Secondary battery
By using Li, Ti, M1 and X coating materials in lithium-ion secondary batteries, the interface resistance between the electrolyte and the positive electrode active substance is reduced, the problem of insufficient cyclic characteristics in the prior art is solved, and a higher capacity is achieved and cycle characteristics, extend battery life and reduce internal resistance.
Patent Information
- Application Number
- CN202380023085.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-13
- Publication Date
- 2024-11-01
AI Technical Summary
The existing lithium-ion secondary batteries have shortcomings in terms of cycle characteristics and magnification characteristics, and it is difficult to form a coating layer by simple element composition, resulting in contact between the electrolyte and the positive electrode active material, resulting in decomposition, affecting the capacity and stability of the battery.
A coating material containing Li, Ti, M1 and X is used, M1 is Be, Mg, Ca, Sr, Ba, Sc, Y, Al, Ga, In, Zr, Sn, and X is composed of F, Cl, Br, I , the electrolyte contains an electrolyte and a non-aqueous solvent, and by reducing the interface resistance between the electrolyte and the positive electrode active substance, it inhibits decomposition and improves the circulation characteristics.
It significantly improves the capacity and circulation characteristics of the secondary battery, extends the service life of the battery, reduces the internal resistance, and improves the charge and discharge efficiency and energy density.
Smart Images

Figure CN118891753A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a secondary battery. Background Art
[0002] Non-aqueous electrolyte secondary batteries, represented by lithium-ion secondary batteries, have high energy density and high output, and are considered promising as power sources for mobile devices such as smartphones, power sources for vehicles such as electric cars, storage devices for natural energy such as solar energy, etc. The positive electrode active material of non-aqueous electrolyte secondary batteries uses, for example, a composite oxide containing lithium and a transition metal.
[0003] In Patent Document 1, in order to improve the cycle characteristics and rate characteristics, it is proposed to form a coating layer containing a metal oxide and a compound containing Li and P on the surface of a composite oxide containing lithium and a transition metal as a positive electrode active material of a non-aqueous electrolyte secondary battery. The above-mentioned metal oxide contains at least one metal element selected from the group consisting of Group 3, Group 13 and lanthanide elements of the periodic table. As compounds containing Li and P, Li3PO4, Li4P2O7 and Li3PO3 are listed.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2013 / 047877 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] The present disclosure provides a novel secondary battery including a coating layer.
[0009] Solutions for solving problems
[0010] The secondary battery of the present disclosure comprises a positive electrode, a negative electrode and an electrolyte.
[0011] The positive electrode comprises a positive electrode active material and a coating material covering at least a portion of a surface of the positive electrode active material.
[0012] The coating material comprises Li, Ti, M1 and X,
[0013] M1 is at least one selected from the group consisting of Be, Mg, Ca, Sr, Ba, Sc, Y, Al, Ga, In, Zr and Sn, X is at least one selected from the group consisting of F, Cl, Br and I,
[0014] The electrolyte solution includes an electrolyte and a non-aqueous solvent.
[0015] Effects of the Invention
[0016] According to the present disclosure, a novel secondary battery including a covering layer can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 1 is a longitudinal sectional view schematically showing a secondary battery 10 according to an embodiment of the present disclosure.
[0018] Figure 2 It is a graph showing the charge and discharge curves of the batteries of Example 1 and Comparative Example 1 in the first cycle.
[0019] Figure 3 It is a graph showing the charge and discharge curves of the batteries of Example 1 and Comparative Example 1 at the 50th cycle.
[0020] Figure 4 This is a graph showing the transition of the discharge capacity of the batteries of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0021] (Insights that form the basis of this disclosure)
[0022] As described in the background art column, in order to improve the cycle characteristics, Patent Document 1 proposes forming a coating layer containing a metal oxide and a compound containing Li and P on the surface of a composite oxide containing lithium and a transition metal. However, due to concerns that a specific element may not be easily available, it is necessary to be able to form the coating layer with a variety of elements.
[0023] Based on the above findings, the present inventors have completed the following secondary battery of the present disclosure.
[0024] (Overview of one embodiment of the present disclosure)
[0025] A secondary battery according to a first aspect of the present disclosure includes a positive electrode, a negative electrode, and an electrolyte solution.
[0026] The positive electrode comprises a positive electrode active material and a coating material covering at least a portion of a surface of the positive electrode active material.
[0027] The coating material comprises Li, Ti, M1 and X,
[0028] The M1 is at least one selected from the group consisting of Be, Mg, Ca, Sr, Ba, Sc, Y, Al, Ga, In, Zr and Sn, and the X is at least one selected from the group consisting of F, Cl, Br and I,
[0029] The electrolyte solution includes an electrolyte and a non-aqueous solvent.
[0030] In the secondary battery according to the first aspect, the resistance of the interface between the electrolyte solution and the positive electrode active material is reduced, so the capacity is increased. Furthermore, the decomposition caused by the contact between the electrolyte solution and the positive electrode active material is suppressed, and the cycle characteristics can be improved.
[0031] In the second aspect of the present disclosure, for example, in the secondary battery according to the first aspect, X may contain F.
[0032] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0033] In a third aspect of the present invention, for example, in the secondary battery according to the first or second aspect, the coating material includes a material represented by the following composition formula (2):
[0034] Li 6-(4-a)b (Ti 1-a M1 a ) b X6…Formula (2)
[0035] Here, 0<a<1 and 0<b≤2 may be satisfied.
