Separating membrane, secondary battery, sodium supplementing method of secondary battery, battery module, battery pack and electric device

By adding sodium supplementation agent to the isolation film of the sodium battery and decomposing it into sodium ions during the battery charge and discharge cycle, the problem of sodium ions loss during the first charge and discharge of the sodium battery is solved, and the battery capacity and cycle life are improved.

CN118943653APending Publication Date: 2024-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202310521475.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the first charging and discharging process, sodium ions are lost due to the formation of the solid electrolyte membrane on the negative electrode surface, resulting in low efficiency and irreversible capacity loss of the battery for the first time, limiting the battery capacity and cycle life.

Method used

Design an isolation film with sodium supplementation agent in the coating, which decomposes into sodium ions and removes the isolation film during the charge and discharge cycle of the battery. By heating up, the by-products are removed from the battery, thereby compensating for lost active sodium ions and improving battery capacity and circulation. life.

Benefits of technology

It effectively compensates for the loss of sodium ions during the first charge and discharge, improves the capacity and cycle life of the battery, and at the same time, the release of by-products does not adversely affect the positive and negative electrode sheets and electrolytes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943653A_ABST
    Figure CN118943653A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to an isolating membrane, a secondary battery and a sodium supplementing method thereof, a battery module, a battery pack and an electric device, the isolating membrane comprises a base membrane and a coating located on at least one side surface of the base membrane, and the coating comprises a sodium supplementing agent. The isolating membrane with the structure and the composition is assembled together with a positive pole piece and a negative pole piece according to a conventional battery assembly process of the battery, the sodium supplementing agent is decomposed into sodium ions and by-products capable of being separated from the isolating membrane during charging and discharging cycles of the battery, and the by-products are separated from the sodium battery during heating after formation is finished. The by-products are separated from the battery as much as possible, the content of the residual by-products in the battery is limited, and / or the influence on positive and negative electrode materials or electrolyte is small, and decomposed sodium ions are used for compensating active sodium ions lost in the first charge-discharge cycle, so that the capacity and cycle life of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to an isolation membrane, a secondary battery and a sodium replenishment method thereof, a battery module, a battery pack and an electrical device. Background Art

[0002] As the application of lithium-ion battery technology in consumer electronics, electric vehicles, energy storage and other markets gradually expands, the problem of insufficient lithium resources has also begun to emerge. Sodium batteries have gradually attracted attention due to their abundant reserves of sodium elements, and have an important strategic position in application fields with high cost requirements such as energy storage. Secondly, sodium batteries have higher conductivity than lithium batteries under the same electrolyte concentration, which further reduces production costs.

[0003] Due to some irreversible reactions such as the formation of the solid electrolyte film (SEI film) on the negative electrode surface during the initial charge and discharge process, the positive electrode material will lose sodium ions, resulting in low initial coulombic efficiency of the entire battery. The huge irreversible capacity loss has limited the improvement of battery capacity and cycle life. Summary of the invention

[0004] In view of the above problems, the present application provides an isolation membrane, a secondary battery and a sodium replenishment method thereof, a battery module, a battery pack and an electrical device, which are used to alleviate the problem of capacity loss and cycle performance degradation caused by the irreversible reaction of the negative electrode during the first charge and discharge cycle of the sodium battery.

[0005] In a first aspect, the present application provides an isolation film, the isolation film comprising:

[0006] Basement membrane;

[0007] A coating layer, located on at least one side surface of the base film;

[0008] The coating contains a sodium supplement, which decomposes into sodium ions and byproducts that can escape from the isolation membrane during the battery charge and discharge cycle.

[0009] The separator with the above structure and composition is assembled with the positive electrode sheet and the negative electrode sheet according to the conventional battery assembly process to form a sodium battery. During the battery charge and discharge cycle, the sodium supplement is decomposed into sodium ions and byproducts that can escape from the separator. The byproducts escape from the sodium battery during the temperature rise after the formation. On the one hand, the byproducts will not have a bad impact on the positive and negative electrode sheets and the electrolyte. On the other hand, the byproducts escape from the battery as much as possible, and the residual byproduct content in the battery is limited and / or the impact on the positive and negative electrode materials or the electrolyte is small. The decomposed sodium ions are used to compensate for the active sodium ions lost in the first charge and discharge cycle, which is beneficial to improve the capacity and cycle life of the battery.

