Method for manufacturing reinforcing member material
By heating and cooling the felt layer with a dual-belt press and combining it with powder binder coating, the environmental problems caused by SBR latex impregnation are solved, enabling sustainable manufacturing of heel stabilizer materials while maintaining material performance.
Patent Information
- Application Number
- CN202380027871.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-15
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-01
AI Technical Summary
Existing heel stabilizer materials use SBR latex impregnation, which is environmentally unfriendly and affects material performance during manufacturing. A more sustainable alternative material and manufacturing method are needed.
An uncompressed felt layer is heated to below 20°C (the melting point of the fiber material) using a dual-belt press and then cooled to below the glass transition temperature. Combined with a powder binder coating, a compressed material is formed, avoiding latex impregnation.
It provides material properties similar to existing technologies while reducing environmental impact, enabling the sustainable manufacture of reinforcement component materials.
Smart Images

Figure CN118891152A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a felt material suitable for use as a reinforcing member in a shoe and a method of producing such a material. Background Art
[0002] Almost all modern shoes include reinforcement members in their internal structure. Shoe reinforcement members include, but are not limited to, toe pads at the front and heel counters in the heel to provide and maintain the desired shape throughout the useful life of the shoe.
[0003] In the heel area of a shoe, a heel counter is typically positioned between the outer material and the lining of the upper. The purpose of the heel counter is to reinforce the rear of the shoe, provide a suitable shape, and prevent the rear of the shoe from losing said shape, while providing some form of support to the heel area and maintaining the positive elements of foot physiology for the wearer. The most common manufacturing processes used to produce heel counters include film extrusion, dipping, and sintering.
[0004] One material currently used to form a heel counter is a polyester nonwoven fabric impregnated with an emulsion polymer. Specifically, the polyester nonwoven fabric is impregnated with a water-based SBR latex at a ratio of approximately 2:1 impregnant to fiber. The material is then cured, dried in an oven, and finally coated with a hot melt adhesive. The compatibility of the heel counter with the fabric and any adhesive used during shoe manufacturing may affect the resilience, stiffness, and shape retention of the heel counter and the shoe.
[0005] SBR latex is a synthetic rubber derived from organic compounds. It is a consumable product that is not considered to be environmentally friendly. In order to improve environmental reputation and sustainability, manufacturers and consumers are reluctant to use and purchase materials made from products such as SBR latex. It is now preferred to use materials made from recyclable materials or sustainable materials. Therefore, a more sustainably manufactured improved material for use as a reinforcement member is needed. In particular, it is desirable to avoid the need for latex dipping without causing any significant damage to the material properties of the reinforcement member. A method for manufacturing this material is also needed. Summary of the invention
[0006] The present invention provides a method for manufacturing a reinforcement component material, the method comprising:
[0007] An uncompressed felt layer is provided, wherein the uncompressed felt layer comprises a density of 0.08 g / cm 3 Up to 0.16g / cm 3 The main fiber material;
[0008] Passing the felt layer through a double belt press; wherein
[0009] As the felt layer passes through the double belt press, the felt layer is held under constant pressure while first heated to within 20°C of the melting point of the primary fiber material and then cooled below the glass transition temperature of the primary fiber material to form a compressed material.
[0010] An advantage of the method of the present invention is that it can provide a reinforcement member material having material properties similar to those of prior art materials impregnated with latex without the need for such impregnation. This is achieved by using a double belt press with integrated contact heating and contact cooling. In particular, the primary fibers are heated to within 20°C of the melting point of the primary fiber material and then cooled to below the glass transition temperature of the primary fiber material while the felt layer is maintained under pressure in the double belt press, resulting in a material having advantageous properties compared to the prior art. A suitable double belt press is shown in the accompanying drawings and discussed below. However, it should be understood that any heated double belt press capable of implementing the method of the present invention may be used, and such an apparatus will be immediately apparent to those skilled in the art.