[0036] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0037] In a fourth aspect of the present disclosure, for example, in the secondary battery according to any one of the first to third aspects, the ratio of the amount of Li to the total amount of Ti and M1 may be 0.5 or more and 4.5 or less.
[0038] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0039] In a fifth aspect of the present disclosure, for example, in the secondary battery according to any one of the first to fourth aspects, M1 may be Al.
[0040] Al is inexpensive and is suitable as an element for improving the ion conductivity of the coating material. According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0041] In a sixth aspect of the present disclosure, for example, in the secondary battery according to any one of the first to fifth aspects, the coating material may cover 80% or more of the surface of the positive electrode active material.
[0042] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0043] In a seventh aspect of the present disclosure, for example, in the secondary battery according to the sixth aspect, the coating material may cover 95% or more of the surface of the positive electrode active material.
[0044] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0045] In an eighth aspect of the present disclosure, for example, in the secondary battery according to any one of the first to seventh aspects, the positive electrode active material may include a composite oxide containing lithium and a transition metal.
[0046] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0047] In a ninth aspect of the present invention, for example, in the secondary battery according to the eighth aspect, the composite oxide has a composition represented by the following composition formula (3):
[0048] LiNi x1 Co y1 M2 1-x1-y1 O2…Formula (3)
[0049] Here, 0≤x1<1, 0≤y1≤1, and 0≤1-x1-y1≤0.35 are satisfied, and M2 may be at least one selected from the group consisting of Al and Mn.
[0050] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0051] In a tenth aspect of the present invention, for example, in the secondary battery according to the eighth aspect, the composite oxide has a composition represented by the following composition formula (4):
[0052] LiNi x2 M3 1-x2 O2…Formula (4)
[0053] Here, 0.3≤x2<1 is satisfied, and M3 may be at least one selected from the group consisting of Co, Mn, Al, Ti, and Fe.
[0054] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0055] In the 11th aspect of the present disclosure, for example, in the secondary battery according to the 8th aspect, the composite oxide has a composition represented by the following composition formula (5):
[0056] Li x3 M4 y3 (PO4) z3 …Formula (5)
[0057] Here, 2.7≤x3≤3.3, 0.9≤y3≤2.2, and 0.9≤z3≤3.3 are satisfied, and M4 may be at least one selected from the group consisting of Ni, Co, Mn, Fe, and V.
[0058] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0059] In a twelfth aspect of the present disclosure, for example, in the secondary battery according to any one of the first to eleventh aspects, a solid electrolyte other than the solid electrolyte included as the covering material may not be included.
[0060] According to the above configuration, the capacity and cycle characteristics of the secondary battery can be improved.
[0061] Hereinafter, embodiments of the secondary battery according to the present disclosure will be described. The present disclosure is not limited to the following embodiments.
[0062] A secondary battery according to one embodiment of the present invention comprises a positive electrode, a negative electrode and an electrolyte. The positive electrode comprises a positive electrode active material and a coating material covering at least a portion of the surface of the positive electrode active material. The coating material comprises Li, Ti, M1 and X, M1 is at least one selected from the group consisting of Be, Mg, Ca, Sr, Ba, Sc, Y, Al, Ga, In, Zr and Sn, and X is at least one selected from the group consisting of F, Cl, Br and I. The electrolyte comprises an electrolyte and a non-aqueous solvent.
[0063] According to the above configuration, the resistance of the interface between the electrolyte and the positive electrode active material is reduced, so the capacity of the secondary battery is increased. Furthermore, the decomposition of the electrolyte due to the contact between the electrolyte and the positive electrode active material is suppressed, and the cycle characteristics of the secondary battery are improved.
[0064] Figure 1 Schematically shows a longitudinal cross-sectional view of a secondary battery 10 according to an embodiment of the present disclosure. Figure 1 As shown, the secondary battery 10 is a cylindrical battery including a cylindrical battery case, a wound electrode group 14, and an electrolyte solution (not shown). The electrode group 14 is housed in the battery case and is in contact with the electrolyte solution.
[0065] The battery case is composed of a case body 15 which is a bottomed cylindrical metal container and a sealing body 16 which seals the opening of the case body 15. A gasket 27 is arranged between the case body 15 and the sealing body 16. The airtightness of the battery case is ensured by the gasket 27. Insulating plates 17 and 18 are arranged at both ends of the electrode group 14 in the winding axis direction of the electrode group 14 in the case body 15.
[0066] The housing body 15 has, for example, a step portion 21. The step portion 21 can be formed by partially punching the side wall of the housing body 15 from the outside. The step portion 21 can also be formed in an annular shape on the side wall of the housing body 15 along the circumferential direction of the imaginary circle defined by the housing body 15. In this case, the sealing body 16 is supported by, for example, the surface of the step portion 21 on the opening side.
[0067] The sealing body 16 includes a metal plate 22 with an opening, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cover 26. These members are stacked in sequence in the sealing body 16. The sealing body 16 is attached to the opening of the housing body 15 in such a manner that the cover 26 is located outside the housing body 15 and the metal plate 22 with an opening is located inside the housing body 15.
[0068] Each of the above-mentioned members constituting the sealing body 16 is, for example, in a disk shape or a ring shape. Except for the insulating member 24, each of the above-mentioned members is electrically connected to each other.