[0010] In some embodiments, the sodium supplement agent decomposes into sodium ions and byproducts that can escape from the isolation membrane during the first charge and discharge cycle of the battery.

[0011] In some embodiments, the by-product comprises a gas at normal temperature and pressure and / or a liquid with a boiling point of less than or equal to 100°C.

[0012] In some embodiments, the gas comprises one or a combination of two or more of nitrogen, carbon dioxide, gaseous alkanes, hydrogen sulfide, and hydrogen fluoride;

[0013] The liquid comprises water, liquid alkane, or a combination of two or more thereof.

[0014] In some embodiments, the gaseous alkane comprises one or a combination of two or more of methane, ethane, propane, n-butane, and isobutane.

[0015] In some embodiments, the liquid alkane comprises one or a combination of two or more of n-pentane, isopentane, neopentane, n-hexane, 2,2-dimethylbutane, 2-methylpentane, 2,3-dimethylbutane, 3-methylpentane, and isomers of heptane.

[0016] In some embodiments, the sodium supplement comprises one or a combination of two or more inorganic sodium supplements or organic sodium supplements.

[0017] In some embodiments, the inorganic sodium supplement comprises one or a combination of two or more of sodium nitride, sodium azide, sodium sulfide, sodium oxide, sodium peroxide, sodium fluoride or sodium carbonate;

[0018] The organic sodium supplement comprises Na2C x O y , RCOONa; and x, y contain natural numbers from 2 to 8; R contains one or a combination of two or more of H, C1 to C5 alkane groups.

[0019] In some embodiments, the Na2C x O y Here x is 2 and y is 4.

[0020] In some embodiments, R in the RCOONa comprises one or a combination of two or more of H, methyl, ethyl, n-propyl, and isopropyl.

[0021] In some embodiments, the sodium supplement comprises one or a combination of two or more of sodium nitride, sodium oxalate, sodium formate, sodium acetate, sodium propionate, sodium butyrate, and sodium isobutyrate.

[0022] In some embodiments, the mass of the sodium supplement accounts for 1% to 10% of the mass of the coating, preferably 3% to 6%.

[0023] In some embodiments, the coating layer comprises a filler, and the filler comprises one or a combination of two or more of an inorganic filler, an organic filler, and an organic-inorganic hybrid filler.

[0024] In some embodiments, the coating further comprises a binder, and the binder comprises one or a combination of two of polyacrylate, acrylic resin, polystyrene butadiene copolymer, and fluorine-containing olefin monomer homopolymer or copolymer.

[0025] In some embodiments, the coating further comprises a wetting agent, the wetting agent comprises one or a combination of two or more of alcohols and nitrogen-containing amines, the alcohol comprises one or a combination of two or more of methanol, ethanol, propanol, ethylene glycol, glycerol, and 1,3-propylene glycol, and the nitrogen-containing amine comprises one or a combination of two or more of dimethylformamide, methylpyrrolidone, and ethylpyrrolidone.

[0026] In a second aspect, the present application provides a secondary battery, which includes a positive electrode plate, a negative electrode plate, an electrolyte, and the isolation membrane described in the first aspect.

[0027] In a third aspect, the present application provides a method for replenishing sodium of the secondary battery of the second aspect, the method comprising: after the formation process is completed, heating is performed to allow byproducts of decomposition of the sodium replenisher to escape from the battery.

[0028] Among them, the battery charge and discharge cycle described in the first aspect includes a formation process and a temperature increase. Under the formation process of the present application, the gaseous substances in the decomposition byproducts of the sodium supplement are easier to escape from the sodium battery, and part of the liquid substances, such as alkanes with low boiling points, are also escaped. The remaining part needs to be escaped with the help of temperature increase.

