and shaped to obtain the diaphragm substrate, wherein the thickness of the diaphragm substrate is controlled at 5 μm.
[0067] 2. Preparation of coating slurry: Take sodium carboxymethyl cellulose powder and add it to deionized water (CMC: deionized water = 5:100, mass ratio), use a high-speed mixer to mix and stir to obtain sodium carboxymethyl cellulose solution, and the stirring time is 60 minutes. PMMA microspheres with a particle size of 2μm, boehmite powder with a particle size of 0.4μm and nanocellulose are dry-blended for 45 minutes, and then deionized water and sodium hexametaphosphate are added to prepare the slurry. Use a planetary stirrer to stir for 120 minutes, add sodium carboxymethyl cellulose solution, and stir for 30 minutes. Then add polyacrylate binder and fatty acid polyoxyethylene ether and stir for 40 minutes. Among them, the mass ratio of PMMA microspheres, boehmite powder, nanocellulose and deionized water is: 10:100:5:250, the mass ratio of fatty acid polyoxyethylene ether, polyacrylate binder, and sodium hexametaphosphate is 0.03:12:0.7, and the mass ratio of boehmite powder to polyacrylate binder is 10:0.7.
[0068] 3. Preparation of coated diaphragm: The slurry prepared in step 2 is coated on one side of the diaphragm substrate in step 1 using a micro-gravure roller, and the coating thickness is controlled at 2 μm. After coating, it is dried in an oven, and the drying temperature is controlled at 70°C.
[0069] 4. Preparation of composite diaphragm: The diaphragm substrate prepared in step 1 and the diaphragm substrate coated in step 3 are composited by hot pressing at a temperature of 90° C. and a pressure of 1 MPa to obtain a highly wettable composite diaphragm.
[0070] Example 5
[0071] A method for preparing a highly wettable composite diaphragm comprises the following steps:
[0072] 1. Preparation of diaphragm substrate: Ultra-high molecular weight polyethylene (molecular weight 1 million) and paraffin oil are melt-blended and extruded into sheets at a mass ratio of 3:7, cooled and shaped, extracted and pore-formed by dichloromethane, and then stretched and shaped to obtain the diaphragm substrate, wherein the thickness of the diaphragm substrate is controlled at 10 μm.
[0073] 2. Preparation of coating slurry: Take sodium carboxymethyl cellulose powder and add it to deionized water (CMC: deionized water = 5:100, mass ratio), use a high-speed mixer to mix and stir to obtain sodium carboxymethyl cellulose solution, and stir for 60 minutes. Dry blend the ordered mesoporous carbon, PMMA microspheres with a particle size of 2μm, boehmite powder with a particle size of 0.4μm, and nanocellulose for 45 minutes, then add deionized water and octylphenol polyoxyethylene ether to prepare the slurry, stir it with a planetary stirrer for 120 minutes, add sodium carboxymethyl cellulose solution, and stir for 30 minutes. Then add polyacrylate binder and polyether modified polysiloxane and stir for 40 minutes. Among them, the mass ratio of ordered mesoporous carbon, PMMA microspheres, boehmite powder, nanocellulose and deionized water is 2:10:100:5:250, the mass ratio of polyether modified polysiloxane, polyacrylate binder and octylphenol polyoxyethylene ether is 0.03:12:0.7, and the mass ratio of boehmite powder to polyacrylate binder is 10:0.7.
[0074] 3. Preparation of coated diaphragm: The slurry prepared in step 2 is coated on one side of the diaphragm substrate in step 1 using a micro-gravure roller, and the coating thickness is controlled at 3 μm. After coating, it is dried in an oven, and the drying temperature is controlled at 70°C.
[0075] Comparative Example 1
[0076] A method for preparing a composite diaphragm comprises the following steps:
[0077] 1. Preparation of diaphragm substrate: Ultra-high molecular weight polyethylene (molecular weight 1 million) and paraffin oil are melt-blended and extruded into sheets at a mass ratio of 3:7, cooled and shaped, extracted and pore-formed by dichloromethane, and then stretched and shaped to obtain the diaphragm substrate, wherein the thickness of the diaphragm substrate is controlled at 10 μm.
[0078] 2. Preparation of coating slurry: Take sodium carboxymethyl cellulose powder and add it to deionized water (CMC: deionized water = 5:100, mass ratio), use a high-speed mixer to mix and stir to obtain sodium carboxymethyl cellulose solution, and stir for 60 minutes. Add boehmite powder with a particle size of 0.8μm to deionized water and octylphenol polyoxyethylene ether to prepare slurry, stir for 120 minutes using a planetary stirrer, add sodium carboxymethyl cellulose solution, and stir for 30 minutes. Then add polyacrylate binder and polyether modified polysiloxane and stir for 40 minutes. Among them, the mass ratio of boehmite powder, polyether modified polysiloxane, polyacrylate binder, and octylphenol polyoxyethylene ether is 100:0.03:12:0.7.