[0011] The pressure applied to the uncompressed felt layer by the double belt press may be any suitable pressure for compressing the material to a suitable thickness. In an embodiment of the present invention, the pressure applied may be 10 N / cm 2 Up to 100N / cm 2 , 20N / cm 2 Up to 80N / cm 2 、30N / cm 2 Up to 70N / cm 2 , or 40N / cm 2 Up to 60N / cm 2 , for example 55N / cm 2 .
[0012] In an embodiment of the present invention, the main fiber material can be polyester. However, other suitable materials can be used and these materials are immediately obvious to those skilled in the art. A suitable alternative material is polylactic acid, which can be obtained from natural sources. The main fiber material can be polylactic acid, or can be a mixture of polyester and polylactic acid fibers, or can be any other suitable material. In addition to the main fiber material, the felt layer can also contain additional fiber materials with a melting point lower than the main fiber material. The main fiber material will account for at least 50% of the felt layer, and can account for 60%, 70%, 80%, 90% or 100% of the felt layer.
[0013] If the main fibre material is polyester it may be virgin material or recycled material or a mixture thereof.The polyester fibre used in the present invention may have any suitable coarseness, for example 1-12 dtex.
[0014] In an embodiment of the present invention, the felt layer or compressed material may be coated with a powder adhesive on one or both sides before passing through a double belt press or any other suitable heating and compression machine. It is generally advantageous that the double belt press used to compress the uncompressed felt layer of the present invention is used to heat and compress the powder adhesive applied to the material. For this reason, the description listed below relates to a double belt press, but where appropriate, this should be understood to refer to a double belt press or any other machine that can be used to heat and compress a powder adhesive on a flat material.
[0015] Suitable powder adhesives include, but are not limited to, polycaprolactone, ethylene vinyl acetate, polyurethane, polyester or polyamide powders or any suitable combination thereof.A powder adhesive may be used for coating to impart adhesive properties to the final material produced by the method of the present invention.
[0016] Often, it may be advantageous to coat opposite sides of the material separately. That is, a first side of the material may be coated with a powder adhesive and then the material may be passed through a heated double belt press to adhere the powder adhesive to the first side of the material, and then a second side of the material may be subsequently coated with a powder adhesive and then the material may be passed through a heated double belt press to adhere the powder coating to the second side of the material. In alternative embodiments of the present invention, the first and second sides of the material may be coated simultaneously.
[0017] After heating and compressing the uncompressed felt layer, coating the material with a powder binder can be performed as an additional process step. For example, after heating, compressing and cooling the felt layer according to the method of the present invention, the compressed material can be coated on one or both sides and then passed through a heated double belt press to compress and adhere the powder coating to the compressed material. Alternatively, coating on one or both sides can be performed simultaneously with heating and compressing the uncompressed felt layer.
[0018] Coating of the material on one or both sides with a powder binder can be performed as an additional process step, or as an in-line process with heating and pressing of the uncompressed felt layer, or as an in-line process to form a laminate or sandwich material.
[0019] It is readily understood that the heating and compression of the adhesive powder coating can be performed at lower temperatures and pressures than the heating and compression of the uncompressed felt layer, and if performed after the heating and compression of the uncompressed felt layer, can be performed at higher processing rates. For example, it may only be necessary to heat the powdered adhesive layer to less than 150°C, less than 120°C, or less than 100°C. In an embodiment of the present invention, a temperature of 90°C may be used to heat the powdered adhesive coating. Similarly, a pressure of less than 50 N / cm 2 , less than 40N / cm 2 , less than 30N / cm 2or less than 20N / cm 2 The pressure of 10N / cm2 may be sufficient to compress the powdered adhesive layer. 2 The pressure compresses the powdered adhesive coating.
[0020] According to the method of the present invention, the uncompressed felt layer is heated to within 20°C of the melting point of the main fiber material. In embodiments of the present invention, the felt layer can be heated to within 15°C, 10°C or 5°C of the melting point of the main fiber material, or to the melting point of the main fiber material. It is believed that heating the main fiber material to the melting point of the main fiber material can result in a harder final material.
