Electrolyte and lithium ion battery containing same
By using multi-connection nitrogen and sulfur-containing heterocyclic structure compound A as additives in lithium-ion batteries, the safety hazards and energy attenuation of lithium-ion batteries in high-nickel ternary positive electrode material are solved under high temperature and fast charging, and the safety hazards and energy attenuation of lithium-ion batteries are achieved. Excellent high-temperature storage, circulation and low-temperature fast charging performance.
Patent Information
- Application Number
- CN202411181499.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
AI Technical Summary
The lithium-ion battery with high nickel ternary positive electrode material has safety hazards and energy attenuation problems under high temperature and fast charging conditions, and the electrode interface impedance increases when charging at high rates, resulting in lithium-ion and battery inflation.
Using multi-connection of heterocyclic structure compound A with nitrogen and sulfur as an additive, it forms a stable combination of complexes and transition metal ions, reduces interface side reactions, improves lithium ion transport characteristics, and forms a sulfur-containing and nitrogen-containing polymer interface at the negative electrode. , inhibits the decomposition of the SEI interface.
It significantly improves the high-temperature storage and cycling performance of lithium-ion batteries, improves the low-temperature and fast charging performance, and enhances the overall performance and safety of lithium-ion batteries.
Smart Images

Figure CN118919853A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new energy batteries, and in particular relates to an electrolyte and a lithium-ion battery containing the electrolyte. Background Art
[0002] Lithium-ion batteries have been widely used in consumer electronics, electric vehicles, energy storage and other fields due to their high specific energy, long cycle life and environmental friendliness. With the development of transportation and the introduction of the concept of carbon neutrality, the demand for lithium-ion batteries in the electric vehicle (EV) field has increased dramatically. Currently, there is an urgent need for good performance in terms of energy and power density, cycle life, and wide temperature suitability. At present, the mainstream development route of automotive lithium-ion batteries is high-nickel (nickel content > 0.5) ternary positive electrode materials with silicon-carbon negative electrodes. Since high-nickel ternary positive electrode materials have higher specific capacity and silicon-carbon negative electrodes have more lithium removal / lithium insertion capacity, the overall energy density of lithium-ion batteries has exceeded 300wh / kg.
[0003] Although high-nickel ternary cathode materials have the advantages of high reversible specific capacity, low price and environmental friendliness, the increase in nickel content in high-nickel ternary cathode materials leads to a higher discharge voltage of lithium-ion batteries. Therefore, the electrolyte (organic solvent, additive) is more likely to decompose at the interface between the cathode and the electrolyte, thereby generating gas and causing battery bloating. At the same time, the layered structure stability and thermal stability of high-nickel ternary cathode materials are also reduced. In the case of poor material structure stability, high-rate charging is prone to lithium precipitation, which can easily cause battery safety problems. In addition, when lithium-ion batteries with conventional electrolyte systems are charged rapidly with high currents, the electrode interface impedance increases, and lithium ions cannot be effectively embedded in the anode, resulting in lithium precipitation, which in turn causes electrode reaction polarization, a lower discharge platform, and energy decay of lithium-ion batteries, and even brings safety hazards.
[0004] Therefore, it is very challenging to realize the application of high-nickel ternary positive electrode materials, especially lithium-ion batteries with silicon-carbon negative electrode materials. Summary of the invention
[0005] The object of the present invention is to provide an electrolyte and a lithium-ion battery containing the electrolyte, which can effectively improve the fast charging, high temperature and low temperature performance of the lithium-ion battery, and is conducive to the promotion and application of high-nickel ternary positive electrode materials.
[0006] In order to achieve the above object, the present invention provides an electrolyte solution, comprising an electrolyte salt, an organic solvent and an additive. The additive comprises a compound A, and the structural formula of the compound A is shown in structural formula I, structural formula II or structural formula III.
[0007]
[0008] Among them, at least one of X, Y and Z is S, at least one is NR, and R is H or a C1-C6 hydrocarbon group.
