Method for extracting, separating, enriching and preparing gallium alum from gallium-containing solution

By using specific extractants and dilute sulfuric acid back-extractants during the extraction and neutralization processes, and controlling the pH value to generate gallium alum, the problem of separating gallium from impurities is solved, achieving efficient gallium extraction and easy-to-filter gallium alum generation, thus improving industrial production efficiency.

CN118910434APending Publication Date: 2024-11-08DANXIA SMELTER OF SHENZHEN ZHONGJIN LINGNAN NONFEMET CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410951623.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-01-25
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In existing technologies, when separating and extracting gallium from gallium-containing solutions, impurities such as zinc, aluminum, and copper are difficult to separate from gallium effectively, resulting in a large number of impurities in the gallium concentrate, which affects industrial production efficiency.

Method used

Extraction is performed using phosphate esters, carboxylic acids, amines, or hydroxyoxime extractants, with dilute sulfuric acid as the back-extraction agent. By controlling the pH value between 2.0 and 2.8 for neutralization, easily filterable gallium ferrite granular crystals are generated. Combined with oil removal and acid separation steps, gallium is separated from impurities.

Benefits of technology

It improves the gallium content of gallium sulfate, solves the problem of gallium being difficult to separate from impurities, and the generated gallium sulfate is easy to filter, thus improving industrial production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910434A_ABST
    Figure CN118910434A_ABST
Patent Text Reader

Abstract

The invention relates to a method for extracting, separating and enriching gallium alum from a gallium-containing solution. The method for extracting, separating, enriching and preparing gallium alum from the gallium-containing solution comprises the following steps: S1, adding an extracting agent, mixing the extracting agent with the gallium-containing solution, and performing 1-6-stage extraction to obtain an organic phase; s2, a dilute sulfuric acid solution with a certain concentration is used for conducting circulating reverse extraction on the organic phase, and gallium-containing reverse extraction liquid is obtained; s3, carrying out acid separation after oil removal treatment to obtain low-acid gallium-containing strip liquor; s4, slowly adding a neutralizer, controlling the reaction temperature to be 50-85 DEG C and the pH value to be 2.0-2.8, reacting for 2-12 hours, and carrying out solid-liquid separation to obtain a gallium alum crude product; and S5, adding pure water, washing at a constant temperature, and carrying out solid-liquid separation to obtain a washed gallium alum finished product. According to the method for extracting, separating, enriching and preparing the gallium alum from the gallium-containing solution, the gallium-containing grade of the gallium alum can be effectively improved, and the problem that gallium is difficult to separate from other amphoteric metal cations due to the fact that the pH values of hydrolytic precipitation are similar is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a method for preparing gallium sulfide by extraction, separation and enrichment from a gallium-containing solution. Background Art

[0002] Gallium (Ga) is one of the important rare metals. Compound semiconductor materials and special alloys composed of metallic gallium and certain metals have become new technology support materials required by contemporary communications, electronic computers, space development, energy and health departments. Gallium is an important rare metal. 90% of the original metallic gallium comes from aluminum smelting, and the rest of the metallic gallium comes from zinc smelting and coal. In addition, comprehensive recovery from secondary resources has also become an important source of gallium. In order to recover the gallium metal, acid solution is usually used to treat it to obtain a gallium-containing leaching solution. At present, the separation and extraction of gallium from gallium-containing acidic leaching solution mainly adopts extraction method, resin adsorption or precipitation method.

[0003] During the extraction process, the content of impurities such as Zn, Al, Cu, and Fe in the leaching solution is generally much higher than the concentration of Ga. Therefore, during the extraction process, the extraction pH of impurities such as Zn, Al, Cu, and Fe is very close to that of Ga. While extracting gallium, impurities such as Zn, Al, Cu, and Fe also partially enter the organic phase. High-concentration sulfuric acid is used as the stripping agent. During the stripping process, gallium is easily stripped into the stripping solution of gallium together with zinc, aluminum, and copper. The stripping rates of zinc and copper are higher than those of gallium, and the stripping rate of aluminum is close to that of gallium. Gallium concentrate is generally obtained by neutralization and hydrolysis precipitation after extraction to obtain gallium-containing stripping solution. However, during hydrolysis precipitation, due to the high stripping acidity, a large amount of neutralizer needs to be added to neutralize the free acid on the one hand, and the activity of gallium in the solution is similar to that of zinc and lower than that of aluminum. In order to precipitate gallium thoroughly, the pH value needs to be increased to 4.5-5.2. Therefore, the gallium concentrate obtained contains a large amount of Al and a small amount of zinc and copper in addition to gallium. Since gallium, aluminum and zinc are all amphoteric elements, the presence of impurity aluminum makes it very difficult to dissolve the gallium concentrate in alkali, and it is even impossible to filter, which seriously restricts its application in industrial production. Summary of the invention