[0021] Typically, in embodiments of the present invention, the thickness of the compressed material will be between 0.5 mm and 2.5 mm. A thickness less than 0.5 mm is undesirable because the reinforcement member material may form a brittle crystalline structure. It has been found that keeping the material thickness greater than 0.5 mm can avoid this problem. The maximum thickness, which may be, for example, 2.5 mm, is the maximum thickness that can achieve relatively uniform heating and cooling of the felt layer.
[0022] In an embodiment of the present invention, the density of the compressed material may be 0.4 g / cm 3 Up to 1.1g / cm 3 Materials of this density are considered suitable for use as reinforcement components for shoes. To form materials of this density, it has been found that materials with a density of 0.08 to 0.16 g / cm 3 A layer of uncompressed felt is usually suitable.
[0023] The double belt press of the present invention can be operated at any suitable speed. It is expected that those skilled in the art will be able to determine the appropriate speed for operating the press. For example, the speed at which the machine is operated may be greater than 1 m / min and may be less than 30 m / min. For the density step of passing the uncompressed felt layer through the double belt press, speeds at the lower end of this range may be preferred. For example, it may be preferred that the double belt press is operated at a speed of less than 10 m / min or less than 5 m / min. For subsequent processing of the laminate and / or coating material, as described above, it may be preferred that the double belt press is operated at a higher speed, for example, at a speed greater than 15 m / min or greater than 20 m / min.
[0024] The reinforcement member material of the present invention can be a single layer material formed as a direct output of the method of claim 1 of the present invention. In an embodiment of the present invention, the reinforcement member material can undergo further processing. For example, the method can also include a subsequent step of forming a laminated material comprising two or more layers of compressed materials. Additionally or alternatively, the method can also include a subsequent step of forming a sandwich material comprising two layers of compressed materials, the sandwich material having a filler material between the two layers of compressed materials. Any suitable filler material can be used, such as original or recycled materials. In some embodiments of the present invention, shredded lining materials can be used as filler materials, or powdered waste can be used. Coating the material with a powder adhesive can be performed in an online process of forming a laminated material or sandwich material. That is, the coating of the material can be performed simultaneously with the formation of the laminated material or sandwich material.
[0025] The formation of the laminate or sandwich material according to the present invention can be carried out using a double belt press or any similar machine. If a double belt press is used, this can be the same double belt press used to form the compressed material.
[0026] If a double belt press is used to form a layered or sandwich material, it is generally advantageous to operate it at the same speed and / or temperature and / or pressure as the double belt press is operated to form laminates and sandwich materials. It should be understood that those skilled in the art will understand the optimal conditions for operating a double belt press to form a layered or sandwich material.
[0027] The present invention also provides a reinforcing member material manufactured according to the method of the present invention. In particular, the present invention provides a reinforcing member material made of a compressed felt containing a main fiber material, wherein the density is 0.4 to 1.1 g / cm 3 , with a thickness of 0.5 to 2.5 mm. The material may have any of the properties and / or components listed above in the description of the method of the invention. For example, the material may have a powder coating, may be a laminate of two, three, four or more layers, and may be a sandwich material with a filler material between two layers of compressed material.
[0028] The reinforcing member material of the present invention may be used to form toe caps, heel counters, insoles, or any other reinforcing component for use with shoes or any other product that needs to be reinforced in a similar manner.
[0029] Density: 0.4g / cm 3 Up to 1.1g / cm 3 A material of 0.08 g / cm2 is considered suitable for use as a reinforcing component of a shoe. To form a material of this density, it has been found that a material with a density of 0.08 g / cm2 can be used. 3 Up to 0.16g / cm 3 An uncompressed felt layer is advantageous.