[0069] The electrode group 14 includes a positive electrode 11, a negative electrode 12, and a separator 13. The positive electrode 11, the negative electrode 12, and the separator 13 are all in a strip shape. The width direction of the strip-shaped positive electrode 11 and the negative electrode 12 is, for example, parallel to the winding axis of the electrode group 14. The separator 13 is arranged between the positive electrode 11 and the negative electrode 12. The positive electrode 11 and the negative electrode 12 are wound in a spiral shape with the separator 13 interposed between these electrodes.
[0070] When viewing a cross section of the secondary battery 10 in a direction perpendicular to the winding axis of the electrode group 14 , the positive electrodes 11 and the negative electrodes 12 are alternately stacked in a radial direction of an imaginary circle defined by the case body 15 with the separator 13 interposed therebetween.
[0071] The positive electrode 11 is electrically connected to the cap 26 also serving as a positive electrode terminal via a positive electrode lead 19. One end of the positive electrode lead 19 is connected, for example, to the vicinity of the center of the positive electrode 11 in the longitudinal direction of the positive electrode 11. The positive electrode lead 19 extends from the positive electrode 11 to the metal plate 22 with an opening through a through hole formed in the insulating plate 17. The other end of the positive electrode lead 19 is, for example, welded to the surface of the metal plate 22 with an opening on the electrode group 14 side.
[0072] The negative electrode 12 is electrically connected to the case body 15 also serving as a negative electrode terminal via a negative electrode lead 20. One end of the negative electrode lead 20 is connected to, for example, an end of the negative electrode 12 in the longitudinal direction of the negative electrode 12. The other end of the negative electrode lead 20 is welded to the inner bottom surface of the case body 15, for example.
[0073] Hereinafter, each structure of the secondary battery 10 will be described in detail.
[0074] (positive electrode 11)
[0075] The positive electrode 11 can store or release lithium and includes a positive electrode active material and a coating material that covers at least a part of the surface of the positive electrode active material.
[0076] The coating material includes Li, Ti, M1, and X. Here, M1 is at least one selected from the group consisting of Be, Mg, Ca, Sr, Ba, Sc, Y, Al, Ga, In, Zr, and Sn, and X is at least one selected from the group consisting of F, Cl, Br, and I.
[0077] In order to improve ion conductivity, the coating material may contain anions other than X. The anions other than X are at least one selected from the group consisting of O and Se.
[0078] The coating material may be substantially composed of Li, Ti, M1 and X. Here, "the coating material is substantially composed of Li, Ti, M1 and X" means that the ratio of the total amount of Li, Ti, M1 and X to the total amount of all elements constituting the coating material (i.e., molar fraction) is 90% or more. As an example, the ratio may be 95% or more. The coating material may be composed only of Li, Ti, M1 and X.
[0079] X may contain F. X may be F.
[0080] The oxidation resistance of the coating material is improved by including F. Since the oxidative decomposition of the coating material is suppressed, the increase in the internal resistance of the battery can be suppressed, and the capacity of the secondary battery is further increased.
[0081] In order to improve the ion conductivity of the coating material, the ratio of the amount of Li to the total amount of Ti and M1 may be 0.5 or more and 4.5 or less.
[0082] The ratio of the amount of X to the total amount of Li, Ti, M1, and X may be 0.4 to 0.8, or 0.5 to 0.7.
[0083] The coating material may include a material represented by the following composition formula (1): Here, α, β, γ, and δ are values greater than zero.
[0084] Li α Ti β M1 γ X δ ……Formula 1
[0085] In the composition formula (1), δ may be a value greater than α. δ may also be a value greater than α, β, and γ, respectively.
[0086] In the composition formula (1), 1.7≤α≤3.7, 0<β<1.5, 0<γ<1.5 and 5≤δ≤7 may be satisfied.
[0087] In the composition formula (1), 2.5≤α≤3, 0.1≤β≤0.6, 0.4≤γ≤0.9 and 5<δ≤6 may be satisfied.
[0088] The coating material may contain the material represented by the composition formula (1) as a main component. Here, the "main component" refers to the component with the largest content in terms of mass ratio.
[0089] The coating material includes a material represented by the following composition formula (2),
[0090] Li 6-(4-a)b (Ti 1-a M1 a ) b X6……Formula (2)
[0091] Here, 0<a<1 and 0<b≤2 may be satisfied.
[0092] In order to improve the ion conductivity of the coating material, in the formula (2), 0.1≤a≤0.9 and 0.8≤b≤1.2 may be satisfied, or 0.5≤a≤0.9 and 0.8≤b≤1.2 may be satisfied.
[0093] M1 may contain Al. M1 may also be Al.
[0094] The thickness of the coating material covering at least a portion of the surface of the positive electrode active material may be 1 nm or more and 500 nm or less.
[0095] When the thickness of the coating material is 1 nm or more, the direct contact between the positive electrode active material and the electrolyte can be suppressed, and the oxidative decomposition of the electrolyte can be suppressed. Therefore, the charge and discharge efficiency of the battery can be improved. When the thickness of the coating material is 500 nm or less, the thickness of the coating material will not be too thick. Therefore, the internal resistance of the battery can be fully reduced. Therefore, the energy density of the battery can be improved.
[0096] The method for measuring the thickness of the coating material is not particularly limited, and the thickness of the coating material can be determined, for example, by directly observing the thickness of the coating material using a transmission electron microscope or the like.