[0004] Based on this, the object of the present invention is to provide a method for extracting, separating, enriching and preparing gallium sulfide from a gallium-containing solution, comprising the following steps:

[0005] S1: extraction, adding an extractant and the gallium-containing solution to mix the two phases and perform 1-6 levels of extraction to obtain an organic phase;

[0006] S2: stripping and enrichment, the organic phase obtained in step S1 is subjected to cyclic stripping using a dilute sulfuric acid solution of a certain concentration to obtain a gallium-containing stripping solution;

[0007] S3: degreasing and acid separation, pumping the gallium-containing stripping solution in step S2 into an acid separation device after degreasing to obtain a low-acid gallium-containing stripping solution;

[0008] S4: Neutralization reaction, slowly adding a neutralizing agent to the low-acid gallium-containing stripping solution obtained in step S3, controlling the reaction temperature to be greater than 50° C. and the pH value to be 2.0-2.8, reacting for 2-12 hours, and performing solid-liquid separation to obtain a crude gallium alum product;

[0009] S5: washing. The gallium alum obtained in step S4 is added with pure water and washed at a constant temperature for a certain period of time, and then the washed finished product of gallium alum is obtained by solid-liquid separation.

[0010] The extractant in step S1 includes one or more of a phosphate extractant, a carboxylic acid extractant, an amine extractant or a hydroxamate extractant. It should be noted that the selection of the extractant is based on the subsequent stripping and the use of dilute sulfuric acid as a stripping agent for gallium to achieve a full sulfuric acid system, which is compatible with the sulfuric acid leaching system of a hydrometallurgical zinc smelting enterprise, avoids the introduction of other impurity ions, and especially avoids the corrosion of chloride ions to the production system equipment.

[0011] See also Figure 1 The present invention provides a method for extracting, separating and enriching gallium sulfide from a gallium-containing solution, using a dilute sulfuric acid solution of a certain concentration as a stripping agent, and the gallium-containing stripping solution obtained by stripping can be circulated for stripping and enrichment when the concentration is lower than the limit value. The stripping solution is deoiled to separate free acid, which can reduce the use of neutralizing agents and reduce the production of industrial salts, as well as the adverse effects of industrial salt byproducts and oil on subsequent processes. The low-acid gallium-containing stripping solution after deoiling accurately controls the reaction pH value between 2.0-2.8, and gallium sulfide can be generated in the presence of cations. The specific reaction is as follows:

[0012] K 2 SO 4 +3Ga 2 (SO 4 ) 3 +12H 2 O=2KGa 3 (SO 4 ) 2 (OH) 6 +6H 2 SO 4

[0013] (NH 4 ) 2 SO 4 +3Ga 2 (SO 4 ) 3 +12H 2 O=2(NH 4 )Ga 3 (SO4 ) 2 (OH) 6 +6H 2 SO 4

[0014] Na 2 SO 4 +3Ga 2 (SO 4 ) 3 +12H 2 O=2NaGa 3 (SO 4 ) 2 (OH) 6 +6H 2 SO 4

[0015] 2H 2 SO 4 +Me 2 CO 3 =2MeSO 4 +2H 2 O+CO 2 (Me:Na + , K + NH 4 + )

[0016] By controlling the pH range, gallium ions can be successfully separated from aluminum ions and zinc ions, thereby improving the gallium content of gallium alum and solving the problem of difficulty in separating gallium from other amphoteric metal cations due to similar pH values ​​of hydrolysis and precipitation.

[0017] Compared with the current neutralization hydrolysis precipitation method commonly used in the industry to prepare gallium alum, the gallium hydroxide directly precipitated by this method is an amorphous colloid, which is difficult to filter and seriously affects the efficiency of industrial production. By using sulfuric acid as the stripping agent and controlling the pH value of the reaction system, gallium only reacts with the neutralizer to generate granular gallium alum, which has a good precipitated crystal form and is easy to filter, thereby improving the efficiency of industrial production.