[0009] Compared with the prior art, the compound A in the electrolyte of the present invention is a multi-linked heterocyclic structure containing nitrogen and sulfur, which can form a stable complex with transition metal ions through its own coordination bond, alleviate the destructive effect of transition metals on the negative electrode interface film, and thus has better high temperature performance. In addition, compound A can form a sulfur- and nitrogen-containing polymer interface at the negative electrode, which can reduce the interfacial side reactions of the battery during the cycle and storage process, effectively inhibit the decomposition of the SEI interface, and thus improve the high temperature storage and high temperature cycle performance of the lithium ion battery. And the formed interface film has better lithium ion transmission characteristics, which can improve the low temperature and fast charging characteristics.
[0010] As a technical solution of the present invention, the compound A is at least one selected from compounds 1 to 8.
[0011]
[0012]
[0013] As a technical solution of the present invention, the compound A accounts for 0.1 to 5.0% of the mass of the electrolyte.
[0014] As a technical solution of the present invention, the electrolyte salt includes a first electrolyte salt and a second electrolyte salt.
[0015] As a technical solution of the present invention, the first electrolyte salt is 2-trifluoromethyl-4,5-dicyanoimidazole lithium.
[0016] As a technical solution of the present invention, the second electrolyte salt includes at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethylsulfonyl imide), lithium methane sulfonate, lithium trifluoromethyl sulfonate, lithium fluorosulfonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorobis(oxalatophosphate), lithium bis(fluorosulfonyl imide), lithium diphosphate and lithium lower aliphatic carboxylate.
[0017] As a technical solution of the present invention, the first electrolyte salt accounts for 0.01-10.00% of the mass of the electrolyte, and the second electrolyte salt accounts for 8-15% of the mass of the electrolyte.
[0018] As a technical solution of the present invention, the organic solvent is at least one of carbonate, carboxylate and ether compounds.
[0019] In a second aspect of the present invention, a lithium-ion battery is provided, which includes a positive electrode material, a negative electrode material, and the aforementioned electrolyte. The lithium-ion battery of the present invention has excellent fast charging, high-temperature, and low-temperature performance.
[0020] As a technical solution of the present invention, the positive electrode material is LiNi x Co y Mn z M 1-x-y-z O2 or LiNi x Co y Al z M 1-x-y-z O2, where M is any one of Mg, Cu, Zn, Sn, B, Ga, Cr, Sr, V, and Ti, 0.5 ≤ x < 1.0, 0 < y < 1.0, 0 < z < 1.0, and 0.9 < x + y + z ≤ 1.0. Specific Embodiments
[0021] The lithium-ion battery of the present invention is applicable to lithium-ion batteries, especially to lithium-ion batteries with a high-nickel ternary positive electrode material and a silicon-carbon negative electrode material. The lithium-ion battery includes a positive electrode material, a negative electrode material, and an electrolyte. Among them, the positive electrode material is LiNi x Co y Mn z M 1-x-y-z O2 or LiNi x Co y Al z M 1-x--y-z O2, where M is any one of Mg, Cu, Zn, Sn, B, Ga, Cr, Sr, V, and Ti, 0.5 ≤ x < 1.0, 0 < y < 1.0, 0 < z < 1.0, and 0.9 < x + y + z ≤ 1.0. The negative electrode material includes at least one of a carbon-based material, a silicon-based material, a tin-based material, and a lithium negative electrode material. The carbon-based material includes graphite, hard carbon, soft carbon, graphene, and mesophase carbon microspheres, etc. The silicon-based material may include silicon, silicon oxide, silicon-carbon composite material, and silicon alloy material, etc. The tin-based material may include tin, tin-carbon, tin-oxygen, and tin metal compounds. The lithium negative electrode material may include metallic lithium or a lithium alloy. The lithium alloy may be at least one of a lithium-silicon alloy, a lithium-sodium alloy, a lithium-potassium alloy, a lithium-aluminum alloy, a lithium-tin alloy, and a lithium-indium alloy.