[0097] The mass ratio of the coating material to the positive electrode active material may be 0.01% or more and 30% or less.
[0098] When the mass ratio of the coating material to the positive electrode active material is 0.01% or more, the direct contact between the positive electrode active material and the electrolyte can be suppressed, and the oxidative decomposition of the electrolyte can be suppressed. Therefore, the charge and discharge efficiency of the battery can be improved. When the mass ratio of the coating material to the positive electrode active material is 30% or less, the thickness of the coating material will not become too thick. Therefore, the internal resistance of the battery can be fully reduced. Therefore, the energy density of the battery can be improved.
[0099] The coating material can evenly coat the surface of the positive electrode active material. Thus, the direct contact between the positive electrode active material and the electrolyte can be suppressed, and the oxidative decomposition of the electrolyte can be suppressed. Therefore, the charge and discharge characteristics of the battery can be further improved, and the internal resistance of the battery during charging can be suppressed.
[0100] The coating material may cover a portion of the surface of the positive electrode active material. A plurality of positive electrode active materials are in direct contact with each other via the portion not covered by the coating material, and the electron conductivity between the positive electrode active materials is improved. Therefore, the battery can operate at a high output.
[0101] The coating material may cover more than 30%, more than 60%, more than 80%, more than 90%, or more than 95% of the surface of the positive electrode active material. The coating material may cover substantially the entire surface of the positive electrode active material.
[0102] The positive electrode active material is a material that can absorb or release lithium. The positive electrode active material may include a composite oxide containing lithium and a transition metal. The transition metal may include at least one selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), iron (Fe), copper (Cu), chromium (Cr), titanium (Ti), niobium (Nb), zirconium (Zr), vanadium (V), tantalum (Ta) and molybdenum (Mo). Hereinafter, "composite oxide" refers to a composite oxide containing lithium and a transition metal.
[0103] The composite oxide is synthesized by a coprecipitation method or the like, for example, a lithium compound is mixed with a transition metal-containing compound obtained by a coprecipitation method or the like, and the obtained mixture is calcined under specified conditions. The composite oxide usually forms secondary particles formed by aggregation of multiple primary particles. The average particle size (D50) of the composite oxide particles is, for example, greater than 3 μm and less than 25 μm. It should be noted that the average particle size (D50) refers to the particle size (volume average particle size) when the volume cumulative value becomes 50% in the volume-based particle size distribution measured by a laser diffraction scattering method.
[0104] The composite oxide may contain metals other than transition metals. The metals other than transition metals may contain at least one selected from the group consisting of aluminum (Al), magnesium (Mg), calcium (Ca), strontium (Sr), zinc (Zn) and silicon (Si). In addition, the composite oxide may contain boron (B) and the like in addition to metals.
[0105] From the viewpoint of high capacity, the transition metal may include Ni. The composite oxide may include Ni and at least one selected from the group consisting of Co, Mn, Al, Ti and Fe. From the viewpoint of high capacity and high output, the composite oxide may include Ni and at least one selected from the group consisting of Co, Mn and Al, or may include Ni and Co and at least one selected from the group consisting of Mn and Al. In the case where Co is included in addition to Li and Ni in the composite oxide, the phase change of the composite oxide including Li and Ni is suppressed during charge and discharge, the stability of the crystal structure is improved, and the cycle characteristics are easily improved. In the case where the composite oxide further includes at least one selected from the group consisting of Mn and Al, thermal stability is improved.
[0106] From the viewpoint of facilitating high capacity, in the composite oxide, the atomic ratio of Ni to the total of metals other than Li (Ni / Me) may be 0.3 or more and less than 1, or 0.5 or more and less than 1.
[0107] From the viewpoint of improving cycle characteristics and high output, the composite oxide may include a composite oxide having a layered rock salt type crystal structure and containing at least one selected from the group consisting of Ni and Co, or may include a composite oxide having a spinel type crystal structure and containing Mn. From the viewpoint of high capacity, the composite oxide may be a composite oxide having a layered rock salt type crystal structure, containing Ni and a metal other than Ni, and having a total atomic ratio (Ni / Me) of Ni to metals other than Li of 0.3 or more and less than 1 (hereinafter also referred to as a nickel-based composite oxide).
[0108] The crystal structure of nickel composite oxide is relatively unstable, and due to contact with the non-aqueous electrolyte in the positive electrode of high potential, it is easy to deteriorate due to the dissolution of Ni, and the cycle characteristics are easily reduced. Therefore, in the case of nickel composite oxide, the improvement effect of the cycle characteristics brought about by coating with the coating material can be significantly obtained. By coating with the coating material, the high capacity of the nickel composite oxide can be fully drawn out.
[0109] From the viewpoint of improving cycle characteristics, increasing capacitance and increasing output, the composite oxide has a composition represented by the following composition formula (3):
[0110] LiNi x1 Co y1 M2 1-x1-y1 O2……Formula (3)
[0111] Here, 0.3≤x1<1, 0<y1≤0.5 and 0<1-x1-y1≤0.35 are satisfied, and M2 may be at least one selected from the group consisting of Al and Mn. In the composition formula (3), 0.5≤x1<1 may be satisfied. In the composition formula (3), 0<y1≤0.35 may be satisfied.