[0030] Other features and advantages of the present invention will be apparent from the embodiments of the present invention discussed below and illustrated in the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a schematic diagram of a double belt press suitable for use in the method of the present invention; and
[0032] Figure 2 It is shown that the use Figure 1 A graph of the thickness of the material of the reinforcement member produced by the double press according to the invention;
[0033] Figure 3 It is shown that the use Figure 1 A graph of the density of the reinforcement member material produced by the method according to the invention on a double press;
[0034] Figure 4 It is shown that the use Figure 1 A diagram of the stiffness of the material of the reinforcement member produced by the method according to the invention on a double press;
[0035] Figure 5 is a schematic diagram of a three-step dual-belt process for forming a coated laminate;
[0036] Figure 6 is a schematic diagram of a two-step dual-belt process for forming a coated laminate;
[0037] Figure 7 is a graph showing the weight of reinforcement member material produced according to the present invention;
[0038] Figure 8 is a graph showing the thickness of the reinforcement member material produced according to the present invention;
[0039] Fig. 9 are two graphs showing the density of reinforcement member materials produced according to the present invention;
[0040] Fig.10 are two graphs showing the density of reinforcement member materials produced according to the present invention; and
[0041] Fig.11 are two graphs showing the stiffness of the reinforcement member material according to the present invention.
[0042] Figure 1A schematic diagram of a belt press 1 suitable for the present invention is shown in . The belt press 1 includes two counter-rotating unperforated belts 2, each of which is mounted around a roller 3 at each end. The belt 2 is controlled to rotate in a suitable direction to pull the material through the belt press and compress the material. A hot plate 4 is provided to heat the material via the belt 2 and the hot roller 5. The hot plate 4 is heated using an oil or electric power unit (not shown). A cooling plate 6 is also provided. Cold water flows through the cooling plate 6 and the associated cold roller 7 via a centrifugal pump (not shown). The belt 2 is supported by the roller 3, the hot roller 5 and the cold roller 7, wherein pressure is applied to the material along the entire length of the belt press and the belt distance can be adjusted from a central control panel.
[0043] According to the invention, the process is carried out on an uncompressed felt material consisting of polyester (PET) fibers. Figure 1 The belt press 1 is operated to produce a reinforcing member material having a thickness of 0.5 mm to 2.5 mm. The melting point of the PET fiber is 245°C to 260°C, and the belt press 1 is operated to heat the felt material to 240°C to 245°C. The belt press 1 is operated at 50 and 60 N / cm 2 This will increase the density of the uncompressed felt material from 0.08-0.16g / cm 3 Increase to 0.4-1.1g / cm2 of finished product 3 The details of the uncompressed felt materials used are shown in Table 1 below:
[0044] weight thickness density gsm mm <![CDATA[g / cm 3 ]]> 256 2.7 0.0948 279 2.81 0.099288 530 3.5 0.151429 500 3.4 0.147059 600 3.8 0.157895 550 3.6 0.152778
[0045] Table 1: Uncompressed felt samples used showing initial density
[0046] Figure 2 Details of the thickness of the reinforcement member material produced from the above-described samples according to the invention are shown in FIG. Figure 3 Details of the density of the reinforcement member material are shown in . Figure 4 Details of the DLC (stiffness) in Newtons are shown in . From the data shown in these figures it can be seen that reinforcement member materials with a thickness of 0.5mm to 2.5mm, a stiffness of 20N to 100N and a weight of 500gsm to 750gsm can be produced using the method of the present invention.
[0047] Figure 5 A three-step method for forming a layered material according to the present invention is shown. The method uses a method based essentially on Figure 1 Double belt press 1 with hot plate 4 and cooling plate 6. In a first step, two 250 gsm sheets of compressed material formed in the manner immediately above are fed through the double belt press 1 at a feed speed of 8 m / min and a pressure of 55 N / cm 2The double belt press 1 is operated at a temperature of 247° C. This first step is used to form a laminated uncoated reinforcement member material.
[0048] In a second step, the first side of the laminate was powder coated with a powder adhesive by feeding at a feed rate of 20 m / min, 10 N / cm 2 The double belt press 1 is operated at a pressure of 1000 rpm and a temperature of 90° C. This forms a laminated reinforcement member material coated on a first side.