[0022] The electrolyte includes an electrolyte salt, an organic solvent, and an additive.
[0023] The additive includes compound A, the structural formula of compound A is shown in structural formula I, structural formula II or structural formula III, wherein at least one of X, Y and Z is S, at least one is NR, and R is H or a C1-C6 hydrocarbon group. The hydrocarbon group is an alkyl, alkenyl or alkynyl group. Further, R is H or a C1-C3 hydrocarbon group. Further, R is H, an alkyl, ethylene, propyl, isopropyl, vinyl or ethynyl group. Compound A accounts for 0.1-5.0% of the mass of the electrolyte, and further, compound A accounts for 0.1-3% of the mass of the electrolyte. Illustratively, compound A accounts for 0.1%, 0.2%, 0.5%, 0.8%, 1.0%, 1.5%, 2.0%, 2.2%, 2.5%, 3.0%, 3.2%, 3.5%, 3.8%, 4.0%, 4.2%, 4.5%, 4.8%, and 5% of the total mass of the electrolyte, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024]
[0025] Compound A is at least one selected from Compound 1 to Compound 8.
[0026]
[0027] CAS:88537-32-0CAS:1228819-48-4CAS:59958-32-6CAS:122833-64-1
[0028]
[0029] CAS:2135689-03-9CAS:79461-38-4CAS:59958-34-8CAS:59958-33-7
[0030] The organic solvent is at least one of carbonate, carboxylic acid ester and ether compounds. Carbonate is cyclic carbonate and / or chain carbonate. Cyclic carbonate can be but not limited to ethylene carbonate (EC), propylene carbonate, butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC) or their derivatives. Chain carbonate includes but is not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC) and propylene carbonate (PC). Carboxylic acid ester is cyclic carboxylic acid ester and / or chain carboxylic acid ester, and cyclic carboxylic acid ester can be but not limited to at least one of γ-butyrolactone, γ-valerolactone and δ-valerolactone. Chain carboxylic acid ester can be but not limited to at least one of methyl acetate (MA), ethyl acetate (EA), propyl acetate (EP), butyl acetate, propyl propionate (PP) and butyl propionate. The ether compound includes cyclic ether or chain ether, and the cyclic ether may be, but is not limited to, at least one of 1,3-dioxolane (DOL), 1,4-dioxolane (DX), crown ether, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-CH3-THF) and 2-trifluoromethyltetrahydrofuran (2-CF3-THF). The chain ether may be, but is not limited to, at least one of dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether and diethylene glycol dimethyl ether.
[0031] The electrolyte salt accounts for 5 to 25% of the total mass of the electrolyte. Further, the electrolyte salt accounts for 6 to 20% of the mass of the electrolyte, and preferably, the electrolyte salt accounts for 8 to 18% of the mass of the electrolyte. As an example, the electrolyte salt accounts for 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25% of the mass of the electrolyte. However, it is not limited to the listed values, and other unlisted values within the numerical range are also applicable. The electrolyte salt includes a first electrolyte salt and a second electrolyte salt. The first electrolyte salt is 2-trifluoromethyl-4,5-dicyanoimidazole lithium (LiTDI). The second electrolyte salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium bis(trifluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium methanesulfonate (LiCH3SO3), lithium trifluoromethylsulfonate (LiCF3SO3), lithium fluorosulfonate (LiSO2F), lithium bis(oxalate)borate (LiBC4O8), lithium difluorooxalate borate (LiBF2C2O4), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalate)phosphate (LiDFBP), lithium diphosphate (LiPO2F2), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and lower aliphatic lithium carboxylates. Further, lower aliphatic lithium carboxylates include but are not limited to lithium chloroborane, lithium tetraphenylborate, lithium imide salts, etc. The first electrolyte salt accounts for 0.01-10.00% of the mass of the electrolyte. For example, the first electrolyte salt may account for, but is not limited to, 0.01%, 0.10%, 1.00%, 3.00%, 5.00%, 8.00%, or 10.00% of the mass of the electrolyte. The second electrolyte salt accounts for 5-15% of the mass of the electrolyte. For example, the second electrolyte salt may account for, but is not limited to, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, or 15% of the mass of the electrolyte.