[0112] The composite oxide has a composition represented by the following composition formula (4):
[0113] LiNi x2 M3 1-x2 O2……Formula (4)
[0114] Here, 0.3≤x2<1 is satisfied, and M3 can be at least one selected from the group consisting of Co, Mn, Al, Ti and Fe. When x2 is within the above range, the effect of Ni and the effect of element M3 can be well balanced. In composition formula (4), x2 can be greater than 0.5 or greater than 0.75.
[0115] The composite oxide has a composition represented by the following composition formula (5),
[0116] Li x3 M4 y3 (PO4) z3 ……Formula (5)
[0117] Here, 2.7≤x3≤3.3, 0.9≤y3≤2.2, and 0.9≤z3≤3.3 are satisfied, and M4 may be at least one selected from the group consisting of Ni, Co, Mn, Fe, and V.
[0118] At least a portion of the surface of the composite oxide may be covered with a coating material different from the coating material. Examples of the coating material include oxides. Examples of oxides used in the coating material include Li-Nb-O compounds such as LiNbO3, Li-BO compounds such as LiBO2 and Li3BO3, Li-Al-O compounds such as LiAlO2, Li-Si-O compounds such as Li4SiO4, Li-SO compounds such as Li2SO4, Li4Ti5O 12 Li-Ti-O compounds, Li-Zr-O compounds such as Li2ZrO3, Li-Mo-O compounds such as Li2MoO3, Li-VO compounds such as LiV2O5, Li-WO compounds such as Li2WO4, and Li-PO compounds such as Li3PO4.
[0119] According to the above configuration, the oxidation resistance of the positive electrode active material can be further improved, thereby suppressing an increase in the internal resistance of the battery during charging.
[0120] The coating material and the positive electrode active material at least part of the surface of which is covered with the coating material in the secondary battery of one embodiment can be produced by the following method, for example.
[0121] A raw material powder of a binary halide having a mixing ratio that is the composition of the target coating material is prepared. 2.7 Ti 0.3 Al 0.7 In the case of F6, LiF, TiF4 and AlF3 are prepared at a molar ratio of LiF:TiF4:AlF3 = 2.7:0.3:0.7. The mixing ratio may be adjusted in advance to offset the change in composition during the synthesis process.
[0122] After the raw material powders are fully mixed, the raw material powders are mixed, crushed and reacted with each other using a mechanochemical grinding method. Then, the raw material powders can be fired in a vacuum or an inert atmosphere. Alternatively, the raw material powders can be fully mixed and fired in a vacuum or an inert atmosphere. The firing conditions are preferably, for example, fired at a temperature of 100° C. or more and 300° C. or less for more than 1 hour. In addition, in order to suppress changes in the composition during the firing process, the raw material powders are preferably sealed in a sealed container such as a quartz tube and fired.
[0123] Thus, a coating material having the above-mentioned composition is obtained.
[0124] Next, a composite oxide with a predetermined mass ratio is prepared as a positive electrode active material. For example, Li(NiCoMn)O2 is prepared as a composite oxide. 2.7 Ti 0.3 Al 0.7 F6 is put into the same reaction container, and a shear force is applied to the two materials by a rotating blade, or the two materials are collided by a jet of gas, so that at least a part of the surface of the composite oxide Li(NiCoMn)O2 can be coated with Li as a coating material. 2.7 Ti 0.3 Al 0.7 F6. For example, a dry particle compounding device NOBILTA (manufactured by Hosokawa Micron), a high-speed airflow impact device (manufactured by Nara Machinery Co., Ltd.), a jet mill, or the like can be used.
[0125] By the above method, a positive electrode active material, namely, a composite oxide Li(NiCoMn)O2, at least a portion of the surface of which is covered with a covering material can be obtained. However, the method for producing the covering material and the covered positive electrode active material is not limited to the above.
[0126] The positive electrode 11 may include a positive electrode current collector and a positive electrode mixture layer supported on the surface of the positive electrode current collector. The positive electrode mixture layer may be formed, for example, by applying a positive electrode slurry obtained by dispersing a positive electrode mixture in a dispersion medium to the surface of the positive electrode current collector and drying it. The dried coating may be rolled as needed. The positive electrode mixture layer may be formed on one surface of the positive electrode current collector or on both surfaces. As a dispersion medium, for example, N-methyl-2-pyrrolidone (NMP) or the like is used.
[0127] The positive electrode mixture layer includes a positive electrode active material and a coating material that covers at least a portion of the surface of the positive electrode active material. The positive electrode mixture layer may further include a binder, a conductive agent, and the like.
[0128] As the binder, resin materials such as fluororesins, polyolefin resins, polyamide resins, polyimide resins, acrylic resins, and vinyl resins can be exemplified. As fluororesins, polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF) can be cited. The binder can be used alone or in combination of two or more.
[0129] Examples of the conductive agent include carbon blacks such as acetylene black, conductive fibers such as carbon fibers and metal fibers, and carbon fluoride. The conductive agent may be used alone or in combination of two or more.
[0130] The positive electrode current collector may be, for example, a metal foil. Examples of the metal constituting the positive electrode current collector include aluminum, titanium, alloys containing these metal elements, and stainless steel. The thickness of the positive electrode current collector is not particularly limited, and is, for example, 3 μm or more and 50 μm or less.
[0131] (negative electrode 12)
[0132] The negative electrode 12 includes a material having the property of storing and releasing metal ions (for example, lithium ions). The negative electrode 12 includes, for example, a negative electrode active material.