[0029] In some embodiments, the heating comprises a heating rate of 0.5°C / min to 2°C / min, and the temperature is heated to 50°C to 100°C and then kept warm for a period of time.

[0030] In some embodiments, the heating comprises heating at a rate of 0.8°C / min to 1.8°C / min, heating to 55°C to 90°C, and then maintaining the temperature for 1h to 5h.

[0031] In some embodiments, the heating is performed at a pressure no higher than standard atmospheric pressure.

[0032] In some embodiments, the environment no higher than standard atmospheric pressure comprises a negative pressure of 0.01 MPa to 0.1 MPa.

[0033] In a fourth aspect, the present application provides a battery module, wherein the battery module comprises the secondary battery described in the second aspect or the secondary battery made by the sodium supplementation method described in the third aspect.

[0034] In a fifth aspect, the present application provides a battery pack, comprising the battery module described in the fourth aspect.

[0035] In a sixth aspect, the present application provides an electrical device, which comprises the isolation membrane described in the first aspect, the secondary battery described in the second aspect, the secondary battery made by the sodium supplementation method described in the third aspect, the battery module described in the fourth aspect, or the battery pack described in the fifth aspect.

[0036] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0038] Figure 1 This is a schematic diagram of the structure of the isolation membrane in some embodiments of the present application;

[0039] The reference numerals in the specific implementation manner are as follows:

[0040] 100, isolation film; 110, base film; 120, coating; 1201, sodium supplement;

[0041] Coordinate axis z direction: isolation film thickness direction;

[0042] Coordinate axis x direction: length or width direction of the isolation film. DETAILED DESCRIPTION

[0043] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0045] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined. Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0046] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0047] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0048] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0049] The content of lithium in the earth's crust is only 0.0065%, while the content of sodium in the earth's crust is as high as 2.64%. Compared with lithium-ion batteries composed of scarce elements such as lithium, cobalt, and nickel, sodium batteries have a natural advantage in cost over lithium batteries. During the first charging process of sodium batteries, along with the decomposition of the electrolyte, the negative electrode will consume a large amount of active ions to participate in the formation of the solid electrolyte membrane (SEI), resulting in a decrease in the coulomb efficiency of the battery in the first week, and the huge irreversible capacity loss has limited the improvement of battery capacity, rate performance and cycle life.

[0050] To solve the above problems, the study found that using capacity compensation technology to replenish the active ions consumed in the formation of SEI during the first week of charging of sodium batteries is one of the more feasible methods to improve the energy density and cycle life of sodium batteries.

[0051] Capacity compensation technology includes pre-sodium treatment of electrodes, such as negative electrode pre-sodium treatment and positive electrode pre-sodium treatment. As the name suggests, the method of pre-sodium treatment of the positive electrode of the battery is called positive electrode pre-sodium treatment, and vice versa is called negative electrode pre-sodium treatment.

[0052] Among them, the negative electrode pre-sodiumization includes the negative electrode electrochemical method and the negative electrode chemical method. The negative electrode electrochemical method is to form a battery with the negative electrode, the sodium source and the electrolyte before the battery is assembled, and the negative electrode is charged, and a certain amount of sodium ions are stored in the negative electrode in advance, and then the negative electrode is assembled into a full battery together with the corresponding positive electrode material. The disadvantage of this method is the problem of disassembly and reassembly of the battery, which makes the entire operation complicated, the process cost is high, and it is not suitable for mass production. The negative electrode chemical method is to carry out an oxidation-reduction reaction between the negative electrode material and metallic sodium or other low-potential sodium-containing chemical reagents to make up for the loss of sodium. Although this solution has a simple process and high sodium supplementation efficiency, the capacity of metallic sodium is very high, and due to technical limitations, the surface capacity of the supplemented sodium source far exceeds the actual required active sodium ion capacity. In addition, sodium foil and other low-potential sodium-containing reagents are highly active and easily react with water, air and other gases in the air. The safety hazard is very large and it is difficult to be compatible with the existing assembly process.