[0018] Furthermore, in step S2, the loaded organic phase is stripped using a dilute sulfuric acid solution of a certain concentration to obtain a gallium stripping solution. When the stripping solution is lower than 5 g / L, concentrated sulfuric acid is added to circulate the gallium stripping until the gallium concentration of the gallium-containing stripping solution is greater than 5 g / L.

[0019] Preferably, the concentration of dilute sulfuric acid in step S2 is 50-300 g / L.

[0020] Furthermore, the oil removal treatment in step S3 is one or more of air flotation oil removal, ultrasonic oil removal, resin adsorption oil removal, and activated carbon adsorption oil removal. The gallium-containing stripping solution is deoiled until the oil concentration of the gallium-containing stripping solution is less than 5 mg / L. By removing the oil and adhering organic matter at the same time to reduce the organic components in the gallium-containing stripping solution, the filtration speed of the subsequent solid-liquid separation can be increased.

[0021] Furthermore, the concentration of dilute sulfuric acid in the low-acid gallium-containing stripping solution obtained after acid separation in step S3 is less than 20 g / L, which reduces the amount of subsequent neutralizing agent used and avoids the adverse effects of neutralizing agent byproducts on subsequent processes.

[0022] Specifically, in step S3, the gallium-containing stripping solution after degreasing is pumped into a diffusion dialysis membrane device for acid separation; the diffusion dialysis membrane device is internally divided into a dialysis chamber and a diffusion chamber by an anion exchange membrane, the gallium-containing stripping solution obtained by stripping and enrichment in step S2 flows into the dialysis chamber, pure water flows into the diffusion chamber as a receiving liquid, and the acid radical ions in the dialysis chamber pass through the anion exchange membrane into the diffusion chamber. After the diffusion dialysis is completed, the liquid in the dialysis chamber is a low-acid gallium-containing stripping solution, and the liquid in the diffusion chamber is free sulfuric acid. The separated free sulfuric acid can be recycled by adding concentrated sulfuric acid and continued to be used for the cyclic stripping in step S2.

[0023] Furthermore, in step S4, the neutralizing agent is one or more of sodium carbonate, ammonium carbonate, potassium carbonate, sodium bicarbonate, ammonium bicarbonate, potassium bicarbonate, sodium hydroxide, potassium hydroxide and ammonia water. Preferably, the neutralizing agent is preferably ammonium carbonate, sodium carbonate or ammonia water.

[0024] Furthermore, in step S5, the liquid-solid ratio of pure water added is (4-6):1, the temperature of the washing liquid is 45-85°C, and the washing time is 1-2h.

[0025] The beneficial effects of the present invention are:

[0026] (1) By using oil removal and acid separation to accurately precipitate gallium ions, gallium ions can be successfully separated from other amphoteric cations, the gallium content of gallium alum can be improved, and the problem of difficulty in separating gallium from other amphoteric metal cations due to the similar pH values ​​of hydrolysis precipitation can be solved;

[0027] (2) By forming a granular crystal form of gallium alum that is easy to filter, the problem of generating amorphous colloids and causing difficulty in filtering in the traditional method is solved.

[0028] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A flow chart of the method for extracting, separating, enriching and preparing gallium sulfide from a gallium-containing solution provided in this application;

[0030] Figure 2 This is the XRD pattern of the sample prepared in Example 1. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] The leaching solution from the zinc smelting process is taken as a gallium-containing solution, in which the Zn content is 28g / L, the Ga content is 1.2g / L, the Fe content is 0.2g / L, the Al content is 3.2g / L, the Cu content is 16.5g / L, the As content is 0.3g / L, and the H 2 SO 4 The content is 18g / L.

[0034] An extraction system consisting of 5% P204 di(2-ethylhexyl) phosphate + 2% YW100 (C7-9 isohydroxamic acid) + 93% kerosene was added to the gallium-containing solution and five-stage extraction was performed to obtain an organic phase.

[0035] 250 g / L of dilute sulfuric acid was added to the organic phase for 5-stage cyclic stripping to obtain 1 L of gallium-containing stripping solution, in which the Zn content was 1.8 g / L, the Ga content was 15.5 g / L, the Fe content was 0.1 g / L, the Al content was 10.5 g / L, the Cu content was 0.2 g / L, the As content was 0.1 g / L, and the H 2 SO 4 The content is 210g / L and the oil content is 110mg / L.

