Secondary battery and electric device
By employing a specially designed separator and negative electrode material layer in lithium-ion batteries, the problem of balancing cycle performance, safety performance, and energy density has been solved, achieving a comprehensive improvement in battery performance.
Patent Information
- Application Number
- CN202410939379.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
Existing lithium-ion batteries face the challenge of balancing cycle performance, safety performance, and energy density, especially in separator design where it is difficult to simultaneously improve electrolyte absorption capacity, structural stability, and adhesion.
The electrode assembly employs a wound structure and utilizes two membranes with different properties: the first membrane consists of two ceramic coating layers and one adhesive layer, and the second membrane consists of two adhesive layers and one ceramic coating layer. These membranes leverage their respective advantages in the corner and straight areas to improve electrolyte absorption capacity and structural stability. Combined with the coating and doping elements of the negative electrode material layer, the length and porosity of the material layer are optimized, and the coating weight and pore size are controlled.
It achieves a balance between cycle performance, safety performance and energy density in lithium-ion batteries, improving the overall performance of the battery, especially in terms of electrolyte absorption and interface stability.
Smart Images

Figure CN118899618A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electrical device. Background Art
[0002] Secondary batteries, such as lithium-ion batteries, have the advantages of high energy density, long cycle life, low self-discharge rate and environmental protection, and have been widely used in aviation, aerospace, navigation, electric vehicles and other fields. The performance of the diaphragm in lithium-ion batteries determines the interface structure, internal resistance, etc. of lithium-ion batteries, and directly affects the capacity, cycle and safety performance of lithium-ion batteries. Diaphragms with excellent performance play an important role in improving the comprehensive performance of lithium-ion batteries. At present, when improving the performance of lithium-ion batteries through diaphragms, its cycle performance, safety performance and energy density are usually difficult to take into account. Summary of the invention
[0003] The purpose of the present application is to provide a secondary battery and an electrical device that take into account the cycle performance, safety performance and energy density of the secondary battery.
[0004] It should be noted that in the invention content of this application, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solutions are as follows:
[0005] The first aspect of the present application provides a secondary battery, which includes an electrode assembly of a winding structure, the electrode assembly includes a positive electrode sheet, a negative electrode sheet, a first separator and a second separator, the negative electrode sheet is located between the first separator and the second separator, and the electrode assembly includes a straight area and a corner area. The negative electrode sheet includes a negative electrode collector and a first negative electrode material layer and a second negative electrode material layer located on both sides of the thickness direction of the negative electrode collector, the first separator is adjacent to the first negative electrode material layer, and the second separator is adjacent to the second negative electrode material layer. The first separator in the corner area includes a first base film, a first bonding layer and a first ceramic coating, the first bonding layer is arranged on the side of the first base film away from the first negative electrode material layer, the first ceramic coating is arranged on both sides of the first base film, the first ceramic coating is located between the first base film and the first bonding layer, and one layer of the first ceramic coating is in direct contact with the first negative electrode material layer. The second separator in the corner area includes a second base film, a second bonding layer and a second ceramic coating, the second bonding layer is arranged on both sides of the second base film, the second ceramic coating is arranged on the side of the second base film away from the second negative electrode material layer, and the second ceramic coating is located between the second base film and the second bonding layer. In the corner area, a positive electrode sheet corner section is adjacent to a first negative electrode material layer corner section, the positive electrode sheet corner section is farther away from the winding center of the electrode assembly than the first negative electrode material layer corner section, the first diaphragm is located between the positive electrode sheet corner section and the first negative electrode material layer corner section, and the positive electrode sheet corner section is in contact with the first adhesive layer. The secondary battery of the present application uses the first diaphragm and the second diaphragm in combination, each of which has different advantages, so that the cycle performance, safety performance and energy density of the secondary battery can be taken into account.
[0006] In some embodiments of the present application, along the winding direction of the electrode assembly, the length of the first negative electrode material layer is greater than the length of the second negative electrode material layer. In the secondary battery of the present application, the first diaphragm includes two layers of first ceramic coating and one layer of first bonding layer, and its performance of absorbing and storing electrolyte is better than that of the second diaphragm. The first diaphragm is adjacent to the first negative electrode material layer and the length of the first negative electrode material layer is greater than that of the second negative electrode material layer, which is conducive to the negative electrode sheet of the secondary battery absorbing more electrolyte and reducing the risk of cycle bridge failure.
[0007] In some embodiments of the present application, the first negative electrode material layer includes a first negative electrode active material, the surface of the particles of the first negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage content W1 of the coating element is 0.05% to 0.5% based on the mass of the first negative electrode material layer. The cycle performance of the secondary battery is further improved, and both safety performance and energy density can be taken into account.
[0008] In some embodiments of the present application, the second negative electrode material layer includes a second negative electrode active material, the surface of the particles of the second negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and based on the mass of the second negative electrode material layer, the mass percentage content W2 of the coating element is 0.05% to 0.5%. The cycle performance of the secondary battery is further improved, and the safety performance and energy density can be taken into account.
[0009] In some embodiments of the present application, the first negative electrode material layer includes a first negative electrode active material, the first negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and based on the mass of the first negative electrode material layer, the mass percentage content W1' of the doping element is 0.05% to 0.5%. The cycle performance of the secondary battery is further improved, and the safety performance and energy density can be taken into account.
[0010] In some embodiments of the present application, the second negative electrode material layer includes a second negative electrode active material, the second negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and based on the mass of the second negative electrode material layer, the mass percentage content W2' of the doping element is 0.05% to 0.5%. The cycle performance of the secondary battery is further improved, and the safety performance and energy density can be taken into account.
[0011] In some embodiments of the present application, the first negative electrode active material and the second negative electrode active material each independently include natural graphite, artificial graphite, mesophase microbeads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x 、Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O 12 、Li-Al alloy or metallic lithium, where 0 < x < 2. By selecting the above first negative electrode active material and second negative electrode active material and including the above coating element or doping element, the cycle performance of the secondary battery can be further improved, and by using the first separator and the second separator in the present application in combination, the cycle performance, safety performance and energy density of the secondary battery can be better taken into account.
[0012] In some embodiments of the present application, the positive electrode tab includes a positive electrode current collector and a first positive electrode material layer and a second positive electrode material layer located on both sides in the thickness direction of the positive electrode current collector. In the same winding layer, the first positive electrode material layer is closer to the winding center of the electrode assembly than the second positive electrode material layer, and at the winding end of the electrode assembly, the length of the first positive electrode material layer is greater than the length of the second positive electrode material layer.
[0013] In some embodiments of the present application, the porosity P1 of the first base film is greater than the porosity P2 of the second base film, 40% ≤ P1 ≤ 70%, 5% ≤ P2 ≤ 50%. In some embodiments of the present application, 50% ≤ P1 ≤ 60%, 10% ≤ P2 ≤ 40%. The first base film has a higher porosity, which can further improve the cycle performance of the secondary battery. At the same time, by regulating the porosity P1 of the first base film and the porosity P2 of the second base film within the scope of the present application, the mechanical strength of the first diaphragm and the second diaphragm is high, and the secondary battery obtained also has good safety performance.
[0014] In some embodiments of the present application, the pore size D1 of the first base membrane is larger than the pore size D2 of the second base membrane, 80nm≤D1≤700nm, 50nm≤D2≤200nm. In some embodiments of the present application, 250nm≤D1≤520nm, 100nm≤D2≤150nm. The first base membrane has a larger pore size, which can further improve the cycle performance of the secondary battery. At the same time, by regulating the pore size D1 of the first base membrane and the pore size D2 of the second base membrane within the scope of the present application, the mechanical strength of the first diaphragm and the second diaphragm is high, and the secondary battery obtained also has good safety performance.
[0015] In some embodiments of the present application, the coating weight of the first ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 , and / or, the coating weight of the first adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 By regulating the coating weight of the first ceramic coating and / or the coating weight of the first adhesive layer within the above range, the first separator has high liquid retention capacity and good structural stability and adhesion, which is conducive to further improving the cycle performance of the secondary battery and taking into account safety performance and energy density.
[0016] In some embodiments of the present application, the coating weight of the second ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 , and / or, the coating weight of the second adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 By regulating the coating weight of the second ceramic coating and / or the coating weight of the second adhesive layer within the above range, the second separator has high structural stability and adhesion and good liquid retention capacity, which is conducive to further improving the safety performance and energy density of the secondary battery while taking into account the cycle performance.
[0017] In some embodiments of the present application, the first adhesive layer includes a first adhesive, the second adhesive layer includes a second adhesive, and the first adhesive and the second adhesive each independently include at least one of polyvinylidene fluoride, polyacrylonitrile, polyethylene oxide or polyimide. By selecting the first adhesive and the second adhesive of the above type, it is beneficial to improve the bonding force between the first diaphragm and the positive electrode plate, between the first diaphragm and the negative electrode plate, between the second diaphragm and the positive electrode plate, and between the second diaphragm and the negative electrode plate, strengthen the interface between the above two, facilitate the transmission of lithium ions, and improve the cycle performance of the secondary battery; at the same time, the possibility of the first ceramic coating and the second ceramic coating falling off is reduced, and the thickness of the secondary battery is reduced, that is, the energy density of the secondary battery is improved.
[0018] In some embodiments of the present application, the first ceramic coating includes first ceramic particles, the second ceramic coating includes second ceramic particles, and the first ceramic particles and the second ceramic particles each independently include at least one of aluminum oxide, boehmite, silicon oxide, magnesium oxide, titanium oxide, tin oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, aluminum hydroxide, magnesium hydroxide, or calcium hydroxide. The type of the first ceramic particles in the first ceramic coating and the type of the second ceramic particles in the second ceramic coating are within the scope of the present application, which can further improve the liquid retention capacity of the first diaphragm and the second diaphragm, improve the interface problem caused by insufficient electrolyte between the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery.
[0019] In some embodiments of the present application, the mass percentage of the first ceramic particles is 10% to 50% based on the mass of the first ceramic coating; the mass percentage of the second ceramic particles is 10% to 50% based on the mass of the second ceramic coating. The mass percentage of the first ceramic particles in the first ceramic coating and the mass percentage of the second ceramic particles in the second ceramic coating are regulated within the above ranges, so that the first ceramic particles and the first ceramic particles can fully play their respective roles, and the first diaphragm and the second diaphragm with good liquid storage capacity and wetting performance are obtained, which are applied to secondary batteries, which is conducive to making the secondary batteries have good cycle performance, while taking into account the energy density and safety performance of the secondary batteries.
[0020] In some embodiments of the present application, the thickness H1 of the first separator is 7.5 μm to 15.0 μm, and the thickness H2 of the second separator is 6.0 μm to 13.0 μm. By adjusting the thickness H1 of the first separator and the thickness H2 of the second separator within the above range, the secondary battery obtained has a high energy density while taking into account both cycle performance and safety performance.
[0021] A second aspect of the present application provides an electrical device, which includes the secondary battery in any of the aforementioned embodiments.