[0133] The negative electrode active material may include a carbon material that absorbs and releases lithium ions. Examples of carbon materials that absorb and release lithium ions include graphite (natural graphite, artificial graphite), easily graphitized carbon (soft carbon), and difficultly graphitized carbon (hard carbon). Among them, graphite is preferred because it has excellent charge and discharge stability and a small irreversible capacity.
[0134] The negative electrode active material may include an alloy material. An alloy material refers to a material containing at least one metal that can form an alloy with lithium, such as silicon, tin, silicon alloys, tin alloys, and silicon compounds. As a silicon compound, a composite material having a lithium ion conductive phase and silicon particles dispersed in the phase can be used. As a lithium ion conductive phase, a silicate phase such as a lithium silicate phase, a silicon oxide phase having more than 95% by mass of silicon dioxide, a carbon phase, etc. can be used.
[0135] As the negative electrode active material, an alloy material and a carbon material may be used in combination. In this case, the ratio of the carbon material to the total of the alloy material and the carbon material may be, for example, 80% by mass or more, or 90% by mass or more.
[0136] The negative electrode active material may include lithium titanium oxide. The lithium titanium oxide may include a material selected from the group consisting of Li4Ti5O 12 、Li7Ti5O 12 At least one of the group consisting of LiTi2O4. Furthermore, TiO2 may also be included.
[0137] As the negative electrode active material, an alloy material and a carbon material, or a lithium titanium oxide and a carbon material may be used in combination.
[0138] The shape and thickness of the negative electrode current collector can be selected based on the shape and range of the positive electrode current collector. Examples of metals constituting the negative electrode current collector include copper (Cu), nickel (Ni), iron (Fe), and alloys containing these metal elements.
[0139] The negative electrode may include a negative electrode current collector and a negative electrode mixture layer supported on the surface of the negative electrode current collector. The negative electrode mixture layer may be formed, for example, by applying a negative electrode slurry obtained by dispersing a negative electrode mixture in a dispersion medium to the surface of the negative electrode current collector and drying it. The dried coating may be rolled as required. The negative electrode mixture layer may be formed on one surface of the negative electrode current collector or on both surfaces. As a dispersion medium, for example, water or NMP is used.
[0140] The negative electrode mixture layer contains a negative electrode active material. The negative electrode mixture layer may further contain a binder, a conductive agent, a thickener, etc. As the binder and the conductive agent, the substances exemplified in the positive electrode can be used. In addition, the binder may also use a rubber material such as styrene-butadiene copolymer rubber (SBR). As a thickener, for example, carboxymethyl cellulose (CMC) and its modified bodies (Na salt, etc.) can be cited.
[0141] (Electrolyte)
[0142] The electrolyte solution includes a non-aqueous solvent and an electrolyte. The electrolyte solution may include a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the electrolyte solution may be, for example, 0.5 mol / liter or more and 2 mol / liter or less. By controlling the lithium salt concentration within the above range, an electrolyte solution having excellent ion conductivity and moderate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.
[0143] As the non-aqueous solvent, for example, cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates, etc. can be used. As cyclic carbonates, propylene carbonate (PC), ethylene carbonate (EC), etc. can be mentioned. Cyclic carbonates can include cyclic carbonates with unsaturated bonds of carbon-carbon such as fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), vinylene carbonate (VC), and vinyl ethylene carbonate. As chain carbonates, diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), etc. can be mentioned. As cyclic carboxylates, γ-butyrolactone (GBL), γ-valerolactone (GVL), etc. can be mentioned. As chain carboxylates, methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, etc. can be mentioned. The non-aqueous solvent can be used alone or in combination of two or more.
[0144] As the lithium salt, a known lithium salt can be used. Preferred lithium salts include LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiCF3CO2, LiAsF6, LiB 10 Cl 10 , lithium lower aliphatic carboxylates, LiCl, LiBr, LiI, borates, imide salts, etc. Examples of borates include lithium bis(1,2-benzenediolate (2-)-O,O')borate, lithium bis(2,3-naphthalenediolate (2-)-O,O')borate, lithium bis(2,2'-biphenylediolate (2-)-O,O')borate, and lithium bis(5-fluoro-2-olate-1-benzenesulfonic acid-O,O')borate. Examples of imide salts include lithium bis(fluorosulfonyl)imide (LiN(FSO2)2), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF3SO2)2), lithium trifluoromethanesulfonate nonafluorobutanesulfonyl imide (LiN(CF3SO2)(C4F9SO2)), and lithium bis(pentafluoroethanesulfonyl)imide (LiN(C2F5SO2)2). The lithium salt may be used alone or in combination of two or more.
[0145] (Separator 13)
[0146] Usually, it is preferred to sandwich a separator between the positive electrode and the negative electrode. The separator 13 has high ion permeability and has appropriate mechanical strength and insulation. As the separator 13, microporous films, woven fabrics, nonwoven fabrics, etc. can be used. As the material of the separator 13, for example, a polymer can be used. The polymer can be, for example, a polyolefin such as polypropylene and polyethylene.
[0147] In the secondary battery of the present disclosure, the electrolyte solution may be impregnated in a polymer provided as a separator, for example. That is, the secondary battery of the present disclosure may have a structure using both the electrolyte solution and the polymer.