[0079] 3. Preparation of coated diaphragm: The slurry prepared in step 2 is coated on one side of the diaphragm substrate in step 1 using a micro-gravure roller, and the coating thickness is controlled at 2 μm. After coating, it is dried in an oven, and the drying temperature is controlled at 70°C.
[0080] Comparative Example 2
[0081] A method for preparing a composite diaphragm comprises the following steps:
[0082] 1. Preparation of diaphragm substrate: Ultra-high molecular weight polyethylene (molecular weight 1 million) and paraffin oil are melt-blended and extruded into sheets at a mass ratio of 3:7, cooled and shaped, extracted and pore-formed by dichloromethane, and then stretched and shaped to obtain the diaphragm substrate, wherein the thickness of the diaphragm substrate is controlled at 10 μm.
[0083] 2. Preparation of coating slurry: Take sodium carboxymethyl cellulose powder and add it to deionized water (CMC: deionized water = 5:100, mass ratio), use a high-speed mixer to mix and stir to obtain sodium carboxymethyl cellulose solution, and stir for 60 minutes. Add boehmite powder with a particle size of 0.3 μm to deionized water and octylphenol polyoxyethylene ether to prepare slurry, stir for 120 minutes using a planetary stirrer, add sodium carboxymethyl cellulose solution, and stir for 30 minutes. Then add polyacrylate binder and polyether modified polysiloxane and stir for 40 minutes. Among them, the mass ratio of boehmite powder, polyether modified polysiloxane, polyacrylate binder, and octylphenol polyoxyethylene ether is 100:0.03:12:0.7.
[0084] 3. Preparation of coated diaphragm: The slurry prepared in step 2 is coated on one side of the diaphragm substrate in step 1 using a micro-gravure roller, and the coating thickness is controlled at 2 μm. After coating, it is dried in an oven, and the drying temperature is controlled at 70°C.
[0085] Performance Testing
[0086] The air permeability of the composite membranes obtained in the examples and comparative examples was tested using a Wangyan EG01-55-1MR air permeability tester.
[0087] The composite diaphragm was cut into samples of 10×10 cm, and a piece of A4 paper was placed on the top and bottom and put into a vacuum oven. After baking at 130°C for 1 hour, the thermal shrinkage was measured.
[0088] A 10×10 cm sample was fixed in the center of the stage using a two-dimensional projector, 1 mL of polyvinyl carbonate was added, and the infiltration distance on one side of the basement membrane was recorded within 5 min to test its infiltration speed.
[0089] Cut a 250mm×100mm sample and weigh it to get the initial weight. Immerse the sample completely in a beaker containing a certain amount of electrolyte, seal the beaker with plastic wrap, take out the test strip with tweezers after 1 hour, wipe the electrolyte on the surface with filter paper, place the test strip in a clean beaker, and continue to place it in a fume hood for 1 hour, weigh and record the weight of the membrane after it is left to stand, and the liquid retention rate is obtained by subtracting the weight of the first test from the weight of the second test compared with the original weight of the composite membrane sample.
[0090] The test results are shown in Table 1.
[0091] Table 1 Properties of the composite diaphragms obtained in Examples and Comparative Examples
[0092]
[0093]
[0094] By comparing the properties of the composite diaphragm obtained in the embodiment with those in comparative example 1, it can be seen that the composite coating in the embodiment has significantly improved the wetting speed, liquid retention rate and heat shrinkage resistance of the diaphragm. The improvement of liquid retention rate and wetting speed is conducive to extending the cycle life of the battery and reducing the risk of lithium precipitation in the battery core, improving the battery life and safety attributes, but the air permeability will increase to a certain extent, increasing the internal resistance of the battery. By comparing the properties of the composite diaphragm obtained in the embodiment with those in comparative examples 1 and 2, it can be seen that small-particle ceramics are conducive to improving the heat shrinkage resistance, but the composite diaphragms of comparative examples 1 and 2 will curl toward the ceramic surface. This is because the different heat resistance of the materials on both sides leads to uneven heat shrinkage, and placing the coating in the composite diaphragm is conducive to balancing this phenomenon. By comparing the properties of the composite diaphragms obtained in Example 1 and Example 2, it can be seen that increasing the thickness of the coating in the composite diaphragm is conducive to increasing the wetting speed and heat shrinkage resistance of the electrolyte, but the air permeability will increase accordingly. By comparing the properties of the composite membranes obtained in Example 1 and Example 3, it can be seen that the addition of nanocellulose is beneficial to increasing the infiltration speed of the electrolyte on the membrane and the heat shrinkage resistance, indicating that the electrolyte is easily transmitted along the cellulose network and plays a skeletal support role in the heat shrinkage resistance. By comparing the properties of the composite membranes obtained in Example 1 and Example 4, it can be seen that in the absence of ordered mesoporous carbon, the infiltration speed and liquid retention rate of the composite membrane have decreased to a certain extent, and its electrolyte storage function is limited. By comparing the properties of the composite membranes obtained in Example 1 and Example 5, it can be seen that the heat shrinkage resistance and liquid retention rate of the composite membrane that has not been hot-pressed are significantly reduced.