[0022] Beneficial effects of this application:
[0023] The present application provides a secondary battery and an electric device, wherein the secondary battery comprises an electrode assembly of a winding structure, the electrode assembly comprises a positive electrode sheet, a negative electrode sheet, a first diaphragm and a second diaphragm, the negative electrode sheet is located between the first diaphragm and the second diaphragm, the electrode assembly comprises a straight area and a corner area, the negative electrode sheet comprises a first negative electrode material layer and a second negative electrode material layer, the first diaphragm in the corner area comprises a first base film, a first bonding layer and a first ceramic coating, the first bonding layer is arranged on the side of the first base film away from the first negative electrode material layer, the first ceramic coating is arranged on both sides of the first base film, and the first ceramic coating is located between the first base film and the first bonding layer; the second diaphragm in the corner area comprises a second base film, a second bonding layer and a second ceramic coating, the second bonding layer is arranged on both sides of the second base film, the second ceramic coating is arranged on the side of the second base film away from the second negative electrode material layer, and the second ceramic coating is located between the second base film and the second bonding layer. The secondary battery is used in combination with the first diaphragm and the second diaphragm, each of which plays a different role, so that the cycle performance, safety performance and energy density of the secondary battery can be taken into account.
[0024] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.
[0026] Figure 1 A schematic diagram of the cross-sectional structure of a wound structure electrode assembly wound along the W direction in one embodiment of the present application along its own thickness direction;
[0027] Figure 2 for Figure 1 A partial enlarged view of the middle A;
[0028] Figure 3 This is a schematic diagram of the cross-sectional structure of an electrode assembly in an embodiment of the present application after it is unfolded along its thickness direction;
[0029] Figure 4 This is a schematic diagram of the cross-sectional structure of an electrode assembly along its thickness direction after it is unfolded in another embodiment of the present application. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0031] It should be noted that in the specific implementation manner of the present application, the present application is explained by taking a lithium-ion battery as an example of a secondary battery, but the secondary battery of the present application is not limited to a lithium-ion battery.
[0032] The first aspect of the present application provides a secondary battery, which includes an electrode assembly of a wound structure. Specifically, Figure 1 As shown, the electrode assembly 100 is a wound structure, and the electrode assembly 100 includes a first separator 10, a second separator 20, a negative electrode plate 30 and a positive electrode plate 40. The electrode assembly 100 also includes a straight area 102 and a corner area 101. In the present application, the straight area refers to the straight part of the electrode assembly, and the corner area refers to the curved part of the electrode assembly.
[0033] like Figure 2 and Figure 3As shown, the electrode assembly 100 includes a first separator 10, a second separator 20, a negative electrode plate 30 and a positive electrode plate 40, wherein the negative electrode plate 30 is located between the first separator 10 and the second separator 20. The negative electrode plate 30 includes a negative electrode current collector 31 and a first negative electrode material layer 32 and a second negative electrode material layer 33 located on both sides of the negative electrode current collector 31 in the thickness direction, wherein the first separator 10 is adjacent to the first negative electrode material layer 32, and the second separator 20 is adjacent to the second negative electrode material layer 33. The first separator 10 in the corner area 101 includes a first base film 11, a first bonding layer 12 and a first ceramic coating 13. The first bonding layer 12 is arranged on the side of the first base film 11 away from the first negative electrode material layer 32, the first ceramic coating 13 is arranged on both sides of the first base film 11, and the first ceramic coating 13 is located between the first base film 11 and the first bonding layer 12, that is, the first separator 10 includes a first bonding layer 12 and two first ceramic coatings 13; and one of the first ceramic coatings 13 is in direct contact with the first negative electrode material layer 32. The second separator 20 in the corner area 101 includes a second base film 21, a second bonding layer 22 and a second ceramic coating 23. The second bonding layer 22 is arranged on both sides of the second base film 21, the second ceramic coating 23 is arranged on the side of the second base film 21 away from the second negative electrode material layer 33, and the second ceramic coating 23 is located between the second base film 21 and the second bonding layer 22, that is, the second separator 20 includes two second bonding layers 22 and a second ceramic coating 23. The positive electrode sheet 40 includes a positive electrode current collector 41 and positive electrode material layers disposed on both surfaces of the positive electrode current collector 41, and the positive electrode material layers include a first positive electrode material layer 42 and a second positive electrode material layer 43. In the corner area 101, a corner section of a positive electrode sheet 40 is adjacent to a corner section of a first negative electrode material layer 32, the corner section of the positive electrode sheet 40 is farther from the winding center of the electrode assembly 100 than the corner section of the first negative electrode material layer 32, the first separator 10 is located between the corner section of the positive electrode sheet 40 and the corner section of the first negative electrode material layer 32, and the corner section of the positive electrode sheet 40 is in contact with the first bonding layer 12.
[0034] The ceramic coating in the existing diaphragm usually has good wettability and liquid absorption and retention capabilities, which can improve the cycle performance of the secondary battery; however, the ceramic particles in the ceramic coating are relatively hard, which causes greater wear on the machine and high equipment costs. In addition, the ceramic particles are heavy and not flame retardant, which is not conducive to the energy density and safety of the secondary battery. The bonding layer in the diaphragm has good adhesion, which can inhibit the thermal shrinkage of the base film, improve the structural stability of the diaphragm, and reduce the risk of short circuit between the positive and negative pole pieces, which is beneficial to improving the safety performance of the secondary battery; and the thickness of the bonding layer is usually smaller than that of the ceramic coating, which is beneficial to the energy density of the secondary battery; but the bonding layer will reduce the gap between adjacent layers, which increases the risk of electrolyte bridge breaking in the corner area, which is not conducive to the cycle performance of the secondary battery.
[0035] The inventors have found that the corner area 101 is prone to electrolyte shortage and even electrolyte bridge failure, thereby affecting the cycle performance of the secondary battery. However, when improving the cycle performance of the corner area 101, the safety performance and energy density of the secondary battery are usually affected. The present application can effectively give play to the advantages of each layer by selecting the above-mentioned first diaphragm 10 and the second diaphragm 20 for use, thereby taking into account the cycle performance, safety performance and energy density of the secondary battery. Specifically, the first diaphragm 10 includes two layers of first ceramic coating 13 and a first bonding layer 12, which has a high liquid retention capacity, and the wettability of the adjacent positive electrode sheet 40 and negative electrode sheet 30 is improved, so that the positive electrode sheet 40 and the negative electrode sheet 30 in the corner area 101 are not prone to interface problems caused by insufficient electrolyte, so that the cycle performance of the secondary battery is improved; and the setting of a first bonding layer 12 can also take into account the structural stability and bonding of the first diaphragm 10. At the same time, the second diaphragm 20 includes two layers of second bonding layers 22 and a layer of second ceramic coating 23, which has good structural stability and adhesion, can inhibit the thermal shrinkage of the second base film 21, and improve the safety performance of the secondary battery; and the thickness of the bonding layer is usually small, which is more conducive to improving the energy density of the secondary battery; the setting of a layer of first ceramic coating 23 can also take into account the liquid retention capacity of the second diaphragm 20. In addition, the first negative electrode material layer 32 is closer to the outside of the electrode assembly 100 than the second negative electrode material layer 33. The first negative electrode material layer 32 located on the outside of the corner area 101 is wrapped by the positive electrode plate 40. The winding radius of the positive electrode plate 40 is larger than the winding radius of the first negative electrode material layer 32. The positive-negative electrode ratio (Cell Balance, CB, the ratio of the negative electrode capacity per unit area to the positive electrode capacity per unit area) at the first negative electrode material layer 32 is smaller. The side of the first negative electrode material layer 32 is more prone to lithium deposition, and is more prone to interface problems than the side of the second negative electrode material layer 33 on the inside. Based on this, setting a first diaphragm 10 with high liquid retention capacity adjacent to the first negative electrode material layer 32 is more conducive to improving the interface problems in the corner area 101. At the same time, since the first separator 10 with high liquid retention capacity but relatively low adhesion is used on one side of the first negative electrode material layer 32, in order to prevent the overall adhesion of the electrode assembly 100 from decreasing, the second separator 20 with high structural stability and good adhesion is arranged adjacent to the second negative electrode material layer 33, so that the electrode assembly 100 has good adhesion as a whole. Therefore, the first separator 10 and the second separator 20 with different characteristics are used in combination in the corner area 101 of the electrode assembly 100, each of which plays a different role, so that the cycle performance, safety performance and energy density of the secondary battery can be taken into account.
[0036] In some embodiments of the present application, Figure 3As shown, along the winding direction W of the electrode assembly 100, the length of the first negative electrode material layer 32 is greater than the length of the second negative electrode material layer 33. In addition, along the winding direction W, one end of the first negative electrode material layer 32 and the second negative electrode material layer 33 are flush, and at the other end, the extension length of the first negative electrode material layer 32 is longer than that of the second negative electrode material layer 33. It can be understood that when the length of the first negative electrode material layer 32 is greater than the length of the second negative electrode material layer 33, it can also be that the extension length of the first negative electrode material layer 32 at one end along the winding direction W and the other end opposite to the winding direction W is longer than that of the second negative electrode material layer 33. The reason for this arrangement is that when the first separator 10 is located on one side of the first negative electrode material layer 32 of the negative electrode plate 30, it is beneficial for the negative electrode plate 30 of the secondary battery to absorb more electrolyte, thereby reducing the risk of lithium deposition at the interface between the electrolyte and the negative electrode plate 30 due to electrolyte bridge breakage in the late cycle of the secondary battery. The present application has no particular limitation on the length difference between the first negative electrode material layer and the second negative electrode material layer, and it can be selected according to the specific situation as long as the purpose of the present application can be achieved.
[0037] In some embodiments of the present application, the first negative electrode material layer includes a first negative electrode active material, the surface of the particles of the first negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage content W1 of the coating element is 0.05% to 0.5% based on the mass of the first negative electrode material layer. For example, W1 can be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.5% or a range consisting of any two values therebetween. The first negative electrode active material contains the above-mentioned coating element and regulates its content within the above-mentioned range. On the one hand, the conductive network on the surface of the first negative electrode active material particle is more compact and has better kinetic performance; on the other hand, the specific surface area of the first negative electrode active material can be reduced, and the side reaction between the first negative electrode active material and the electrolyte can be reduced; on the other hand, it is conducive to forming a passivation film on the surface of the first negative electrode active material particle, thereby improving its first effect and reversible capacity. Therefore, the use of the above-mentioned first negative electrode active material is more conducive to improving the interface problem of the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery, and the combination of the first diaphragm and the second diaphragm in this application can better take into account the cycle performance, safety performance and energy density of the secondary battery.
[0038] In some embodiments of the present application, the second negative electrode material layer includes a second negative electrode active material, and the surface of the particles of the second negative electrode active material includes a coating element, and the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage content W2 of the coating element is 0.05% to 0.5% based on the mass of the second negative electrode material layer. For example, W2 can be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.5% or a range consisting of any two values therebetween. The second negative electrode active material contains the above-mentioned coating element and regulates its content within the above-mentioned range. On the one hand, the conductive network on the surface of the second negative electrode active material particles is more compact and has better kinetic performance; on the other hand, the specific surface area of the second negative electrode active material can be reduced, and the side reaction between the second negative electrode active material and the electrolyte can be reduced; on the other hand, it is conducive to the formation of a passivation film on the surface of the second negative electrode active material particles, thereby improving its first effect and reversible capacity. Therefore, the use of the above-mentioned second negative electrode active material is more conducive to improving the interface problem of the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery, and the combination of the first diaphragm and the second diaphragm in this application can better take into account the cycle performance, safety performance and energy density of the secondary battery.