[0036] The gallium-containing stripping solution is transferred to an oil removal device, and oil is removed by flotation + activated carbon. The gallium-containing stripping solution after oil removal is pumped into an acid separation device for diffusion dialysis separation to obtain a low-acid gallium-containing stripping solution. The low-acid gallium-containing stripping solution has a Zn content of 1.7 g / L, a Ga content of 14.5 g / L, a Fe content of 0.05 g / L, an Al content of 9.8 g / L, a Cu content of 0.1 g / L, an As content of 0.05 g / L, and a H 2 SO 4 The content is 15g / L and the oil content is 5mg / L.

[0037] Sodium carbonate was slowly added to the above-mentioned low-acid gallium-containing stripping solution, the reaction temperature was controlled at 85°C, the pH value was between 2.5-2.8, the reaction was performed for 2 hours, and then filtered. After filtration, 200 mL of pure water was added for washing, and the temperature was kept at 45°C to obtain a gallium alum sample. The sample weighed 37.90 g. The content of each cation in the test sample is shown in Table 1; the sample was subjected to XRD test, and the obtained XRD spectrum is shown in Table 1. Figure 2 It can be seen that the sample prepared by the preparation method of this embodiment meets the characteristic peaks of gallium sulfide.

[0038] Example 2

[0039] The leaching solution from the zinc smelting process is taken as a gallium-containing solution, in which the Zn content is 28g / L, the Ga content is 1.2g / L, the Fe content is 0.2g / L, the Al content is 3.2g / L, the Cu content is 16.5g / L, the As content is 0.3g / L, and the H 2 SO 4 The content is 18g / L.

[0040] An extraction system consisting of 5% P204 di(2-ethylhexyl) phosphate + 2% YW100 (C7-9 isohydroxamic acid) + 93% kerosene was added to the gallium-containing solution and five-stage extraction was performed to obtain an organic phase.

[0041] 300 g / L of dilute sulfuric acid was added to the organic phase for 5-stage cyclic stripping to obtain 1 L of gallium-containing stripping solution, in which the Zn content was 1.87 g / L, the Ga content was 17 g / L, the Fe content was 0.12 g / L, the Al content was 11.3 g / L, the Cu content was 0.22 g / L, the As content was 0.12 g / L, and the H 2 SO 4 The content is 230g / L and the oil content is 107mg / L.

[0042] The gallium-containing stripping solution is transferred to an oil removal device, and oil is removed by flotation + activated carbon. The gallium-containing stripping solution after oil removal is pumped into an acid separation device for diffusion dialysis separation to obtain a low-acid gallium-containing stripping solution. The low-acid gallium-containing stripping solution has a Zn content of 1.81 g / L, a Ga content of 16.1 g / L, a Fe content of 0.09 g / L, an Al content of 10.5 g / L, a Cu content of 0.16 g / L, an As content of 0.08 g / L, and a H 2 SO 4 The content is 18g / L and the oil content is 4mg / L.

[0043] Sodium carbonate was slowly added to the above-mentioned low-acid gallium-containing stripping solution, the reaction temperature was controlled at 85°C, the pH value was between 2.0-2.4, and the reaction was filtered after 2 hours. After filtration, 200 mL of pure water was added for washing, and the temperature was kept at 60°C to obtain a gallium alum sample. The sample weighed 35.80 g. The content of each cation in the test sample is shown in Table 1.

[0044] Example 3

[0045] The leaching solution from the zinc smelting process is taken as a gallium-containing solution, in which the Zn content is 28g / L, the Ga content is 1.2g / L, the Fe content is 0.2g / L, the Al content is 3.2g / L, the Cu content is 16.5g / L, the As content is 0.3g / L, and the H 2 SO 4 The content is 18g / L.

[0046] An extraction system consisting of 15% P204+85% kerosene was added to the gallium-containing solution for three-stage extraction to obtain an organic phase.

[0047] 225 g / L of dilute sulfuric acid was added to the organic phase for 5-stage cyclic stripping to obtain 1 L of gallium-containing stripping solution, in which the Zn content was 6.8 g / L, the Ga content was 11.5 g / L, the Fe content was 0.01 g / L, the Al content was 10.5 g / L, the Cu content was 2.5 g / L, the As content was 0.005 g / L, and the H 2 SO 4 The content is 200g / L and the oil content is 50mg / L.