[0049] In the third and final step, the second side of the laminated reinforcement member material is coated with a powder adhesive and is fed at a feed rate of 20 m / min, 10 N / cm 2 The double belt press 1 is operated at a pressure of 1000 Nm and a temperature of 90° C. This forms a laminated reinforcement member material coated on both the first side and the second side.
[0050] The double belt press 1 of the first, second and third steps may be the same double belt press, or two or three separate double belt presses may be used.
[0051] Figure 6 A two-step method for forming a layered material according to the present invention is shown.
[0052] This method uses basically Figure 1 Double belt press 1 with hot plate 4 and cooling plate 6. In a first step, two 250 gsm sheets of compressed material formed in the manner immediately above are fed through the double belt press 1 at a feed speed of 8 m / min, 55 N / cm 2 The uppermost sheet is coated on the first side with a powder adhesive before passing through the double belt press 1. This forms a laminated reinforcement member material coated on the first side.
[0053] In the second and final step, the second side of the laminated reinforcement member material is coated with a powder adhesive and is subjected to a pressure of 10 N / cm2 at a feed rate of 20 m / min. 2 The double belt press 1 is operated with a pressure of 1000 Å and a temperature of 90° C. This forms a laminated reinforcement member material coated on both the first side and the second side.
[0054] The double-belt press 1 of the first and second steps may be the same double-belt press, or two or three separate double-belt presses may be used.
[0055] exist Figure 6 and 7 The powder binder used in the method is caprolactone coating.
[0056] Figure 7 and Figure 8 The weight and thickness of a sample according to the invention formed from two 300gsm sheets or a reinforcing member material formed from a single 500gsm sheet formed according to the invention are shown. The reinforcing member material was coated on both sides with 60gsm caprolactone coating.
[0057] The weight and thickness of the coated reinforcement member material according to the present invention are listed below in Tables 2 and 3. The layered reinforcement member material was formed according to the two-step method described above.
[0058]
[0059]
[0060] Table 2: Weight of coating material formed in the two-step process (g / m 2 )
[0061]
[0062] Table 3: Thickness of coating material formed in the two-step process (mm)
[0063] Fig. 9 The density of various samples of 300 gsm or 500 gsm material formed in accordance with the present invention is shown compared to upper and lower specification levels.
[0064] Fig.10 The density of various samples of materials formed according to the present invention are shown. The samples are 500gsm single layer materials, laminates formed from two layers of 300gsm materials, or 1000gsm laminates formed from two layers of 500gsm materials. The two 1000gsm laminates were formed at a machine speed of either 2.7m / min or 3.2m / min. It can be seen that the 1000gsm material formed at the higher speed generally has a lower density. Fig.10 All materials in the 3 The density of Fig.10 The data are shown in Table 4 below.
[0065]
[0066] Table 4: Density of samples according to the invention (g / cm 3 )
[0067] Fig.11The stiffness of various samples of materials formed according to the present invention are shown. The samples were 500 gsm single layer materials, laminates formed from two layers of 300 gsm materials, or 1000 gsm laminates formed from two layers of 500 gsm materials. All of these materials were coated with 60 gsm CAPA layers on both sides. The two 1000 gsm laminates were formed at a machine speed of either 2.7 m / min or 3.2 m / min. It can be seen that the 1000 gsm laminates formed at higher speeds generally had higher stiffness. From Fig.11 The data are shown in Table 5 below.
[0068]
[0069]
[0070] Table 5: Stiffness of laminated materials relative to single-layer materials (N)
[0071] Unless the context indicates otherwise, the description of the embodiments of the present invention above is for illustration purposes only to explain the present invention.Any feature of the present invention discussed above may be implemented independently of any other feature.
Claims
1. A method for manufacturing a reinforcement member material, the method comprising: An uncompressed felt layer is provided, wherein the uncompressed felt layer comprises a density of 0.08 g / cm 3 Up to 0.16g / cm 3 The main fiber material; The felt layer is passed through a double belt press; wherein As the felt layer passes through the double belt press, the felt layer is held under constant pressure while first heated to within 20°C of the melting point of the primary fiber material and then cooled below the glass transition temperature of the primary fiber material to form a compressed material.