[0039] In some embodiments of the present application, the first negative electrode material layer includes a first negative electrode active material, the first negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and based on the mass of the first negative electrode material layer, the mass percentage content W1' of the doping element is 0.05% to 0.5%. For example, W1' can be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.5% or a range consisting of any two values therebetween. The first negative electrode active material contains the above-mentioned doping element and regulates its content within the above-mentioned range. On the one hand, the conductive network of the first negative electrode active material particles as a whole is more compact and has better kinetic performance; on the other hand, it is conducive to reducing the side reaction between the first negative electrode active material and the electrolyte. Therefore, the use of the above-mentioned first negative electrode active material is more conducive to improving the interface problems between the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery. Moreover, the combined use of the first diaphragm and the second diaphragm in the present application can better take into account the cycle performance, safety performance and energy density of the secondary battery.
[0040] In some embodiments of the present application, the second negative electrode material layer includes a second negative electrode active material, the second negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu, or Ni, and based on the mass of the second negative electrode material layer, the mass percentage content W2' of the doping element is 0.05% to 0.5%. For example, W2' can be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.5%, or any range composed of any two values therebetween. The second negative electrode active material contains the above doping element and regulates its content within the above range. On the one hand, the overall conductive network of the second negative electrode active material particles is denser and the kinetic performance is better; on the other hand, the side reaction between the second negative electrode active material and the electrolyte is reduced. Therefore, using the above second negative electrode active material is more conducive to improving the interface problem between the positive electrode sheet and the negative electrode sheet in the corner area, thereby further improving the cycle performance of the secondary battery. Moreover, by combining the first separator and the second separator in the present application, the cycle performance, safety performance, and energy density of the secondary battery can be better balanced.
[0041] In some embodiments of the present application, the first negative electrode active material and the second negative electrode active material each independently include natural graphite, artificial graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x , Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O 12 , Li-Al alloy, or metallic lithium, where 0 < x < 2. By selecting the above first negative electrode active material and the second negative electrode active material and containing the above coating element or doping element, it is more conducive to improving the interface problem between the positive electrode sheet and the negative electrode sheet in the corner area, thereby further improving the cycle performance of the secondary battery. Moreover, by combining the first separator and the second separator in the present application, the cycle performance, safety performance, and energy density of the secondary battery can be better balanced.
[0042] In the present application, natural graphite, artificial graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x , Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O 12 , Li-Al alloy, or metallic lithium containing the above coating element, and natural graphite, artificial graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x , Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O 12, Li-Al alloy or metallic lithium, all of which can be purchased, and the mass percentage of the coating element or doping element in the negative electrode active material can be tested by the following test method, and the required negative electrode active material can be selected so that W1, W2, W1', W2' are within the above range.
[0043] The types of coating elements or doping elements in the first negative electrode active material can be tested in the following way: weigh a certain amount of the first negative electrode active material, and then use a scanning electron microscope combined with an energy spectrometer to test to obtain the types of coating elements and doping elements in the first negative electrode material layer. When the element is mainly distributed on the surface of the first negative electrode active material particles, the corresponding element is a coating element; when the element is mainly dispersed inside the first negative electrode active material particles, the corresponding element is a doping element. Thus, the types of coating elements or doping elements in the first negative electrode material layer are obtained. Replace the first negative electrode material layer in the above steps with the second negative electrode material layer, and the types of coating elements or doping elements in the second negative electrode material layer can be obtained.
[0044] The mass percentage of the coating element or the mass percentage of the doping element in the first negative electrode active material can be tested in the following manner: weigh a certain amount of the first negative electrode active material, add concentrated nitric acid for microwave digestion to obtain a solution, wash the obtained solution and filter residue multiple times and adjust the volume, test the plasma intensity of the doping element or coating element therein by inductively coupled plasma emission spectrometer (ICP-OES), calculate the content of the doping element or coating element in the solution according to the standard curve of the measured element, and thus calculate the mass percentage of the doping element or coating element in the first negative electrode active material. Replace the first negative electrode active material with the second negative electrode active material, and then the mass percentage of the coating element or the mass percentage of the doping element in the second negative electrode active material can be measured.
[0045] Generally, when other conditions remain unchanged, the mass percentage of the coating element in the first negative electrode active material layer can be adjusted by changing the mass percentage of the coating element in the first negative electrode active material. For example, by increasing the mass percentage of the coating element in the first negative electrode active material, the mass percentage of the coating element in the first negative electrode material layer increases; by decreasing the mass percentage of the coating element in the first negative electrode active material, the mass percentage of the coating element in the first negative electrode material layer decreases. The mass percentage of the coating element in the second negative electrode material layer can be adjusted in the same manner.
[0046] Generally, when other conditions remain unchanged, the mass percentage of the doping element in the first negative electrode active material layer can be regulated by changing the mass percentage of the doping element in the first negative electrode active material. For example, by increasing the mass percentage of the doping element in the first negative electrode active material, the mass percentage of the doping element in the first negative electrode material layer increases; by decreasing the mass percentage of the doping element in the first negative electrode active material, the mass percentage of the doping element in the first negative electrode material layer decreases. The mass percentage of the doping element in the second negative electrode material layer can be regulated in the same manner.
[0047] In some embodiments of the present application, Figure 3 and Figure 4 As shown, the positive electrode sheet 40 includes a positive electrode current collector 41 and a first positive electrode material layer 42 and a second positive electrode material layer 43 located on both sides of the positive electrode current collector 41 in the thickness direction. Figure 3 As shown, along the winding direction W of the electrode assembly 100, the length of the first positive electrode material layer 42 is equal to the length of the second positive electrode material layer 43. Figure 4 As shown, at the winding end of the electrode assembly 100, the length of the first positive electrode material layer 42 is greater than the length of the second positive electrode material layer 43, and the second positive electrode material 43 is farther away from the winding center of the electrode assembly 100 than the first positive electrode material layer 42. Figure 4 As shown, along the winding direction W, one end of the first positive electrode material layer 42 and the second positive electrode material layer 43 are flush, and at the other end, the extension length of the first positive electrode material layer 42 is longer than the extension length of the second positive electrode material layer 43, wherein the other end is the winding end of the positive electrode sheet. The present application has no particular restriction on the difference in length between the first positive electrode material layer and the second positive electrode material layer, and it can be selected according to the specific situation, as long as the purpose of the present application can be achieved. By setting the length of the first positive electrode material layer to be longer than the length of the second positive electrode material layer, as shown in FIG. Figure 1 As described above, at the outermost side of the wound structure of the electrode assembly 100, a section of the positive electrode sheet 40 is coated on one side, that is, the first positive electrode material layer 42 is provided only on one side in the thickness direction of the positive electrode collector 41. This is mainly for the sake of saving negative electrode active materials and the similar potential between the positive electrode collector 41 and the aluminum-plastic film of the secondary battery packaging bag (not shown in the figure), so as to prevent electrochemical corrosion of the aluminum-plastic film of the packaging bag.
[0048] In some embodiments of the present application, the porosity P1 of the first base film is greater than the porosity P2 of the second base film, 40%≤P1≤70%, 5%≤P2≤50%. In some embodiments of the present application, 50%≤P1≤60%, 10%≤P2≤40%. For example, P1 can be 40%, 45%, 50%, 55%, 60%, 65%, 70% or a range consisting of any two values therebetween. For example, P2 can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two values therebetween. The first base film has a higher porosity, which can further increase the liquid retention of the first diaphragm, better improve the interface problems caused by insufficient electrolyte between the positive and negative electrode sheets in the corner area, thereby further improving the cycle performance of the secondary battery. At the same time, by regulating the porosity P1 of the first base film and the porosity P2 of the second base film within the scope of the present application, the mechanical strength of the first separator and the second separator is relatively high, and the obtained secondary battery also has good safety performance.
[0049] In some embodiments of the present application, the aperture D1 of the first base film is larger than the aperture D2 of the second base film, 80nm≤D1≤700nm, 50nm≤D2≤200nm. In some embodiments of the present application, 250nm≤D1≤520nm, 100nm≤D2≤150nm. For example, D1 can be 80nm, 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, or a range consisting of any two values therebetween. For example, D2 can be 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 120nm, 150nm, 180nm, 200nm, or a range consisting of any two values therebetween. The first base film has a larger pore size, which can further increase the liquid retention of the first diaphragm, improve the transmission of lithium ions, and better improve the interface problem caused by insufficient electrolyte between the positive electrode and the negative electrode in the corner area, thereby further improving the cycle performance of the secondary battery. At the same time, by adjusting the pore size D1 of the first base film and the pore size D2 of the second base film within the scope of this application, the mechanical strength of the first diaphragm and the second diaphragm is relatively high, and the secondary battery obtained also has good safety performance.
[0050] In some embodiments of the present application, the thickness h1 of the first base film may be 4.5 μm to 8.0 μm, and the thickness h2 of the second base film may be 4.5 μm to 8.0 μm. The present application does not particularly limit the types of the first base film and the second base film, as long as the purpose of the present application can be achieved. For example, the materials of the first base film and the second base film may include but are not limited to polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex or aramid. The types of the first base film and the second base film may include at least one of a woven film, a nonwoven film, a microporous film, a composite film, a rolled film or a spun film.
[0051] In the present application, the first base film with different porosity and pore size can be purchased, and the first base film with the required porosity and pore size can be selected in combination with the "porosity test" and "pore size test" test methods of the present application. The second base film with different porosity and pore size can be purchased, and the second base film with the required porosity and pore size can be selected in combination with the "porosity test" and "pore size test" test methods of the present application.
[0052] In some embodiments of the present application, the coating weight CW1 of the first ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 For example, the coating weight CW1 of the first ceramic coating may be 7 mg / cm 2 、7.5mg / cm 2 , 8mg / cm 2 、8.5mg / cm 2 , 9mg / cm 2 , 9.2mg / cm 2 、9.5mg / cm 2 , 9.7mg / cm 2 、10mg / cm 2 、10.2mg / cm 2 、10.5mg / cm 2 、10.7mg / cm 2 、11mg / cm 2 , 11.2mg / cm 2 、11.5mg / cm 2 、11.7mg / cm 2 , 12mg / cm 2 , 12.5mg / cm 2 、13mg / cm 2Or a range consisting of any two of the values. By regulating the coating weight CW1 of the first ceramic layer within the above range, the first ceramic coating can absorb part of the electrolyte. Regulating the coating weight of the first ceramic layer within the above range is beneficial to increasing the liquid retention of the first diaphragm, thereby improving the liquid storage performance of the first diaphragm, and is beneficial to improving the cycle performance of the secondary battery. At the same time, it is beneficial to improve the thermal stability and strength of the first diaphragm, improve its mechanical properties, reduce the possibility of large-area contact between the positive electrode and the negative electrode due to the shrinkage of the first diaphragm during the charge and discharge of the secondary battery, and is beneficial to improving the safety performance of the secondary battery.