[0032] In order to further illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific examples. It should be noted that, if specific conditions are not specified in the examples and comparative examples, they can be carried out according to conventional conditions or conditions recommended by the manufacturer, and if the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0033] Example 1
[0034] 1.1 Preparation of electrolyte
[0035] In a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a mass ratio of 2:5:3 to obtain a mixed solvent as an organic solvent, and then additives are added to obtain a mixed solution. The mixed solution is sealed and packaged and placed in a quick freezer (-4°C) for 2 hours, then taken out, and in a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), electrolyte salts are slowly added to the mixed solution and mixed evenly to obtain an electrolyte.
[0036] 1.2 Preparation of positive electrode
[0037] The ternary material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 96.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for current collector. The coating amount is 324g / m 2 , dried at 85°C and then cold pressed; then trimmed, cut into pieces, and slit, and after slitting, dried at 85°C for 4 hours under vacuum conditions, and the tabs were welded to make lithium-ion battery positive electrodes that meet the requirements.
[0038] 1.3 Preparation of negative electrode
[0039] Artificial graphite and silicon oxide material (SiO) are mixed in a mass ratio of 90:10, and then mixed with conductive agent SuperP, thickener CMC, and adhesive SBR (styrene-butadiene rubber latex) in a mass ratio of 95:1.5:1.0:2.5 to make a slurry. The mixture is evenly coated on both sides of the copper foil, and then dried and rolled to make a lithium-ion battery negative electrode sheet that meets the requirements.
[0040] 1.4 Preparation of lithium-ion batteries
[0041] The positive electrode sheet, negative electrode sheet and diaphragm prepared according to the above process were laminated to form a lithium-ion battery with a thickness of 4.7mm, a width of 55mm and a length of 60mm. They were vacuum-baked at 75°C for 10h and the electrolyte prepared in 1.1 was injected. After standing for 24h, they were charged to 4.45V with a constant current of 0.1C (180mA), and then charged at a constant voltage of 4.45V until the current dropped to 0.05C (90mA); then discharged to 3.0V with 0.2C (180mA), and the charge and discharge were repeated twice. Finally, the battery was charged to 3.8V with 0.2C (180mA) to complete the production of the lithium-ion battery.
[0042] The components and contents of the electrolytes of Examples 1 to 15 and Comparative Examples 1 to 5 are shown in Table 1, wherein the preparation processes of the lithium ion battery electrolytes, positive electrode sheets, negative electrode sheets, and lithium ion batteries of Examples 1 to 15 and Comparative Examples 1 to 5 are the same as those of Example 1.
[0043] Table 1 Compositions of the electrolytes of the embodiments and comparative examples
[0044] Example Electrolyte salt / (mass, g) Organic solvent (mass, g) Additives (mass, g) Example 1 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 1 / 1.0 Example 2 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 2 / 1.0 Example 3 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 3 / 1.0 Example 4 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 4 / 1.0 Example 5 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 5 / 1.0 Example 6 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 6 / 1.0 Example 7 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 7 / 1.0 Example 8 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 8 / 1.0 Example 9 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.5 Compound 2 / 0.5 Example 10 <![CDATA[LiPF6 / 6.5+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 85.5 Compound 2 / 2.0 Embodiment 11 <![CDATA[LiPF6 / 6.5+LiTDI / 5.5]]> EC / EMC / DEC(2:5:3) / 85.0 Compound 2 / 3.0 Example 12 <![CDATA[LiPF6 / 6.0+LiTDI / 4.5]]> EC / EMC / DEC(2:5:3) / 84.5 Compound 2 / 5.0 Embodiment 13 <![CDATA[LiPF6 / 13.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 1 / 1.0 Embodiment 14 LiTDI / 13.0 EC / EMC / DEC(2:5:3) / 86.0 Compound 1 / 1.0 Embodiment 15 LiTDI / 8.5+LiFSI / 3.5 EC / PC / EMC / DEC(2:1:4:2) / 87.0 Compound 1 / 1.0 Comparative Example 1 <![CDATA[LiPF6 / 13.0]]> EC / EMC / DEC(2:5:3) / 87.0 Comparative Example 2 LiTDI / 13.0 EC / EMC / DEC(2:5:3) / 87.0 Comparative Example 3 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 87.0 Comparative Example 4 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 9 / 1.0 Comparative Example 5 <![CDATA[LiPF6 / 7.0+LiTDI / 6.0]]> EC / EMC / DEC(2:5:3) / 86.0 Compound 10 / 1.0
[0045]
[0046] CAS:110-02-1CAS:109-97-7
[0047] The lithium ion batteries prepared in Examples 1 to 15 and Comparative Examples 1 to 5 were subjected to high temperature storage performance test, high temperature cycle performance test, room temperature fast charging performance test, high temperature fast charging performance test, and low temperature performance test under the following conditions. The results are shown in Table 2.