[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A highly wettable composite diaphragm, characterized in that: It includes a diaphragm substrate and a coating layer; the high wettability composite diaphragm is a sandwich structure, and the coating layer is located between the diaphragm substrate; The membrane substrate is a single-layer porous PE wet-process membrane, and the coating layer comprises ordered mesoporous carbon, polymethyl methacrylate microspheres, nanocellulose and ceramic powder.
2. The highly wettable composite diaphragm according to claim 1, characterized in that: The mass ratio of the ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder and nanocellulose is (1-10):(5-50):(100-300):(1-10); The thickness of the diaphragm substrate is 3-10 μm, and the thickness of the coating layer is 0.5-5 μm.
3. A method for preparing a highly wettable composite diaphragm according to claim 1 or 2, characterized in that: The steps include: The ultra-high molecular weight polyethylene and paraffin oil are melt-blended and extruded into a sheet, cooled and shaped, pores are formed, and stretched and shaped to obtain a diaphragm substrate; Ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder and nanocellulose are mixed, water is added, stirred, and a stabilizer solution is added to obtain a coating slurry; The coating slurry is coated on one side of the diaphragm substrate and dried, and the coated diaphragm substrate and the uncoated diaphragm substrate are hot-pressed and composited, with the coating slurry located between the diaphragm substrates, to obtain a highly wettable composite diaphragm.
4. The method for preparing a highly wettable composite diaphragm according to claim 3, characterized in that: The molecular weight of the ultra-high molecular weight polyethylene is 500,000-1.5 million; The mass ratio of ultra-high molecular weight polyethylene to paraffin oil is (1-5):(5-10); Alternatively, the pore-forming is performed by extraction with dichloromethane.
5. The method for preparing a highly wettable composite diaphragm according to claim 3, characterized in that: The particle size of the polymethyl methacrylate microspheres is 0.5 to 5 μm; The particle size of the ceramic powder is 0.3 to 0.6 μm; The mass ratio of the ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder, nanocellulose and water is (1-10):(5-50):(100-300):(1-10):(300-800).
6. The method for preparing a highly wettable composite diaphragm according to claim 3, characterized in that: The stabilizer includes sodium carboxymethyl cellulose; In the stabilizer solution, the mass ratio of stabilizer to water is (1-10):100; The mass ratio of the stabilizer to the ceramic powder is (0.5-1.5):(10-30); In the coating slurry preparation process, a stabilizer is mixed with water and stirred to obtain a stabilizer solution; ordered mesoporous carbon, polymethyl methacrylate microspheres, ceramic powder and nanocellulose are mixed, water and a dispersant are added, and after stirring, the stabilizer solution is added, and after stirring again, a binder and a surfactant are added, and stirred to obtain a coating slurry.
7. The method for preparing a highly wettable composite diaphragm according to claim 6, characterized in that: The dispersant includes ammonium polyacrylate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium hexametaphosphate or octylphenol polyoxyethylene ether; The binder is a polyacrylate binder; The surfactant comprises at least one of a silane coupling agent, an alkylphenol polyoxyethylene ether, a fatty alcohol polyoxyethylene ether, a fatty acid polyoxyethylene ether and a polyether-modified polysiloxane; The mass ratio of the ceramic powder, surfactant, binder and dispersant is (100-1600):(0.01-0.1):(10-80):(0.5-5).
8. The method for preparing a highly wettable composite diaphragm according to claim 3, characterized in that: The drying temperature is 50-90°C; Or, the hot pressing compounding has a hot pressing temperature of 60 to 110° C. and a hot pressing pressure of 0.1 to 5 MPa.
9. Use of the high wettability composite separator according to claim 1 or 2 in a battery.
10. A lithium battery, characterized in that: The separator of the lithium battery adopts the high wettability composite separator described in claim 1 or 2.
Citation Information
Patent Citations
Lithium ion battery diaphragm and preparation method thereof
CN113725555A
Diaphragm, preparation method thereof and secondary battery
CN114552122A
Diaphragm and secondary battery
CN116581481A
Modified composite separator and preparation method therefor
WO2023066342A1
Separator, secondary battery using same, battery module, battery pack, and electric apparatus
WO2024011404A1
Cited By
Lithium dendrite growth resistant composite diaphragm, preparation method thereof and lithium ion battery
CN119852641A
Negative-electrode-free battery cell, battery apparatus and electric apparatus
WO2026158043A1