[0053] In some embodiments of the present application, the coating weight CW2 of the first bonding layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 For example, the coating weight CW2 of the first adhesive layer may be 0.0004 mg / mm 2 , 0.0006mg / mm 2 , 0.0008mg / mm 2 , 0.001mg / mm 2 , 0.0012mg / mm 2 、0.0014mg / mm 2 、0.0016mg / mm 2 、0.0018mg / mm 2 , 0.002mg / mm 2 Or a range consisting of any two of the above values. By adjusting the coating weight CW2 of the first adhesive layer within the scope of this application, the first diaphragm has a higher bonding force with the positive electrode sheet and / or the negative electrode sheet, which can strengthen the interface between the first diaphragm and the positive electrode sheet and / or the negative electrode sheet, which is beneficial to the transmission of lithium ions and can further improve the cycle performance of the secondary battery.
[0054] In some embodiments of the present application, the coating weight CW1 of the first ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 The coating weight CW2 of the first adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 By regulating the coating weight CW1 of the first ceramic coating and the coating weight CW2 of the first bonding layer within the above range, the first separator has high liquid retention capacity and good structural stability and adhesion, which is conducive to further improving the cycle performance of the secondary battery and taking into account safety performance and energy density.
[0055] In some embodiments of the present application, the coating weight CW3 of the second ceramic coating is 7 mg / cm 2Up to 13mg / cm 2 For example, the coating weight CW3 of the second ceramic coating may be 7 mg / cm 2 、7.5mg / cm 2 , 8mg / cm 2 、8.5mg / cm 2 , 9mg / cm 2 , 9.2mg / cm 2 、9.5mg / cm 2 , 9.7mg / cm 2 、10mg / cm 2 、10.2mg / cm 2 、10.5mg / cm 2 、10.7mg / cm 2 、11mg / cm 2 , 11.2mg / cm 2 、11.5mg / cm 2 、11.7mg / cm 2 , 12mg / cm 2 , 12.5mg / cm 2 、13mg / cm 2 Or a range consisting of any two of the values. By regulating the coating weight CW3 of the second ceramic layer within the above range, it is beneficial to improve the thermal stability and strength of the second diaphragm, improve its mechanical properties, reduce the possibility of large-area contact between the positive electrode plate and the negative electrode plate due to the shrinkage of the second diaphragm during the charging and discharging of the secondary battery, and help improve the safety performance of the secondary battery. At the same time, the second ceramic coating can absorb part of the electrolyte. Regulating the coating weight of the second ceramic layer within the above range is beneficial to improve the liquid retention of the second diaphragm, thereby improving the liquid storage performance of the first diaphragm, which is beneficial to improve the cycle performance of the secondary battery. In the present application, the coating weight of the second ceramic coating can be regulated by means known to those skilled in the art. For example, when the second ceramic coating slurry is coated on the surface of the second base film, on the basis of a certain solid content of the second ceramic coating slurry, the coating amount of the second ceramic coating slurry is increased to increase the coating weight of the second ceramic coating.
[0056] In some embodiments of the present application, the coating weight CW4 of the second bonding layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 For example, the coating weight CW4 of the second adhesive layer may be 0.0004 mg / mm 2 , 0.0006mg / mm 2 , 0.0008mg / mm 2 , 0.001mg / mm 2 , 0.0012mg / mm2 、0.0014mg / mm 2 、0.0016mg / mm 2 、0.0018mg / mm 2 , 0.002mg / mm 2 Or a range consisting of any two of the above values. By adjusting the coating weight CW4 of the second adhesive layer within the scope of this application, the second diaphragm has a higher bonding force with the positive electrode sheet and / or the negative electrode sheet, which can strengthen the interface between the second diaphragm and the positive electrode sheet and / or the negative electrode sheet, which is beneficial to the transmission of lithium ions and can further improve the cycle performance of the secondary battery.
[0057] In some embodiments of the present application, the coating weight CW3 of the second ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 The coating weight of the second adhesive layer CW4 is 0.0004 mg / mm 2 To 0.002mg / mm 2 By regulating the coating weight CW3 of the second ceramic coating and the coating weight CW4 of the second adhesive layer within the above range, the second separator has high structural stability and adhesion and good liquid retention capacity, which is beneficial to further improve the safety performance and energy density of the secondary battery while taking into account the cycle performance.
[0058] In some embodiments of the present application, the first adhesive layer includes a first adhesive, the second adhesive layer includes a second adhesive, and the first adhesive and the second adhesive each independently include at least one of polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyethylene oxide (PEO) or polyimide (PI). By selecting the first adhesive and the second adhesive of the above type, it is beneficial to improve the bonding force between the first diaphragm and the positive electrode sheet, between the first diaphragm and the negative electrode sheet, between the second diaphragm and the positive electrode sheet, and between the second diaphragm and the negative electrode sheet, strengthen the interface between the first diaphragm and the positive electrode sheet, between the first diaphragm and the negative electrode sheet, between the second diaphragm and the positive electrode sheet, and between the second diaphragm and the negative electrode sheet, which is beneficial to the transmission of lithium ions and improves the cycle performance of the secondary battery; at the same time, the possibility of the first ceramic coating and the second ceramic coating falling off is reduced, and the thickness of the secondary battery is reduced, that is, the energy density of the secondary battery is improved. The present application has no special restrictions on the weight average molecular weight of the first adhesive and the second adhesive, as long as the purpose of the present application can be achieved. For example, the weight average molecular weight of the first binder and the second binder may be 1.5×10 4 to 9×10 6 .
[0059] In one embodiment of the present application, the first adhesive layer may further include a first thickener, and the second adhesive layer may further include a second thickener. Applying the first thickener to the first adhesive layer and the second thickener to the second adhesive layer is conducive to increasing the stability of the first adhesive layer slurry and the second adhesive layer slurry, and preventing the sedimentation of each component in the first adhesive layer slurry and the second adhesive layer slurry. The present application has no particular restrictions on the types of the first thickener and the second thickener, as long as the purpose of the present application can be achieved. For example, the first thickener and the second thickener are each independently selected from at least one of hydroxyethyl cellulose, methyl hydroxyethyl cellulose, sodium carboxymethyl cellulose, polyacrylamide or sodium alginate. The present application has no particular restrictions on the content of the first thickener in the first adhesive layer and the content of the second thickener in the second adhesive layer. Those skilled in the art can select according to actual needs, as long as the purpose of the present application can be achieved. For example, based on the mass of the first adhesive layer, the mass percentage of the first thickener is 0.3% to 6%; based on the mass of the second adhesive layer, the mass percentage of the second thickener is 0.3% to 6%. The present application has no particular restrictions on the content of the first binder in the first adhesive layer and the content of the second binder in the second adhesive layer. Those skilled in the art can select according to actual needs as long as the purpose of the present application can be achieved. For example, based on the mass of the first adhesive layer, the mass percentage of the first binder is 94% to 99.7%; based on the mass of the second adhesive layer, the mass percentage of the second binder is 94% to 99.7%.
[0060] In some embodiments of the present application, the first ceramic coating includes first ceramic particles, the second ceramic coating includes second ceramic particles, and the first ceramic particles and the second ceramic particles each independently include at least one of aluminum oxide, boehmite, silicon oxide, magnesium oxide, titanium oxide, tin oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, aluminum hydroxide, magnesium hydroxide, or calcium hydroxide. The type of the first ceramic particles in the first ceramic coating and the type of the second ceramic particles in the second ceramic coating are within the scope of the present application, which can further improve the liquid retention capacity of the first diaphragm and the second diaphragm, improve the interface problem caused by insufficient electrolyte between the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery.
[0061] In some embodiments of the present application, based on the mass of the first ceramic coating, the mass percentage C1 of the first ceramic particles is 10% to 50%. For example, the mass percentage C1 of the first ceramic particles is 10%, 20%, 25%, 30%, 36%, 42%, 50% or any value between any two of the above numerical ranges. The mass percentage of the first ceramic particles in the first ceramic coating is regulated within the above range so that the first ceramic particles can fully play their corresponding role, and a first diaphragm with good liquid storage capacity and wetting performance is obtained. The first diaphragm is applied to the secondary battery, which is beneficial to the secondary battery having good cycle performance, while taking into account the energy density and safety performance of the secondary battery.
[0062] In some embodiments of the present application, based on the mass of the second ceramic coating, the mass percentage C2 of the second ceramic particles is 10% to 50%. For example, the mass percentage C2 of the second ceramic particles is 10%, 20%, 25%, 30%, 36%, 42%, 50% or any value between any two of the above numerical ranges. The mass percentage of the second ceramic particles in the second ceramic coating is regulated within the above range, so that the second ceramic particles can fully play their corresponding role, so that the second diaphragm can take into account the liquid retention capacity, and the second diaphragm is applied to the secondary battery, which is conducive to making the secondary battery have high energy density and safety performance, and taking into account the cycle performance of the secondary battery.
[0063] In one embodiment of the present application, the first ceramic coating also includes a first ceramic coating binder, and the second ceramic coating also includes a second ceramic coating binder. The present application does not particularly limit the types of the first ceramic coating binder and the second ceramic coating binder, as long as the purpose of the present application can be achieved. For example, the first ceramic coating binder and the second ceramic coating binder are each independently selected from at least one of styrene-butadiene rubber, polyvinyl alcohol, polyvinylidene fluoride, polyacrylic acid, polymethyl methacrylate, polybutyl acrylate or polyacrylonitrile. The present application does not particularly limit the content of the first ceramic particles and the first ceramic coating binder in the first ceramic coating, and the content of the second ceramic particles and the second ceramic coating binder in the second ceramic coating. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. Exemplarily, based on the mass of the first ceramic coating, the mass percentage of the first ceramic coating binder is 50% to 90%; based on the mass of the second ceramic coating, the mass percentage of the second ceramic coating binder is 50% to 90%.
[0064] In some embodiments of the present application, the thickness H1 of the first diaphragm is 7.5 μm to 15.0 μm, and the thickness H2 of the second diaphragm is 6.0 μm to 13.0 μm. For example, the thickness H1 of the first diaphragm can be 7.5 μm, 8.0 μm, 8.5 μm, 9.0 μm, 9.5 μm, 10.0 μm, 10.5 μm, 11.0 μm, 11.5 μm, 12.0 μm, 12.5 μm, 13.0 μm, 13.5 μm, 14.0 μm, 14.5 μm, 15.0 μm, or a range consisting of any two values therebetween. For example, the thickness H2 of the second diaphragm can be 6.0 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm, 11.0 μm, 11.5 μm, 12.0 μm, 12.5 μm, 13.0 μm, or a range consisting of any two values therebetween. By regulating the thickness H1 of the first diaphragm and the thickness H2 of the second diaphragm within the above range, the obtained secondary battery has a high energy density while taking into account both cycle performance and safety performance.
[0065] The present application has no particular restrictions on the preparation method of the first diaphragm, as long as the purpose of the present application can be achieved. For example, the preparation method of the first diaphragm includes but is not limited to the following steps: (1) adding the first binder and the first thickener to the solvent and mixing them evenly to obtain a first bonding layer slurry; (2) adding the first ceramic particles and the first ceramic coating binder to the solvent and mixing them evenly to obtain a first ceramic coating slurry; (3) coating the first ceramic coating slurry on one surface of the first base film, and after drying, forming a first ceramic coating on one surface of the first base film; coating the first ceramic coating slurry on the other surface of the first base film, and after drying, forming a first ceramic coating on the other surface of the first base film; (4) coating the first bonding layer slurry on the surface of the first ceramic coating on one side, and after drying, obtaining the first diaphragm.