[0048] (1) High temperature storage performance test
[0049] At room temperature (25°C), the lithium-ion battery was charged and discharged at 0.5C / 0.5C (the battery discharge capacity was recorded as C0), with an upper limit voltage of 4.4V, and then the battery was charged to 4.4V under 0.5C constant current and constant voltage conditions, and the battery thickness was measured (the thickness was recorded as D0); the battery was placed in a 60°C oven for 30 days, taken out and the battery thickness was measured (the thickness was recorded as D1); the battery was placed in a 25°C environment and discharged at 0.5C (the discharge capacity was recorded as C1); the lithium-ion battery was continued to be charged and discharged at room temperature (25°C) at 0.5C / 0.5C (the battery discharge capacity was recorded as C2), with an upper limit voltage of 4.4V, and the capacity retention rate, capacity recovery rate and thickness expansion rate were calculated.
[0050] Capacity retention rate = (C1 / C0)*100%
[0051] Capacity recovery rate = (C2 / C0)*100%
[0052] Thickness expansion rate = (D1 / D0)*100%
[0053] (2) High temperature cycle test
[0054] Under high temperature (45°C) conditions, the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 1.0C / 1.0C for 400 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0055] Capacity retention rate = (C1 / C0)*100%
[0056] (3) Room temperature fast charging performance test
[0057] At room temperature (25°C), the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 4.0C / 1.0C for 500 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0058] Capacity retention rate = (C1 / C0)*100%
[0059] (4) High temperature fast charging performance test
[0060] Under high temperature (45°C) conditions, the lithium-ion battery is charged and discharged at 1.0C / 1.0C once (the battery discharge capacity is C0) with an upper voltage of 4.4V, and then charged and discharged at 4.0C / 1.0C for 500 cycles at room temperature (the battery discharge capacity is C1), and the capacity retention rate is calculated.
[0061] Capacity retention rate = (C1 / C0)*100%
[0062] (5) Low temperature performance test
[0063] At room temperature (25°C), the lithium-ion battery is charged and discharged at 0.5C / 0.5 (battery cut-off voltage is 3.0V, discharge capacity is C0), and the upper limit voltage is 4.4V (cut-off current 0.05C). Then the battery is fully charged to 4.4V (cut-off current 0.05C) at 0.5C at room temperature (25°C), and then the battery is transferred to -20°C and left for 4h, and discharged to 3.0V at 0.5C, and the discharge capacity is C1. The capacity retention rate is calculated.