[0148] The secondary battery of the present disclosure may further include a solid electrolyte as an electrolyte. That is, the secondary battery of the present disclosure may have a hybrid structure using an electrolyte and a solid electrolyte. Examples of solid electrolytes are halide solid electrolytes, sulfide solid electrolytes, oxide solid electrolytes, or organic polymer solid electrolytes. In the present disclosure, "halide solid electrolyte" refers to a solid electrolyte containing a halogen element as the main component in the anion. "Sulfide solid electrolyte" refers to a solid electrolyte containing sulfur as the main component in the anion. "Oxide solid electrolyte" refers to a solid electrolyte containing oxygen as the main component in the anion. The main component in the anion refers to the anion with the largest mass among all the anions constituting the solid electrolyte. The coating material in the secondary battery of the present disclosure may include a halide solid electrolyte.
[0149] The secondary battery of the present disclosure may not contain a solid electrolyte other than the solid electrolyte contained as a coating material. The secondary battery of the present disclosure may not contain a solid electrolyte as an electrolyte.
[0150] In the embodiment of the present disclosure, as an example of the structure of a secondary battery, Figure 1 The configuration example shown is a secondary battery 10 in which an electrode group in which a positive electrode and a negative electrode are wound with a separator and an electrolyte are housed in an outer body. However, the secondary battery involved in the present disclosure is not limited to this configuration example. The secondary battery involved in the present disclosure can be in any form, such as a cylindrical, square, coin-shaped, button-shaped, laminated, etc. In addition, as the electrode group in the secondary battery involved in the present disclosure, other forms of electrode groups, such as a laminated electrode group in which a positive electrode and a negative electrode are laminated with a separator, can also be used instead of the wound electrode group.
[0151] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0152] Example
[0153] (Example 1)
[0154] [Production of positive electrode]
[0155] In an argon atmosphere, LiF, TiF4 and AlF3 as raw material powders were weighed to a molar ratio of LiF:TiF4:AlF3=2.7:0.3:0.7. Then, a planetary ball mill (manufactured by Fritsch GmbH, P-7 model) was used to grind the powder at 500 rpm for 12 hours to obtain LiF.2.7 Ti 0.3 Al 0.7 The powder of F6 was used as the coating material in Example 1.
[0156] Weigh the layered rock salt type LiNi as the positive electrode active material 0.6 Co 0.2 Mn 0.2 The composite oxide particles (average particle size (D50) 5 μm) and Li 2.7 Ti 0.3 Al 0.7 F6, makes it NCM: Li 2.7 Ti 0.3 Al 0.7 F6 = mass ratio of 100:3. These materials were charged into a dry particle compounding device NOBILTA (manufactured by Hosokawa Micron) and subjected to compounding treatment at 6000 rpm for 30 minutes to obtain a positive electrode active material whose surface was coated with the coating material.
[0157] Next, the positive electrode active material coated with the coating material, acetylene black (AB) and polyvinylidene fluoride (PVDF) were mixed at a mass ratio of coated positive electrode active material: AB: PVDF = 90:7:3 to prepare a positive electrode mixture. N-methyl-2-pyrrolidone (NMP) was added to the positive electrode mixture and stirred to prepare a positive electrode slurry.
[0158] The positive electrode slurry is applied to the surface of the aluminum foil, and after the coating is dried, it is rolled to form a positive electrode mixture layer. The positive electrode mixture layer is formed on one side of the aluminum foil.
[0159] [Production of negative electrode]
[0160] Lithium titanate, acetylene black (AB) and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of lithium titanate:AB:PVDF=90:7:3 to prepare a negative electrode mixture. N-methyl-2-pyrrolidone (NMP) was added to the negative electrode mixture and stirred to prepare a negative electrode slurry.
[0161] The negative electrode slurry is applied to the surface of the aluminum foil, and after the coating is dried, it is rolled to form a negative electrode mixture layer. The negative electrode mixture layer is formed on one side of the aluminum foil.
[0162] [Preparation of electrolyte]
[0163] LiPF6 was dissolved in a mixed solvent of fluoroethylene carbonate (FEC) and dimethyl carbonate (DMC) at a volume ratio of FEC:DMC=2:8 to obtain an electrolyte solution. The concentration of LiPF6 in the electrolyte solution was 1 mol / liter.
[0164] [Manufacturing of Secondary Batteries]
[0165] The positive electrode obtained above was equipped with an Al positive electrode lead. The negative electrode obtained above was equipped with an Al negative electrode lead. In a low dew point atmosphere of -50°C, the positive electrode and the negative electrode were spirally wound with a separator of a polyethylene film interposed therebetween to prepare a wound electrode group.
[0166] The electrode group was housed in a bag-shaped outer casing formed of a laminate sheet having an Al layer, and after the above-mentioned electrolyte was injected, the outer casing was sealed. When the electrode group was housed in the outer casing, a portion of the positive electrode lead and a portion of the negative electrode lead were exposed to the outside from the outer casing. In this way, the battery of Example 1 was obtained.
[0167] (Comparative Example 1)
[0168] In Comparative Example 1, no coating material was used in the preparation of the positive electrode. That is, the positive electrode active material was not coated with the coating material, and the positive electrode active material, acetylene black (AB) and polyvinylidene fluoride (PVDF) were mixed at a mass ratio of positive electrode active material: AB: PVDF = 90:7:3 to prepare a positive electrode mixture. Except for the above, the battery of Comparative Example 1 was prepared by the same method as Example 1.