[0066] In the present application, the coating weight of the first ceramic coating can be regulated by means known to those skilled in the art. For example, when the first ceramic coating slurry is coated on the surface of the first base film, the coating amount of the first ceramic coating slurry is increased on the basis of a certain solid content of the first ceramic coating slurry to increase the coating weight of the first ceramic coating. On the contrary, the coating weight of the first ceramic coating can be reduced. The coating weight of the first bonding layer can be regulated by means known to those skilled in the art. For example, when coating the first bonding layer slurry, the coating amount of the first bonding layer slurry is increased on the basis of a certain solid content of the first bonding layer slurry to increase the coating weight of the first bonding layer. On the contrary, the coating weight of the first bonding layer can be reduced.
[0067] The present application has no particular restrictions on the preparation method of the second diaphragm, as long as the purpose of the present application can be achieved. For example, the preparation method of the second diaphragm includes but is not limited to the following steps: (1) adding the second binder and the second thickener to the solvent and mixing them evenly to obtain a second bonding layer slurry; (2) adding the second ceramic particles and the second ceramic coating binder to the solvent and mixing them evenly to obtain a second ceramic coating slurry; (3) applying the second bonding layer slurry on one surface of the second base film, and after drying, forming a second bonding layer on one surface of the second base film; applying the second ceramic coating slurry on the other surface of the second base film, and after drying, forming a second ceramic coating on the other surface of the second base film; (4) applying the second bonding layer slurry to the surface of the second ceramic coating away from the second base film, and after drying, obtaining a second diaphragm.
[0068] In the present application, the coating weight of the second bonding layer can be regulated by means known to those skilled in the art. For example, when the second bonding layer slurry is coated on the surface of the second base film, the coating amount of the second bonding layer slurry is increased on the basis of a certain solid content of the second bonding layer slurry to increase the coating weight of the second bonding layer. On the contrary, the coating weight of the second bonding layer can be reduced. The coating weight of the second ceramic coating can be regulated by means known to those skilled in the art. For example, when the second ceramic coating slurry is coated, the coating amount of the second ceramic coating slurry is increased on the basis of a certain solid content of the second ceramic coating slurry to increase the coating weight of the second ceramic coating. On the contrary, the coating weight of the second ceramic coating can be reduced.
[0069] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, it can include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or composite current collector, illustratively, the composite current collector can be a lithium copper composite current collector, a carbon copper composite current collector, a nickel copper composite current collector, a titanium copper composite current collector, etc. The present application has no particular restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved, for example, the thickness of the negative electrode current collector is 4μm to 15μm.
[0070] In some embodiments of the present application, the first negative electrode material layer and the second negative electrode material layer may also include a conductive agent and a binder. The present application does not particularly limit the types of conductive agents and binders, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, graphene, metal materials or conductive polymers, and the conductive carbon black may include but is not limited to at least one of acetylene black or Ketjen black. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers, and specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymers may include but are not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole. For example, the binder may include, but is not limited to, at least one of polyacrylic acid, sodium polyacrylate, potassium polyacrylate, lithium polyacrylate, polyimide, polyvinyl alcohol, carboxymethyl cellulose, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, polyimide, polyamide-imide, styrene-butadiene rubber or polyvinylidene fluoride. The present application does not particularly limit the mass ratio of the negative electrode active material, the conductive agent and the binder in the first negative electrode material layer and the second negative electrode material layer. Those skilled in the art can choose according to actual needs as long as the purpose of the present application can be achieved. The present application does not particularly limit the thickness of the first negative electrode material layer and the second negative electrode material layer as long as the purpose of the present application can be achieved. For example, the thickness of the first negative electrode material layer and the second negative electrode material layer are each independently 30 μm to 120 μm.
[0071] The present application has no particular limitation on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, it may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector).
[0072] The positive electrode material layer includes a positive electrode active material. The present application has no particular limitation on the positive electrode active material as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include but is not limited to at least one of lithium nickel cobalt manganese oxide (such as NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium iron manganese phosphate or lithium titanate.
[0073] The positive electrode material layer may also include a conductive agent and a binder. The present application does not particularly limit the types of the conductive agent and the binder, as long as the purpose of the present application can be achieved. For example, it may be at least one of the above conductive agent and the above binder. The present application does not particularly limit the mass ratio of the positive electrode active material, the conductive agent, and the binder in the positive electrode material layer. Those skilled in the art can select according to actual needs, as long as the purpose of the present application can be achieved.
[0074] The present application has no particular limitation on the thickness of the positive electrode current collector and the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5 μm to 20 μm, and the thickness of the positive electrode material layer is 30 μm to 120 μm.
[0075] In the present application, the secondary battery further includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent.
[0076] The present application has no particular restrictions on lithium salts, as long as the purpose of the present application can be achieved. For example, the lithium salt may include but is not limited to at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalatoborate) (LiBOB) or lithium difluoroborate. The present application has no particular restrictions on the content of lithium salts in the electrolyte, as long as the purpose of the present application can be achieved.
[0077] The present application has no particular restrictions on non-aqueous solvents, as long as the purpose of the present application can be achieved, for example, non-aqueous solvents may include but are not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of linear carbonate compounds, cyclic carbonate compounds or fluorinated carbonate compounds. The above-mentioned linear carbonate compounds may include but are not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or ethyl methyl carbonate (MEC). The above-mentioned cyclic carbonate may include but are not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The fluorinated carbonate compound may include, but is not limited to, at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The above-mentioned carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone, or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate. The present application has no particular restrictions on the content of the non-aqueous solvent in the electrolyte, as long as the purpose of the present application can be achieved.
[0078] The secondary battery also includes a shell for accommodating a positive electrode plate, a separator, a negative electrode plate and an electrolyte, as well as other components known in the field of secondary batteries, and this application does not limit the above-mentioned other components. This application does not particularly limit the shell, and it can be a shell known in the art, as long as the purpose of this application can be achieved. For example, the shell can be a hard shell or a flexible shell. The material of the hard shell can be metal, and this application does not limit the type of metal. A metal hard shell known in the art can be used, as long as the purpose of this application can be achieved. The flexible shell can be a metal plastic film, such as an aluminum plastic film, a steel plastic film, etc.
[0079] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and there is no particular limitation in the present application. For example, the preparation process of the secondary battery may include but is not limited to the following steps: stacking the positive electrode sheet, the first diaphragm, the negative electrode sheet, and the second diaphragm in order, winding them to obtain an electrode assembly of a winding structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the shell as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.
[0080] In some embodiments of the present application, the secondary battery of the present application may include but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery or a lithium ion polymer secondary battery, etc. In some embodiments of the present application, the secondary battery includes a lithium ion battery.
[0081] The second aspect of the present application provides an electric device, which includes the secondary battery in any of the above embodiments. Therefore, the electric device provided by the present application has good performance.
[0082] The present application does not particularly limit the type of electronic device, and it can be used for any electronic device known in the prior art. In some embodiments of the present application, the electronic device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.
[0083] Example
[0084] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0085] Test methods and equipment:
[0086] Tests on the coating element type and its mass percentage W1, the doping element type and its mass percentage W1' in the first negative electrode material layer, and the coating element type and its mass percentage W2, the doping element type and its mass percentage W2' in the second negative electrode material layer:
[0087] The lithium-ion battery was disassembled after being discharged to 3V at 0.2C, the negative electrode sheet was taken out, and the negative electrode sheet was cleaned with dimethyl carbonate (DMC). Among them, the first negative electrode material layer is a longer layer, and the second negative electrode material layer is a shorter layer.
[0088] Cut a cross section of the negative electrode sheet along the thickness direction, and use plasma polishing, then use a scanning electron microscope combined with an energy spectrometer to test to obtain the types of coating elements and doping elements in the first negative electrode material layer. When the element is mainly distributed on the surface of the first negative electrode active material particles, the corresponding element is a coating element; when the element is mainly dispersed inside the first negative electrode active material particles, the corresponding element is a doping element. Thus, the types of coating elements or doping elements in the first negative electrode material layer are obtained.
[0089] By replacing the first negative electrode material layer in the above step with the second negative electrode material layer, the types of coating elements or doping elements in the second negative electrode material layer can be obtained.
[0090] The first negative electrode material layer on the surface of the negative electrode current collector in the negative electrode sheet is scraped off, then weighed, concentrated nitric acid is added for microwave digestion to obtain a solution, and the obtained solution and filter residue are washed multiple times and fixed to volume, and the plasma intensity of the coating element therein is tested by inductively coupled plasma emission spectrometer (ICP-OES), and the content of the coating element in the solution is calculated according to the standard curve of the measured element, thereby calculating the mass percentage content W1 of the coating element in the first negative electrode active material layer. In the above steps, the plasma intensity of the coating element is changed to the plasma intensity of the doping element, and the mass percentage content W1' of the doping element in the first negative electrode material layer can be obtained accordingly.
[0091] By replacing the first negative electrode material layer in the above step with the second negative electrode material layer, the mass percentage content W2 of the coating element in the second negative electrode active material layer and the mass percentage content W2' of the doping element in the second negative electrode material layer can be obtained.
[0092] First and second diaphragm sampling methods:
[0093] The lithium-ion batteries in the tested embodiments and comparative examples were disassembled, the first diaphragm and the second diaphragm were taken out, and the electrolyte residue was removed by soaking in dimethyl carbonate (DMC) for 20 minutes, and then the first diaphragm and the second diaphragm were placed in an oven and dried at 60°C for 12 hours to obtain the first diaphragm sample and the second diaphragm sample. The above method was used to obtain the first diaphragm and the second diaphragm in the following tests unless otherwise specified.
[0094] Sampling method of the first basement membrane and the second basement membrane:
[0095] The first diaphragm and the second diaphragm obtained by the above sampling were placed in containers respectively, N-methylpyrrolidone (NMP) was added, and the containers were placed in an ultrasonic instrument with a heating function for ultrasonication, the temperature was controlled at 45°C, and the ultrasonication was performed for 3 hours. When the first diaphragm and the second diaphragm became completely transparent, they were taken out to obtain the first basement membrane and the second basement membrane. The above method was used to obtain the first basement membrane and the second basement membrane in the following tests unless otherwise specified.
[0096] Porosity test of the first base film and the second base film:
[0097] The gas displacement method is adopted for testing, and the first basement membrane and the second basement membrane are punched out by molds to prepare samples respectively (technical personnel in this field can select molds of common sizes and shapes in this field according to factors such as the size and shape of the test object and the requirements of the test equipment), and the true volume V0 of the sample is measured by a true density tester. The apparent volume V of the sample can be calculated by measuring the area and thickness of the sample. Then, the percentage of the pore volume of the sample to the total area P = (V-V0) / V×100%, that is, the porosity of the first basement membrane or the second basement membrane is obtained respectively.