[0048] The gallium-containing stripping solution is transferred to an oil removal device, and oil is removed by activated carbon. The gallium-containing stripping solution after oil removal is pumped into an acid separation device for diffusion dialysis separation to obtain a low-acid gallium-containing stripping solution. The low-acid gallium-containing stripping solution has a Zn content of 6.5 g / L, a Ga content of 10.5 g / L, a Fe content of 0.005 g / L, an Al content of 10.1 g / L, a Cu content of 1.5 g / L, an As content of 0.005 g / L, and a H 2 SO 4 The content is 16g / L and the oil content is 5mg / L.

[0049] Sodium carbonate was slowly added to the above-mentioned low-acid gallium-containing stripping solution, the reaction temperature was controlled at 50°C, the pH value was between 2.5-2.8, and the reaction was filtered after 12 hours. After filtration, 150 mL of pure water was added for washing, and the temperature was kept at 85°C to obtain a gallium alum sample. The sample weighed 25.45 g. The content of each cation in the test sample is shown in Table 1.

[0050] Example 4

[0051] The leaching solution from the zinc smelting process is taken as a gallium-containing solution, in which the Zn content is 28g / L, the Ga content is 1.2g / L, the Fe content is 0.2g / L, the Al content is 3.2g / L, the Cu content is 16.5g / L, the As content is 0.3g / L, and the H 2 SO 4 The content is 18g / L.

[0052] An extraction system consisting of 25% CA (citric acid)-12+10% sec-octanol+65% kerosene was added to the gallium-containing solution for secondary extraction to obtain an organic phase.

[0053] 50 g / L of dilute sulfuric acid was added to the organic phase for three-stage cyclic stripping to obtain 1 L of gallium-containing stripping solution, in which the Zn content was 6.2 g / L, the Ga content was 11.2 g / L, the Fe content was 0.01 g / L, the Al content was 10.3 g / L, the Cu content was 2.5 g / L, the As content was 0.005 g / L, and the H 2 SO 4 The content is 35g / L and the oil content is 68mg / L.

[0054] The gallium-containing stripping solution is transferred to an oil removal device, and oil is removed by activated carbon. The gallium-containing stripping solution after oil removal is pumped into an acid separation device for diffusion dialysis separation to obtain a low-acid gallium-containing stripping solution. The low-acid gallium-containing stripping solution has a Zn content of 6 g / L, a Ga content of 10.5 g / L, a Fe content of 0.004 g / L, an Al content of 9.9 g / L, a Cu content of 1.6 g / L, an As content of 0.005 g / L, and a H 2 SO 4 The content is 15g / L and the oil content is 5mg / L.

[0055] Sodium carbonate was slowly added to the above-mentioned low-acid gallium-containing stripping solution, the reaction temperature was controlled at 70°C, the pH value was between 2.5-2.8, and the reaction was filtered after 4 hours. After filtration, 120 mL of pure water was added for washing, and the temperature was kept at 85°C to obtain a gallium alum sample. The sample weighed 24.93 g. The content of each cation in the test sample is shown in Table 1.

[0056] Comparative Example 1

[0057] The leaching solution from the zinc smelting process is taken as a gallium-containing solution, in which the Zn content is 28g / L, the Ga content is 1.2g / L, the Fe content is 0.2g / L, the Al content is 3.2g / L, the Cu content is 16.5g / L, the As content is 0.3g / L, and the H 2 SO 4 The content is 18g / L.

[0058] An extraction system consisting of 5% P204 di(2-ethylhexyl) phosphate + 2% YW100 (C7-9 isohydroxamic acid) + 93% kerosene was added to the gallium-containing solution and five-stage extraction was performed to obtain an organic phase.

[0059] 250 g / L of dilute sulfuric acid was added to the organic phase for 5-stage cyclic stripping to obtain 1 L of gallium-containing stripping solution, in which the Zn content was 1.8 g / L, the Ga content was 15.5 g / L, the Fe content was 0.1 g / L, the Al content was 10.5 g / L, the Cu content was 0.2 g / L, the As content was 0.1 g / L, and the H 2 SO 4 The content is 210g / L and the oil content is 110mg / L.

[0060] Sodium carbonate was slowly added to the gallium-containing stripping solution, the reaction temperature was controlled at 55°C, the pH value was between 4.5-5.2, and the reaction was performed after 6 hours of filtration. After filtration, 200 mL of pure water was added for washing, and the temperature was kept at 45°C to obtain gallium hydroxide precipitate. The sample weighed 86.36 g. The content of each cation in the test sample is shown in Table 1.