[0064] Capacity retention rate = (C1 / C0)*100%
[0065] Table 2 Electrochemical performance test results of lithium-ion batteries in each example
[0066]
[0067] From the results in Table 2, it can be seen that the electrochemical performance of the secondary batteries of Examples 1 to 15 is better than that of Comparative Examples 1 to 5. This may be because Examples 1 to 15 contain Compound A, which is a multi-linked nitrogen and sulfur heterocyclic structure. It can form a stable complex with the transition metal ions in the ternary positive electrode material through its own coordination bond, thereby alleviating the destructive effect of the transition metal on the negative electrode interface film, and thus has better high temperature performance. In addition, Compound A can form a sulfur- and nitrogen-containing polymer interface at the negative electrode, which can reduce the interfacial side reactions of the battery during the cycle and storage process, effectively inhibit the decomposition of the SEI interface, and thus improve the high temperature storage and high temperature cycle performance of the lithium-ion battery. And the formed interface film has excellent lithium ion transmission characteristics, which can improve low temperature and fast charging characteristics.
[0068] Although Comparative Example 4 contains thiophene (a sulfur-containing heterocyclic compound), the "tunneling" effect of the compound's chemical product during normal use of the battery causes the lithium-ion battery to produce a large self-discharge during high-temperature storage, resulting in poor high-temperature storage performance.
[0069] Comparative Example 5 containing pyridine (a nitrogen-containing heterocyclic compound) has no significant effect on high-temperature storage and high-temperature cycling. This may be because pyridine is weakly alkaline, which has a certain stabilizing effect on the electrolytic acid value, but pyridine does not improve the high temperature and high-temperature storage performance of the electrolyte. It may be that the interface formed by pyridine does not completely protect the electrode, resulting in continuous side reactions at the battery interface and poor high-temperature stability of the battery.
[0070] By comparing Example 1 and Examples 13 to 14, it can be seen that when the electrolyte salt is a mixture of LiTDI and LiFSI, the performance of the lithium-ion battery is the best. This may be because LiTDI has better thermal stability and can improve the life and fast charging performance of the lithium-ion battery, while the addition of LiFSI can make up for the defect of poor cycle stability of the ternary high-nickel battery caused by the low degree of dissociation of LiTDI in the electrolyte.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An electrolyte comprising an electrolyte salt, an organic solvent and an additive, It is characterized in that The additive includes compound A, the structural formula of the compound A is shown in structural formula I, structural formula II or structural formula III, Among them, at least one of X, Y, and Z is S, at least one is NR, and R is H or C 1 ~C 6 of hydrocarbon groups.
2. The electrolyte according to claim 1, It is characterized in that The compound A is selected from at least one of compounds 1 to 8:
3. The electrolyte according to claim 1, It is characterized in that The compound A accounts for 0.1-5.0% of the mass of the electrolyte.
4. The electrolyte according to claim 1, It is characterized in that The electrolyte salt includes a first electrolyte salt and a second electrolyte salt.
5. The electrolyte according to claim 4, It is characterized in that The first electrolyte salt is 2-trifluoromethyl-4,5-dicyanoimidazole lithium.
6. The electrolyte according to claim 4, It is characterized in that The second electrolyte salt includes at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethylsulfonyl imide, lithium methanesulfonate, lithium trifluoromethylsulfonate, lithium fluorosulfonate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorobisoxalatophosphate, lithium bisfluorosulfonyl imide, lithium diphosphate and lithium lower aliphatic carboxylate.
7. The electrolyte according to claim 1, It is characterized in that The first electrolyte salt accounts for 0.01-10.00% of the mass of the electrolyte, and the second electrolyte salt accounts for 5-15% of the mass of the electrolyte.
8. The electrolyte according to claim 1, It is characterized in that The organic solvent is at least one of carbonate, carboxylate and ether compounds.
9. A lithium ion battery, It is characterized in that The invention comprises a positive electrode material, a negative electrode material and the electrolyte according to any one of claims 1 to 8.
10. The lithium ion battery according to claim 9, It is characterized in that The positive electrode material is LiNi x Co y Mn z M 1-x-y-z O 2 or LiNi x Co y Al z M 1-x-y-z O 2 , where M is any one of Mg, Cu, Zn, Sn, B, Ga, Cr, Sr, V and Ti, 0.5≤x<1.0, 0 <y<1.0,0<z<1.0,0.9<x+y+z≤1.0。