[0098] Pore size test of the first base film and the second base film:
[0099] The specific steps are as follows:
[0100] ① Use anhydrous ethanol to completely wet and fill the pores of the base membrane to be tested, so that positive pressure is formed in the pores due to capillary phenomenon;
[0101] ②Put the basement membrane into a closed tank and use gas pressure to squeeze the liquid out of the capillary pores;
[0102] ③ According to the relative relationship between the pressure ΔP applied when the liquid in a single pore is completely squeezed out of the capillary pore and the pore diameter d, the diaphragm pore diameter can be obtained according to the Laplace equation. The Laplace equation is shown as follows:
[0103] d=-4γcosθ / ΔP×100%
[0104] Wherein, d is the pore diameter (aperture), ΔP is the pressure, γ is the surface tension of anhydrous ethanol, and θ is the contact angle between the diaphragm and anhydrous ethanol. At different pressures, the liquid in the basement membrane will be squeezed out successively and a certain gas penetration flow rate will be generated. The pore size and pore size distribution can be calculated based on the relationship between pressure and flow changes. The above basement membrane is the first basement membrane or the second basement membrane.
[0105] Thickness test of the first and second diaphragms:
[0106] The first diaphragm was subjected to argon ion polishing to obtain a cross section of the first diaphragm, and the cross section of the first diaphragm along the thickness direction was observed by a field emission scanning electron microscope (Philips, XL-30 model) and a scanning electron microscope photograph was taken, and the thickness H1 of the first diaphragm was measured by the scanning electron microscope. The first diaphragm was replaced by the second diaphragm, and the thickness H2 of the second diaphragm was measured.
[0107] Cycle performance test:
[0108] At 25°C, the lithium-ion battery was charged to 4.5V at 2C constant current, and then charged to 0.02C at 4.5V constant voltage. After standing for 5 minutes, it was discharged to 3.0V at 0.7C constant current. This was the first cycle, and the discharge capacity was recorded. The lithium-ion battery was charged and discharged according to the above process. When the cycle reached 1000 cycles (cls), the test was stopped and the capacity retention rate was calculated as an indicator for evaluating the cycle performance of the lithium-ion battery.
[0109] Capacity retention rate (%) = (discharge capacity after 1000 cycles / first cycle discharge capacity) × 100%.
[0110] Drop test:
[0111] At 25℃, charge the lithium-ion battery to 4.5V at 2C, then charge it to 0.02C at 4.5V. At 20±5℃, clamp the lithium-ion battery and drop it from a height of 1m to a concrete drop floor. Perform one test, then perform one test from a height of 1.25m and one test from a height of 1.5m. Perform the above three tests on one side. The order of drop is to perform drop tests on the six sides of the lithium-ion battery, specifically the first three times, the last three times, the top three times, the bottom three times, the left three times, and the right three times. Judgment criteria: No fire, no explosion, no smoke, no leakage, no rupture, no deflation, no disintegration is considered to pass the drop test. Each group tests 10 lithium-ion batteries.
[0112] Drop test pass rate (%) = (number of lithium-ion batteries that passed the drop test / 10) × 100%. The greater the drop test pass rate, the better the safety performance of the lithium-ion battery.
[0113] Extrusion test:
[0114] At 25℃, charge the lithium-ion battery to 4.5V at 2C, and then charge it to 0.02C at 4.5V. Place the lithium-ion battery on the test table at 20±5℃, with 5 lithium-ion batteries facing up and 5 lithium-ion batteries facing up (along the thickness of the lithium-ion battery, one side is the front side and the other side is the back side). Use a blunt nail with a diameter of 6mm, a drop speed of 300N / min, and an extrusion force of 1550N. Test the sample lithium-ion battery body 12mm away from the top seal. Judgment criteria: If there is no fire or explosion, it is considered to have passed the extrusion test. Each group tests 10 lithium-ion batteries.
[0115] Extrusion test pass rate (%) = (number of lithium-ion batteries that passed the extrusion test / 10) × 100%. The greater the extrusion test pass rate, the better the safety performance of the lithium-ion battery.
[0116] Energy density test:
[0117] Place the secondary battery in a 25℃±2℃ thermostat for 30 minutes to allow the secondary battery to reach a constant temperature. Charge the secondary battery at a constant current of 0.5C to a full charge voltage of 4.5V, then charge at a full charge voltage of 4.5V to a current of 0.05C, and discharge at a constant current of 0.2C to a voltage of 3.0V, and record the discharge energy.
[0118] Volume energy density = discharge energy / (length of secondary battery × width of secondary battery × thickness of secondary battery). The length, width and thickness of the secondary batteries in Tables 1 to 3 and 5 are 77 mm, 69 mm and 51 mm, respectively. The length, width and thickness of the secondary batteries in Table 4 are measured by a micrometer, and each value is measured 3 times, and the average value is taken as the final result.
[0119] Capacity retention test:
[0120] A battery performance tester (brand: Xinweier; model: CT-4008W-5V6A-80CH) was used to perform constant current charging with a current of 4A (charging rate of 1C) to a full charge voltage of 4.5V, and then to perform constant voltage charging with a current of 4.5V to a cut-off current of 200mA (0.05C), followed by standing for 10 minutes, and then to perform constant current discharge with a current of 2A (0.5C) to a voltage of 3V, and to stand for 10 minutes. This process was recorded as 1 cycle, and at this time there would be a discharge capacity of 1 cycle; then the charge and discharge were repeated. Among them, the discharge capacity of the first discharge is the initial discharge capacity.
[0121] Capacity retention rate (%)=(discharge capacity at the 1000th cycle / discharge capacity at the first cycle)×100%.
[0122] Example 1-1
[0123] <Preparation of First Separator>
[0124] A polyimide film with a thickness of h1 = 5 μm is used as the first base film, the porosity P1 of the first base film is 55%, and the pore size D1 of the first base film is 380 nm.
[0125] The first binder polyvinylidene fluoride (PVDF, Mw = 8.5 × 10 6 ) and the first thickener sodium carboxymethyl cellulose (Mw = 8 × 10 5 ) are mixed in a mass ratio of 98.5:1.5, deionized water is added as a solvent, and the mixture is stirred evenly to form a first bonding layer slurry with a solid content of 75wt%.
[0126] The first ceramic particles of aluminum oxide (Al2O3), the first ceramic coating binder styrene butadiene rubber (Mw = 7 × 10 6 ) are mixed in a mass ratio of 3:7, deionized water is added as a solvent, and the mixture is stirred evenly to obtain a first ceramic coating slurry with a solid content of 45 wt %.
[0127] A first ceramic coating slurry is coated on one surface of the first base film, and after drying at 60°C, a first ceramic coating is formed on one surface of the first base film; a first ceramic coating slurry is coated on the other surface of the first base film, and after drying at 60°C, a first ceramic coating is formed on the other surface of the first base film. A first bonding layer slurry is coated on the surface of the first ceramic coating on one side, and after drying at 60°C, a first bonding layer is formed on the surface of the first ceramic coating on one side, thereby obtaining a first diaphragm. Based on the mass of the first ceramic coating, the mass percentage C1 of the first ceramic is 30%, and the coating weight CW1 of the first ceramic coating is 9 mg / cm 2 The coating weight CW2 of the first adhesive layer is 0.0006 mg / mm 2 .
[0128] <Preparation of Second Separator>
[0129] A polyimide film with a thickness of h2 = 5 μm is used as the first base film, the porosity P2 of the second base film is 28%, and the pore size D2 of the second base film is 120 nm.
[0130] The second binder polyvinylidene fluoride (PVDF, Mw = 8.5 × 10 6 ) and the second thickener sodium carboxymethyl cellulose (Mw = 8 × 10 5 ) are mixed in a mass ratio of 98.5:1.5, deionized water is added as a solvent, and after stirring evenly, a second bonding layer slurry with a solid content of 75wt% is formed.
[0131] The second ceramic particles of aluminum oxide (Al2O3), the second ceramic coating binder styrene butadiene rubber (Mw = 7 × 10 6 ) were mixed in a mass ratio of 3:7, deionized water was added as a solvent, and the mixture was stirred evenly to obtain a second ceramic coating slurry with a solid content of 45 wt%.
[0132] A second bonding layer slurry is coated on one surface of the second base film, and after drying at 60°C, a second bonding layer is formed on one surface of the second base film; a second ceramic coating slurry is coated on the other surface of the second base film, and after drying at 60°C, a second ceramic coating is formed on the other surface of the second base film. A second bonding layer slurry is coated on the surface of the second ceramic coating, and after drying at 60°C, a second bonding layer is formed on the surface of the second ceramic coating away from the second base film, thereby obtaining a second diaphragm. Wherein, based on the mass of the second ceramic coating, the mass percentage C2 of the first ceramic is 30%, and the coating weight CW4 of the second bonding layer is 0.0006 mg / mm 2 The coating weight of the second ceramic coating CW3 is 9 mg / cm 2 .
[0133] <Preparation of negative electrode sheet>
[0134] The negative electrode active materials artificial graphite, styrene-butadiene rubber and sodium carboxymethyl cellulose are mixed in a mass ratio of 97.6:1.1:1.3, and then deionized water is added as a solvent. After stirring evenly, a first negative electrode slurry with a solid content of 70wt% is obtained. At the same time, the first negative electrode slurry is also used as the second negative electrode slurry. The first negative electrode slurry is coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 90°C to obtain a negative electrode sheet with a first negative electrode material layer coated with a thickness of 50μm. The second negative electrode slurry is coated on the other surface of the negative electrode current collector copper foil. After drying, the thickness of the second negative electrode material layer coated on the surface is 50μm, thereby obtaining a negative electrode sheet with a total thickness of 106μm. The negative electrode sheet after coating is cold pressed and then cut into a specification of 74mm×824mm for standby use. Among them, the compaction density of the first negative electrode material layer is 1.735g / cm 3 , length is 720mm, and the compaction density of the second negative electrode material layer is 1.735g / cm 3 , with a length of 680 mm, one end of the first negative electrode material layer and the second negative electrode material layer are flush, and the first negative electrode material layer is longer than the second negative electrode material layer at the other end, wherein the other end is the starting end of the winding of the electrode assembly.
[0135] <Preparation of positive electrode sheet>
[0136] The positive electrode active material lithium cobalt oxide, the conductive agent conductive carbon black and the positive electrode binder polyvinylidene fluoride are mixed in a mass ratio of 95:2.5:2.5, N-methylpyrrolidone (NMP) is added as a solvent, and the mixture is stirred and evenly mixed to form a positive electrode slurry with a solid content of 75wt%. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 90°C to obtain a positive electrode sheet with a single-sided positive electrode material layer with a thickness of 55μm. The positive electrode slurry is coated on the other surface of the positive electrode current collector aluminum foil. After drying, the thickness of the positive electrode material layer coated on the surface is 55μm, that is, a double-sided positive electrode material layer is obtained, and a positive electrode sheet with a total thickness of 120μm is obtained. The positive electrode sheet after coating is cold pressed and then cut into a specification of 70mm×800mm for standby use. Among them, the compaction density of the first positive electrode material layer is 4.23g / cm 3 , length is 750mm, and the compaction density of the second positive electrode material layer is 4.23g / cm 3 , with a length of 680 mm, one end of the first positive electrode material layer and the second positive electrode material layer are flush, and at the other end, the first positive electrode material layer is longer than the second positive electrode material layer.