[0169] [Evaluation 1: Charge and discharge capacity]
[0170] (1) Charge and discharge
[0171] Using the batteries of Example 1 and Comparative Example 1, a charge and discharge test was performed as follows. After constant current charging at a current of 0.2C until the voltage reached 2.75V, constant voltage charging was performed at a voltage of 2.75V until the current reached 0.05C. Then, constant current discharge was performed at a current of 0.2C until the voltage reached 0.95V. The pause time between charging and discharging was set to 60 minutes. Charging and discharging were performed at 25°C. The above-mentioned charging and discharging was regarded as one cycle and a cycle test was performed.
[0172] Figure 2 It is a graph showing the charge and discharge curves of the batteries of Example 1 and Comparative Example 1 in the first cycle. Figure 3 It is a graph showing the charge and discharge curves of the batteries of Example 1 and Comparative Example 1 at the 50th cycle.
[0173] (2) Measurement of discharge capacity change with cycling
[0174] In the cycle test, the change in discharge capacity up to 52 cycles was measured. Figure 4 This is a graph showing the transition of the discharge capacity of the batteries of Example 1 and Comparative Example 1.
[0175] [Evaluation 2: Measurement of internal resistance at the 3rd cycle and the 50th cycle]
[0176] The batteries of Example 1 and Comparative Example 1 were charged to SOC 50% after the 3rd and 50th cycles of charge and discharge, and the voltage drop ΔV at the start of constant current discharge at a current I of 0.3 C was measured. ΔV / I was calculated as the internal resistance.
[0177] Table 1 shows the relative values of the internal resistances of Example 1 and Comparative Example 1 after 3 cycles and after 50 cycles, assuming that the internal resistance of the battery of Example 1 after 3 cycles is 1.
[0178] [Table 1]
[0179] Internal resistance after 3 cycles Internal resistance after 50 cycles Example 1 1.00 1.30 Comparative Example 1 1.05 1.71
[0180] In Example 1, a higher discharge capacity than that of Comparative Example 1 was obtained, and even after 50 cycles, a higher discharge capacity than that of Comparative Example 1 was maintained. In addition, by measuring the internal resistance, Example 1 had a lower internal resistance than Comparative Example 1. It is speculated that this result indicates that the discharge capacity of Example 1 is higher than that of Comparative Example 1. In addition, even when the resistance after 50 cycles increases, Example 1 is less than Comparative Example 1. It is speculated that this indicates that the discharge capacity is maintained.
[0181] Industrial Applicability
[0182] The secondary battery of the present disclosure is suitable for use as a power source for mobile devices such as smartphones, a power source for vehicles such as electric cars, and a storage device for natural energy such as solar energy.
Claims
1. A secondary battery comprising a positive electrode, a negative electrode and an electrolyte, The positive electrode comprises a positive electrode active material and a coating material covering at least a portion of a surface of the positive electrode active material. The coating material comprises Li, Ti, M1 and X, M1 is at least one selected from the group consisting of Be, Mg, Ca, Sr, Ba, Sc, Y, Al, Ga, In, Zr and Sn, X is at least one selected from the group consisting of F, Cl, Br and I, The electrolyte solution includes an electrolyte and a non-aqueous solvent.
2. The secondary battery according to claim 1, wherein X contains F.
3. The secondary battery according to claim 1 or 2, wherein: The coating material comprises a material represented by the following composition formula (2), Li 6-(4-a)b (Ti 1-a M1 a ) b X6……Formula (2) Here, 0<a<1 and 0<b≤2 are satisfied.
4. The secondary battery according to any one of claims 1 to 3, wherein In the coating material, the ratio of the amount of Li to the total amount of Ti and M1 is 0.5 or more and 4.5 or less.
5. The secondary battery according to any one of claims 1 to 4, wherein M1 is Al.
6. The secondary battery according to any one of claims 1 to 5, wherein The coating material covers more than 80% of the surface of the positive electrode active material.
7. The secondary battery according to claim 6, wherein The coating material covers 95% or more of the surface of the positive electrode active material.
8. The secondary battery according to any one of claims 1 to 7, wherein The positive electrode active material includes a composite oxide containing lithium and a transition metal.
9. The secondary battery according to claim 8, wherein The composite oxide has a composition represented by the following composition formula (3), LiNi x1 Co y1 M2 1-x1-y1 O2…Formula (3) Here, 0≤x1<1, 0≤y1≤1, and 0≤1-x1-y1≤0.35 are satisfied, and M2 is at least one selected from the group consisting of Al and Mn.
10. The secondary battery according to claim 8, wherein The composite oxide has a composition represented by the following composition formula (4), LiNi x2 M3 1-x2 O2…Formula (4) Here, 0.3≤x2<1 is satisfied, and M3 is at least one selected from the group consisting of Co, Mn, Al, Ti, and Fe.
11. The secondary battery according to claim 8, wherein The composite oxide has a composition represented by the following composition formula (5), Li x3 M4 y3 (PO4) z3 …Formula (5) Here, 2.7≤x3≤3.3, 0.9≤y3≤2.2, and 0.9≤z3≤3.3 are satisfied, and M4 is at least one selected from the group consisting of Ni, Co, Mn, Fe, and V.
12. The secondary battery according to any one of claims 1 to 11, wherein The secondary battery does not contain a solid electrolyte other than the solid electrolyte contained as the covering material.
Citation Information
Cited By
Positive electrode material, pole piece and secondary battery
CN119673988A
Positive electrode active material, secondary battery, and electric device
CN120895642A