[0061] Table 1 Cation contents of samples prepared in Examples 1-4 and Comparative Example 1

[0062] project Zn(%) Ga(%) Fe(%) Al(%) Cu(%) As(%) Example 1 0.068 35.09 0.0005 0.79 0.034 0.001 Example 2 0.062 37.01 0.0005 0.78 0.034 0.001 Example 3 0.055 34.19 0.0005 1.57 0.03 0.001 Example 4 0.058 34.89 0.0005 1.6 0.034 0.001 Comparative Example 1 4.2 15.4 0.4 12.2 0.5 0.001

[0063] As can be seen from Table 1, the Ga content in the samples prepared by the preparation methods used in Examples 1-4 is significantly higher than the Ga content in the sample prepared by the traditional method in Comparative Example 1, indicating that after oil removal and acid separation, the gallium ions are accurately precipitated, which can successfully separate the gallium ions from other amphoteric cations, improve the gallium content of gallium alum, and solve the problem of difficulty in separating gallium from other amphoteric metal cations due to similar pH values ​​of hydrolysis precipitation. At the same time, since the granular crystal form of gallium alum is easy to filter, the problem of difficulty in filtering caused by the generation of amorphous colloids in the traditional method is solved.

[0064] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.

Claims

1. A method for extracting, separating and enriching gallium sulfide from a gallium-containing solution, characterized in that: The following steps are involved: S1: adding an extractant and the gallium-containing solution to mix the two phases and perform 1-6 levels of extraction to obtain an organic phase; S2: The organic phase obtained in step S1 is subjected to cyclic stripping using a dilute sulfuric acid solution of a certain concentration to obtain a gallium-containing stripping solution; S3: removing oil from the gallium-containing stripping solution in step S2 and then performing acid separation to obtain a low-acid gallium-containing stripping solution; S4: slowly adding a neutralizing agent to the low-acid gallium-containing stripping solution obtained in step S3, controlling the reaction temperature to 50-85° C. and the pH value to 2.0-2.8, reacting for 2-12 hours, and performing solid-liquid separation to obtain a crude gallium alum product; S5: After the gallium alum obtained in step S4 is added with pure water and washed at a constant temperature for a certain period of time, the washed gallium alum product is obtained by solid-liquid separation.

2. The method for preparing gallium sulfide by extraction, separation and enrichment from a gallium-containing solution according to claim 1, characterized in that: The extractant in step S1 includes one or more of a phosphate extractant, a carboxylic acid extractant, an amine extractant or a hydroxamate extractant.

3. The method for preparing gallium sulfide by extraction, separation and enrichment from a gallium-containing solution according to claim 1, characterized in that: The concentration of dilute sulfuric acid in step S2 is 50-300 g / L.

4. The method for preparing gallium sulfide by extraction, separation and enrichment from a gallium-containing solution according to claim 1, characterized in that: The gallium concentration of the gallium-containing stripping solution obtained in step S2 is greater than 5 g / L.

5. The method for preparing gallium sulfide by extraction, separation and enrichment from a gallium-containing solution according to claim 1, characterized in that: The oil removal in step S3 is one or more of flotation oil removal, ultrasonic oil removal, resin adsorption oil removal, and activated carbon adsorption oil removal; the oil concentration of the gallium-containing stripping solution after oil removal is ≤5 mg / L.

6. The method for preparing gallium sulfide by extraction, separation and enrichment from a gallium-containing solution according to claim 1, characterized in that: The dilute sulfuric acid concentration of the low-acid gallium-containing stripping solution obtained after acid separation in step S3 is less than 20 g / L.

7. The method for preparing gallium sulfide by extraction, separation and enrichment from a gallium-containing solution according to claim 1, characterized in that: The neutralizing agent is one or more of sodium carbonate, ammonium carbonate, potassium carbonate, sodium bicarbonate, ammonium bicarbonate, potassium bicarbonate, sodium hydroxide, potassium hydroxide and ammonia water.

8. The method for preparing gallium sulfide by extraction, separation and enrichment from a gallium-containing solution according to claim 1, characterized in that: In step S5, the liquid-to-solid ratio of pure water added is (4-6):1, the temperature of the washing liquid is 45-85°C, and the washing time is 1-2h.