2. The method of claim 1, wherein the primary fiber material is polyester.
3. The method according to claim 2, wherein the felt layer consists only of the primary fiber material.
4. The method according to claim 1 or 2, wherein the felt layer comprises a second fiber material having a lower melting point than the main fiber material.
5. A method according to any one of claims 1 to 4, wherein the compressed material is coated on one or both sides with a powder binder and then passed through a heated double belt press.
6. The method of claim 5, wherein the compressed material is coated on both sides with a powdered binder and then passed through a heated double belt press.
7. The method of claim 5, wherein the compressed material is coated on a first side with a powder binder and then the compressed material is passed through a heated double belt press; The compressed material is then coated with a powdered binder on a second side opposite the first side and then passed through a heated double belt press.
8. The method according to any one of claims 5 to 7, wherein the heated double belt press is at a temperature of less than 150°C and a pressure of less than 20 N / cm 2 Operate under pressure.
9. The method according to any one of claims 1 to 4, wherein the uncompressed felt material is coated on one or both sides with a powder adhesive before it passes through the heated double belt press.
10. The method of claim 9, wherein the uncompressed felt material is coated on both sides with a powder adhesive before passing the uncompressed felt material through the heated double belt press.
11. The method of claim 9, wherein the uncompressed felt material is coated on a first side with a powdered adhesive before the uncompressed felt material passes through the heated double belt press; The compressed material is then coated with a powdered binder on a second side opposite the first side and then passed through a heated double belt press.
12. A method according to any one of claims 5 to 11, wherein the powder binder is one or more of polycaprolactone, ethylene vinyl acetate, polyurethane, polyester or polyamide powder.
13. A method according to any one of the preceding claims, wherein the uncompressed felt layer is heated to the melting point of the principal fibre material as it passes through the double belt press.
14. A method according to any one of the preceding claims, wherein the compressed material has a thickness of 0.5 mm to 2.5 mm.
15. A method according to any one of the preceding claims, wherein the density of the compressed material is 0.4 g / cm 3 Up to 1.1g / cm 3 .
16. A method according to any preceding claim, further comprising the subsequent step of forming a laminate comprising two or more layers of said compressed material.
17. The method of claim 16, wherein the laminate is formed by passing the layers through a heated double belt press.
18. The method according to any one of claims 1 to 16, further comprising the subsequent step of forming a sandwich material comprising two layers of the compressed material, the sandwich material having a filler material between the two layers of the compressed material.
19. The method of claim 18, wherein the sandwich material is formed by passing the layers of compressed material and the layers of filler material through a heated double belt press.
20. A method according to any one of claims 17 or 19, wherein the laminate or sandwich material is coated on at least one side prior to passing through the heated double belt press.
21. The method of claim 20, wherein the laminate or sandwich material is coated on both sides before passing through the double belt press.
22. The method of claim 20, wherein the laminate or sandwich material is coated on a first side prior to passing through the heated double belt press.
23. A method according to claim 22, wherein the laminate or sandwich material is subsequently coated on a second side opposite the first side and then passed through a heated double press.
24. A method according to any one of claims 16 to 19 wherein after forming the laminate or sandwich material the material is coated on one or both sides and passed through a heated double belt press.
25. A reinforcement member material produced according to the method of any preceding claim.
Citation Information
Patent Citations
Shoe stiffner
CA350300A
material in particular intended for the manufacture of hard ends and stiffeners of shoes
FR1009037A
Laminar materials suitable for use in the manufacture of shoes, method of making same and shoe stiffener materials including said laminar materials
US20020022428A1
Method of producing a thermoplastically moldable fiber-reinforced semifinished product
US20060244170A1
Process for producing fiber-reinforced thermoplastic material with a double-belt press
US5395576A