[0137] <Preparation of Electrolyte>
[0138] In a glove box filled with dry argon atmosphere, propylene carbonate (PC), diethyl carbonate (DEC), and ethylene carbonate (EC) are mixed at a mass ratio of 1:1:1 to obtain a base solvent, and then lithium hexafluorophosphate (LiPF6) lithium salt is added to the base solvent to dissolve and mix well to obtain an electrolyte. Among them, based on the mass of the electrolyte, the mass percentage of LiPF6 is 12%, and the remainder is the base solvent.
[0139] <Preparation of lithium-ion batteries>
[0140] The positive electrode sheet, the first separator, the negative electrode sheet, and the second separator prepared above are stacked in order, and then wound to obtain an electrode assembly. The positive electrode tab is spot-welded with an aluminum tab, and the negative electrode tab is spot-welded with a nickel tab. Among them, the first negative electrode material layer is close to the first separator, and the first bonding layer is located on the side of the first base film away from the first negative electrode material layer; the second negative electrode material layer is close to the second separator, and the second ceramic coating is located on the side of the second base film away from the second negative electrode material layer, and the first positive electrode material layer is close to the first separator and adjacent to the first bonding layer (the specific structure can be referred to Figure 4 The electrode assembly was placed in an aluminum-plastic film, dried in a vacuum oven at 80°C for 12 hours to remove moisture, and then injected with the above-prepared electrolyte. After vacuum packaging, standing, formation (charging at 0.02C constant current to 3.5V, and then charging at 0.1C constant current to 3.9V), capacity, and shaping processes, a lithium-ion battery was obtained.
[0141] Example 1-2 to Example 1-16
[0142] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. Among them, when the negative electrode material layer includes a doping element, the mass percentage of the doping element in the selected negative electrode active material = the mass percentage of the doping element in the negative electrode material layer / the mass percentage of the negative electrode active material in the negative electrode material layer × 100%; when the negative electrode material layer includes a coating element, the mass percentage of the coating element in the selected negative electrode active material = the mass percentage of the coating element in the negative electrode material layer / the mass percentage of the negative electrode active material in the negative electrode material layer × 100%. In the present application, the mass percentage of the negative electrode active material in the negative electrode material layer is 97.6%.
[0143] Example 2-1 to Example 2-14
[0144] Except for adjusting the relevant preparation parameters according to Table 2, the rest is the same as Example 1-1.
[0145] Example 2-15 to Example 2-23
[0146] Except for adjusting the relevant preparation parameters according to Table 2, the rest are the same as Example 1-2, Example 1-2, Example 1-2, Example 1-9, Example 1-9, Example 1-9, Example 1-16, Example 1-16, and Example 1-16.
[0147] Example 3-1 to Example 3-15
[0148] Except for adjusting the relevant preparation parameters according to Table 3, the rest is the same as Example 1-1.
[0149] Example 3-16 to Example 3-24
[0150] Except for adjusting the relevant preparation parameters according to Table 3, the rest are the same as Example 1-2, Example 1-2, Example 1-2, Example 1-9, Example 1-9, Example 1-9, Example 1-16, Example 1-16, and Example 1-16.
[0151] Example 4-1 to Example 4-10
[0152] Except for adjusting the relevant preparation parameters according to Table 4, the rest is the same as Example 1-1.
[0153] Example 4-11 to Example 4-16
[0154] Except for adjusting the relevant preparation parameters according to Table 4, the rest are the same as Example 1-2, Example 1-2, Example 1-2, Example 1-9, Example 1-9, Example 1-9, Example 1-16, Example 1-16, and Example 1-16.
[0155] Example 5-1 to Example 5-14
[0156] Except for adjusting the relevant preparation parameters according to Table 5, the rest is the same as Example 1-1. When the mass percentage content C1 of the first ceramic particles changes, the content of the first ceramic coating binder changes accordingly, and the sum of the mass percentage content of the first ceramic particles and the mass percentage content of the first ceramic coating binder is 100%. When the mass percentage content C2 of the second ceramic particles changes, the content of the second ceramic coating binder changes accordingly, and the sum of the mass percentage content of the second ceramic particles and the mass percentage content of the second ceramic coating binder is 100%.
[0157] Example 5-15 to Example 5-20
[0158] Except for adjusting the relevant preparation parameters according to Table 4, the rest are the same as Example 1-2, Example 1-2, Example 1-9, Example 1-9, Example 1-16, and Example 1-16. When the mass percentage C1 of the first ceramic particles changes, the content of the first ceramic coating binder changes accordingly, and the sum of the mass percentage of the first ceramic particles and the mass percentage of the first ceramic coating binder is 100%. When the mass percentage C2 of the second ceramic particles changes, the content of the second ceramic coating binder changes accordingly, and the sum of the mass percentage of the second ceramic particles and the mass percentage of the second ceramic coating binder is 100%.
[0159] Comparative Example 1
[0160] Except that the first diaphragm is used to replace the second diaphragm, the rest is the same as Example 1-1.
[0161] Comparative Example 2
[0162] Except for using the second diaphragm to replace the first diaphragm, the rest is the same as Example 1-1.
[0163] Comparative Example 3
[0164] Except that the first separator and the second separator are exchanged in position, the rest is the same as Example 1-1. The second negative electrode material layer is close to the first separator, and the first bonding layer is located on the side of the first base film away from the second negative electrode material layer; the first negative electrode material layer is close to the second separator, and the second ceramic coating is located on the side of the second base film away from the first negative electrode material layer.
[0165] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 to 5.
[0166] Table 1
[0167]
[0168] Note: “ / ” in Table 1 means there is no corresponding parameter.
[0169] It can be seen from Examples 1-1 to 1-16 and Comparative Examples 1 to 3 that the negative electrode sheet is located between the first diaphragm and the second diaphragm, and the electrode assembly includes a straight area and a corner area. By using the first diaphragm and the second diaphragm together, the lithium-ion battery can have a high energy density, extrusion test pass rate, drop test pass rate and capacity retention rate at the same time, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account. In Comparative Example 1, both diaphragms are the first diaphragm, and the first diaphragm includes two layers of the first ceramic coating and one layer of the first bonding layer. Although the energy density of the lithium-ion battery is not much different from that of the embodiment and the cycle performance is good, its safety performance is poor. In Comparative Example 2, both diaphragms are the second diaphragm, and the second diaphragm includes a second ceramic coating and two layers of the second bonding layer. Although the energy density of the lithium-ion battery is not much different from that of the embodiment and the safety performance is good, its cycle performance is poor. In Comparative Example 3, the first diaphragm and the second diaphragm are swapped. Although the energy density of the lithium-ion battery is not much different from that of the embodiment and the safety performance is good, its cycle performance is poor. That is, Comparative Examples 1 to 3 cannot take into account the energy density, cycle performance and safety performance of the lithium-ion battery at the same time, while the lithium-ion batteries in Examples 1-1 to 1-16 have good energy density, cycle performance and safety performance, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery are taken into account.
[0170] The type of coating element in the first negative electrode active material layer and the mass percentage of the coating element, and the type of coating element in the second negative electrode active material layer and the mass percentage of the coating element usually affect the energy density and cycle performance of the lithium-ion battery. It can be seen from Example 1-1, Example 1-2 to Example 1-8 that when the first negative electrode active material layer and the second negative electrode active material layer contain coating elements, the cycle performance of the lithium-ion battery can be further improved. It can be seen from Example 1-2 to Example 1-8 that by regulating the type of coating elements and the mass percentage of the coating elements within the scope of the present application, the lithium-ion battery has a higher energy density and capacity retention rate, and also has a higher extrusion test pass rate and a higher drop test pass rate, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery are taken into account.
[0171] The type of doping elements in the first negative electrode active material layer and the mass percentage of the doping elements, and the type of doping elements in the second negative electrode active material layer and the mass percentage of the doping elements usually affect the energy density and cycle performance of the lithium-ion battery. It can be seen from Example 1-1, Example 1-9 to Example 1-15 that when the first negative electrode active material layer and the second negative electrode active material layer contain doping elements, the cycle performance of the lithium-ion battery can be further improved. It can be seen from Example 1-9 to Example 1-15 that by regulating the type of doping elements and the mass percentage of doping elements within the scope of the present application, the lithium-ion battery has a higher energy density and capacity retention rate, and also has a higher extrusion test pass rate and a higher drop test pass rate, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery are taken into account.
[0172] It can be seen from Examples 1-1, 1-3, 1-9 and 1-16 that when the first negative electrode active material layer and the second negative electrode active material layer contain both coating elements and doping elements, the cycle performance of the lithium ion battery can be further improved.
[0173] Table 2
[0174]
[0175]
[0176] The porosity of the first base film and the porosity of the second base film usually affect the cycle performance and safety performance of the lithium-ion battery, and have little effect on its energy density. It can be seen from Examples 1-1, 2-1 to 2-14 that by regulating the porosity of the first base film and the porosity of the second base film within the scope of this application, and satisfying that the porosity of the first base film is greater than the porosity of the second base film, the lithium-ion battery can have a higher extrusion test pass rate, drop test pass rate and capacity retention rate. At the same time, referring to Example 1-1, it has a higher energy density, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0177] From Examples 1-2, 2-15 to 2-17, 1-9, 2-18 to 2-20, 1-16, 2-21 to 2-23, it can be seen that by regulating the porosity of the first base film and the porosity of the second base film within the scope of the present application and satisfying that the porosity of the first base film is greater than the porosity of the second base film, the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0178] Table 3
[0179] D1(nm) D2(nm) Extrusion test pass rate (%) Drop test pass rate (%) Capacity retention rate (%) Example 1-1 380 120 80 90 80.0 Example 1-2 380 120 80 90 88.3 Examples 1-9 380 120 90 80 88.1 Examples 1-16 380 120 90 80 93.9 Example 3-1 80 60 100 90 76.8 Example 3-2 160 120 90 90 78.2 Example 3-3 250 120 90 90 79.5 Embodiment 3-4 520 120 70 80 85.0 Embodiment 3-5 700 120 70 60 91.0 Embodiment 3-6 70 120 100 100 76.8 Embodiment 3-7 720 120 60 60 92.2 Embodiment 3-8 380 50 90 100 78.3 Embodiment 3-9 380 80 90 90 79.1 Embodiment 3-10 380 100 90 80 79.6 Example 3-11 380 150 80 80 85.5 Example 3-12 380 200 80 70 88.2 Example 3-13 380 40 100 90 78.5 Embodiment 3-14 380 220 60 70 91.0 Example 3-15 80 120 70 80 82.8 Example 3-16 80 70 90 100 85.6 Example 3-17 380 200 80 70 89.9 Example 3-18 700 50 80 80 88.5 Example 3-19 80 70 100 90 85.3 Example 3-20 380 200 70 80 90.1 Example 3-21 700 50 80 80 87.5 Example 3-22 80 70 90 100 87.8 Example 3-23 380 200 80 70 95.0 Example 3-24 700 50 80 80 92.0
[0180] The pore size of the first base film and the pore size of the second base film usually affect the cycle performance and safety performance of the lithium-ion battery, and have little effect on its energy density. It can be seen from Examples 1-1, 3-1 to 3-15 that by regulating the pore size of the first base film and the pore size of the second base film within the scope of this application, and satisfying that the pore size of the first base film is larger than the pore size of the second base film, the lithium-ion battery can have a higher extrusion test pass rate, drop test pass rate and capacity retention rate. At the same time, referring to Example 1-1, it has a higher energy density, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0181] From Examples 1-2, 3-16 to 3-18, 1-9, 3-19 to 3-21, 1-16, 3-22 to 3-24, it can be seen that by regulating the pore size of the first base membrane and the pore size of the second base membrane within the scope of the present application and satisfying that the pore size of the first base membrane is larger than the pore size of the second base membrane, the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0182] Table 4
[0183]
[0184] The coating weight of the first ceramic coating and / or the coating weight of the second ceramic coating usually affects the cycle performance and safety performance of the lithium-ion battery, and has little effect on its energy density. From Example 1-1, Example 4-7 to Example 4-10, it can be seen that by regulating the coating weight of the first ceramic coating and / or the coating weight of the second ceramic coating within the scope of this application, the lithium-ion battery can have a higher energy density, extrusion test pass rate, drop test pass rate and capacity retention rate, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0185] Compared with Example 1-1, Example 4-7 and Example 4-8, the coating weight of the first ceramic coating and the coating weight of the second ceramic coating in Example 4-9 are smaller, less than 7 mg / cm 2 Although the energy density of lithium-ion batteries is relatively large, the electrolyte infiltration is slightly poor, the capacity retention rate of lithium-ion batteries is relatively low, and the improvement of the cycle performance of lithium-ion batteries is relatively weak; compared with Example 1-1, Example 4-7 and Example 4-8, the coating weight of the first ceramic coating and the coating weight of the second ceramic coating in Example 4-10 are larger, greater than 13 mg / cm 2 Although the mechanical properties of the diaphragm are good, which can make the lithium-ion battery have higher safety performance, the distance between the positive electrode and the negative electrode is large, and the active metal ions (Li +) The transmission path is long, the capacity retention rate of the lithium-ion battery is low, the improvement of the cycle performance of the lithium-ion battery is weak, and the energy density of the lithium-ion battery is low. It can be shown that by adjusting the coating weight of the first ceramic coating and the coating weight of the second ceramic coating within the scope of this application, the energy density, cycle performance and safety performance of the lithium-ion battery can be better taken into account.