[0053] Positive electrode pre-sodiumization includes sodium-rich positive electrode and positive electrode additive method. Sodium-rich positive electrode is to add supersaturated sodium to the positive electrode material by a certain method, and make the supersaturated sodium irreversibly released into the electrolyte during the cycle to achieve compensation for active sodium ions. For example, using a positive electrode material that can store excess sodium ions, this pre-sodiumization method has almost no negative impact on the structure of the positive electrode material, and the prepared intermediate product has no residue after sodium removal. This is an excellent pre-sodiumization method for sodium ion positive electrode materials that can form supersaturated products, but its special selectivity also makes this method difficult to be widely used. The positive electrode additive method involves mixing a sodium supplement reagent, that is, a positive electrode additive, with a positive electrode material to form a slurry, and coating it on a current collector to form an electrode to achieve the goal of pre-sodiumization. The positive electrode additive is electrochemically oxidized during the first charge and discharge process, thereby irreversibly releasing additional sodium ions to compensate for the active sodium ions lost in the cycle. There are many types of positive electrode additives, including Na2S, NaN3, Na2O, Na2NiO2, NaCrO2, Na3C6H5O7, Na2C6O6, Na2CO3, etc. Different positive electrode additives may also exhibit different performance when used in different batteries. Positive electrode additives have many advantages. First, the positive electrode pre-sodiumization process is simple, and its total cost depends on the cost of the additive material itself. Second, some positive electrode additives have low environmental requirements and are highly compatible with existing battery production processes. In addition, the positive electrode pre-sodiumization can accurately adjust the degree of pre-sodiumization by controlling the dosage, which is simple and safe to operate. However, the disadvantages of pre-sodiumization of the positive electrode include: (1) the addition of sodium supplement will affect the dispersion performance of the positive electrode slurry, causing adverse effects on the positive electrode coating; (2) the sodium supplement layer will leave holes in the electrode after charging, affecting the positive electrode structure and the performance of the positive electrode material; (3) many sodium sources used for sodium supplementation release Na during charging. + , will form non-electrochemically active (or very low activity) excess substances, and the efficiency of this compound sodium source to replenish sodium is very low. Therefore, it is urgent to develop new sodium replenishment materials and methods to solve the above technical problems.

[0054] Based on the above considerations, in order to alleviate the problem of capacity loss and cycle performance attenuation caused by the irreversible reaction of the negative electrode during the first charge and discharge cycle of the sodium battery, the present application provides a sodium battery separator and a sodium replenishment method for assembling the separator to form a sodium battery, wherein the separator comprises a base film and a coating located on at least one side of the base film, the coating comprises a sodium replenisher, and the separator having the structure and composition is assembled with the positive electrode sheet and the negative electrode sheet according to the conventional battery assembly process to form a sodium battery. During the battery charge and discharge cycle, the sodium replenisher decomposes into sodium ions and byproducts that can escape from the separator, and the byproducts escape from the sodium battery during the temperature rise after the formation. On the one hand, the byproducts will not have a bad effect on the positive and negative electrode sheets and the electrolyte, and on the other hand, the byproducts are removed from the battery as much as possible, the residual byproduct content in the battery is limited and / or the impact on the positive electrode material or the electrolyte is small, and the decomposed sodium ions are used to compensate for the active sodium ions lost in the first charge and discharge cycle, thereby helping to improve the capacity and cycle life of the battery.

[0055] Isolation film

[0056] According to some embodiments of the present application, the present application provides an isolation film, such as Figure 1 As shown, the isolation membrane 100 includes a base membrane 110 and a coating 120 located on at least one side of the base membrane. The coating 120 includes a sodium supplementer 1201. The sodium supplementer 1201 decomposes into sodium ions and byproducts that are easily removed from the isolation membrane 100 during the charge and discharge cycle of the sodium battery.