[0186] The coating weight of the first adhesive layer and / or the coating weight of the second adhesive layer usually affects the cycle performance and safety performance of the lithium-ion battery, and has little effect on its energy density. It can be seen from Examples 1-1, 4-1 to 4-6 that by regulating the coating weight of the first adhesive layer and / or the coating weight of the second adhesive layer within the scope of the present application, the lithium-ion battery can have a higher energy density, extrusion test pass rate, drop test pass rate and capacity retention rate, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0187] Compared with Example 1-1 and Example 4-1 to Example 4-4, the coating weight of the first adhesive layer and the coating weight of the second adhesive layer in Example 4-5 are smaller, less than 0.0004 mg / mm 2 The bonding between the diaphragm and the electrode is weak, and the active metal ions (such as Li + ) The transmission path is longer, and the improvement of the cycle performance of the lithium-ion battery is weak. Compared with Example 1-1, Example 4-1 to Example 4-4, the coating weight of the first adhesive layer and the coating weight of the second adhesive layer are larger, greater than 0.002 mg / mm 2 Although the diaphragm and the pole piece have good adhesion, which can make the lithium-ion battery have higher safety performance, the electrolyte infiltration is poor, the improvement of the cycle performance of the lithium-ion battery is weak, and the energy density of the secondary battery is affected. It can be shown that by adjusting the coating weight of the first adhesive layer and the coating weight of the second adhesive layer within the scope of this application, the energy density, cycle performance and safety performance of the lithium-ion battery can be better taken into account.
[0188] From Example 1-2, Example 4-11 to Example 4-12, Example 1-9, Example 4-13 to Example 4-14, Example 1-16, Example 4-15 to Example 4-16, it can be seen that by regulating the coating weight of the first ceramic coating, the coating weight of the second ceramic coating, the coating weight of the first bonding layer, and the coating weight of the second bonding layer within the scope of the present application, the energy density, cycle performance, and safety performance of the lithium-ion battery can be taken into account.
[0189] Table 5
[0190]
[0191]
[0192] The type of the first binder and / or the second binder usually affects the cycle performance and safety performance of the lithium-ion battery, and has little effect on its energy density. It can be seen from Example 1-1, Example 5-1 to Example 5-3, and Example 5-7 to Example 5-10 that by regulating the type of the first binder and / or the second binder within the scope of this application, the lithium-ion battery can have a higher extrusion test pass rate, drop test pass rate and capacity retention rate. At the same time, referring to Example 1-1, it has a higher energy density, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0193] The type and content of the first ceramic particles and / or the second ceramic particles usually affect the cycle performance and safety performance of the lithium-ion battery, and have little effect on its energy density. It can be seen from Example 1-1, Example 5-4 to Example 5-6, and Example 5-7 to Example 5-14 that by regulating the type and content of the first ceramic particles and / or the second ceramic particles within the scope of this application, the lithium-ion battery can have a higher extrusion test pass rate, drop test pass rate and capacity retention rate. At the same time, referring to Example 1-1, it has a higher energy density, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0194] From Examples 1-2, 5-15 to 5-16, 1-9, 5-17 to 5-18, 1-16, 5-19 to 5-20, it can be seen that by regulating the type of the first binder and / or the second binder, and the type and content of the first ceramic particles and / or the second ceramic particles within the scope of the present application, the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account.
[0195] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A secondary battery, comprising an electrode assembly of a wound structure, the electrode assembly comprising a positive electrode sheet, a negative electrode sheet, a first separator and a second separator, the negative electrode sheet is located between the first separator and the second separator, and the electrode assembly comprises a straight area and a corner area; The negative electrode sheet comprises a negative electrode current collector and a first negative electrode material layer and a second negative electrode material layer located on both sides of the negative electrode current collector in a thickness direction, the first separator is adjacent to the first negative electrode material layer, and the second separator is adjacent to the second negative electrode material layer; The first separator in the corner area includes a first base film, a first bonding layer and a first ceramic coating, wherein the first bonding layer is arranged on a side of the first base film away from the first negative electrode material layer, the first ceramic coating is arranged on both sides of the first base film, the first ceramic coating is located between the first base film and the first bonding layer, and a layer of the first ceramic coating is in direct contact with the first negative electrode material layer; The second separator in the corner area comprises a second base film, a second bonding layer and a second ceramic coating, wherein the second bonding layer is arranged on both sides of the second base film, the second ceramic coating is arranged on a side of the second base film away from the second negative electrode material layer, and the second ceramic coating is located between the second base film and the second bonding layer; In the corner area, a positive electrode sheet corner segment is adjacent to a first negative electrode material layer corner segment, the positive electrode sheet corner segment is farther away from the winding center of the electrode assembly than the first negative electrode material layer corner segment, the first diaphragm is located between the positive electrode sheet corner segment and the first negative electrode material layer corner segment, and the positive electrode sheet corner segment is in contact with the first bonding layer.
2. The secondary battery according to claim 1, wherein Along the winding direction of the electrode assembly, the length of the first negative electrode material layer is greater than the length of the second negative electrode material layer.
3. The secondary battery according to claim 1, wherein The first negative electrode material layer includes a first negative electrode active material, the second negative electrode material layer includes a second negative electrode active material, and the secondary battery satisfies at least one of the following characteristics: (1) The surface of the particles of the first negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage W1 of the coating element is 0.05% to 0.5% based on the mass of the first negative electrode material layer; (2) The surface of the particles of the second negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage content W2 of the coating element is 0.05% to 0.5% based on the mass of the second negative electrode material layer; (3) The first negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and the mass percentage content W1' of the doping element is 0.05% to 0.5% based on the mass of the first negative electrode material layer; (4) The second negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and the mass percentage W2' of the doping element is 0.05% to 0.5% based on the mass of the second negative electrode material layer.
4. The secondary battery according to claim 3, wherein The first negative electrode active material and the second negative electrode active material each independently include natural graphite, artificial graphite, mesophase micro carbon beads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x , Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structure lithium titanate Li4Ti5O 12 , Li-Al alloy or at least one of metallic lithium, 0 <x<2。 5. The secondary battery according to claim 1, wherein The positive electrode sheet includes a positive electrode current collector and a first positive electrode material layer and a second positive electrode material layer located on both sides of the positive electrode current collector in the thickness direction. In the same winding layer, the first positive electrode material layer is closer to the winding center of the electrode assembly than the second positive electrode material layer. At the winding end of the electrode assembly, the length of the first positive electrode material layer is greater than the length of the second positive electrode material layer.
6. The secondary battery according to any one of claims 1 to 5, wherein The porosity P1 of the first base film is greater than the porosity P2 of the second base film, 40%≤P1≤70%, 5%≤P2≤50%.
7. The secondary battery according to claim 6, wherein 50%≤P1≤60%, 10%≤P2≤40%.
8. The secondary battery according to any one of claims 1 to 5, wherein The pore size D1 of the first base film is larger than the pore size D2 of the second base film, 80nm≤D1≤700nm, 50nm≤D2≤200nm.
9. The secondary battery according to claim 8, wherein 250nm≤D1≤520nm, 100nm≤D2≤150nm.
10. The secondary battery according to any one of claims 1 to 5, wherein The coating weight of the first ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 , and / or, the coating weight of the first adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 .
11. The secondary battery according to any one of claims 1 to 5, wherein The coating weight of the second ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 , and / or, the coating weight of the second adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 .
12. The secondary battery according to any one of claims 1 to 5, wherein The first adhesive layer includes a first adhesive, the second adhesive layer includes a second adhesive, and the first adhesive and the second adhesive each independently include at least one of polyvinylidene fluoride, polyacrylonitrile, polyethylene oxide or polyimide.
13. The secondary battery according to any one of claims 1 to 5, wherein The first ceramic coating includes first ceramic particles, and the second ceramic coating includes second ceramic particles, and the first ceramic particles and the second ceramic particles each independently include at least one of aluminum oxide, boehmite, silicon oxide, magnesium oxide, titanium oxide, tin oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, aluminum hydroxide, magnesium hydroxide or calcium hydroxide.
14. The secondary battery according to claim 13, wherein Based on the mass of the first ceramic coating, the mass percentage of the first ceramic particles is 10% to 50%; based on the mass of the second ceramic coating, the mass percentage of the second ceramic particles is 10% to 50%.
15. The secondary battery according to any one of claims 1 to 5, wherein The thickness H1 of the first diaphragm is 7.5 μm to 15.0 μm, and the thickness H2 of the second diaphragm is 6.0 μm to 13.0 μm. 16 . An electric device comprising the secondary battery according to claim 1 .
Citation Information
Cited By
Composite separator, secondary battery, and electric device
CN120033420A
Secondary battery and electronic device
CN120937145A
Secondary battery and electronic device
CN122315276A
Secondary battery and electronic device
WO2026200045A1