[0057] Among them, at least one side includes forming a coating on one side surface or both sides of the base film, and the coating is formed in any conventional form in the art, such as coating, deposition, etc. The coating contains a sodium supplement, and the sodium supplement is formed in the coating in any conventional form in the art. The byproducts of the sodium supplement decomposition are easily removed, including that the byproducts can be removed from the isolation membrane at room temperature and pressure. Further, the byproducts can be removed from the battery at room temperature and pressure and / or removed from the battery with the help of an external environment, such as a certain temperature or pressure, and removed from the battery as much as possible, such as a small amount of residual byproducts in the battery, which is basically negligible, or a small amount of content that basically does not have an adverse effect on the positive and negative poles or electrolyte of the battery.

[0058] Therefore, the addition of a sodium supplement to the isolation membrane in the present application is beneficial for compensating for the active sodium ions lost in the first charge and discharge cycle, and can also reduce the probability of the sodium supplement having an adverse effect on the positive and negative electrodes or the electrolyte, etc. Therefore, the isolation membrane designed in the present application can easily achieve the technical purpose of increasing the capacity and cycle life of the battery.

[0059] According to some embodiments of the present application, the by-product comprises gas at normal temperature and pressure and / or a liquid with a boiling point less than or equal to 100°C.

[0060] The normal temperature and pressure here include the conventional descriptions of temperature and pressure in this field. For example, it usually refers to a temperature of about 25°C and a pressure of one atmosphere. The specific types of gas and liquid need to be defined in conjunction with the type of sodium supplement. The gas can escape from the isolation membrane and further escape from the battery at normal temperature and pressure, and the liquid can also easily escape from the battery with the help of an external environment. The boiling point of the liquid is less than or equal to 100°C. Part of it can escape during the formation process of sodium battery assembly, and the remaining part can also easily escape from the battery with the help of an external environment. The external environment matches the physical and chemical properties of the liquid and / or gas, and has little effect on battery performance, which can be ignored.

[0061] Specifically, the gas includes one or more combinations of nitrogen, carbon dioxide, gaseous alkanes, hydrogen sulfide, and hydrogen fluoride; wherein the gaseous alkanes include one or more combinations of methane, ethane, propane, n-butane, isobutane, etc., and the liquid includes one or more combinations of water and liquid alkanes, wherein the liquid alkanes include one or more combinations of n-pentane, isopentane, neopentane, n-hexane, 2,2-dimethylbutane, 2-methylpentane, 2,3-dimethylbutane, 3-methylpentane, and isomers of heptane, and the isomers of heptane include any conventional form of isomers in this application. The gas or liquid escapes from the isolation membrane and further escapes from the battery, and has little effect on the isolation membrane, electrolyte, positive and negative electrodes, and even the battery, which can be ignored.

[0062] According to some embodiments of the present application, the sodium supplement comprises one or a combination of two or more inorganic sodium supplements or organic sodium supplements.

[0063] The sodium supplement can be a compound composed of any one of an inorganic sodium supplement or an organic sodium supplement, or a mixture of two or more combinations. The inorganic sodium supplement and / or organic sodium supplement can be decomposed into sodium ions and byproducts that are convenient to be removed from the battery during the first charge and discharge cycle of the sodium battery.

[0064] According to some embodiments of the present application, the inorganic sodium supplement comprises one or a combination of two or more of sodium nitride, sodium azide, sodium sulfide, sodium oxide, sodium peroxide, sodium fluoride or sodium carbonate.

[0065] The types of inorganic sodium supplements listed above decompose into sodium ions and byproducts that are easy to remove from the battery during the first charge and discharge cycle of the sodium battery. The byproducts include nitrogen, hydrogen sulfide, hydrogen fluoride, carbon dioxide and a small amount of water. Among them, nitrogen, hydrogen sulfide, hydrogen fluoride and carbon dioxide are all in gaseous form at room temperature and pressure, which are easy to remove from the battery. A small amount of water is directly dissolved in the electrolyte. Due to the small amount of water, the impact on the electrolyte or positive and negative electrode materials is small and can be ignored. For example, the decomposition principle of sodium nitride is as follows:

[0066]

[0067] According to some embodiments of the present application, the organic sodium supplement comprises Na2C x O y , RCOONa; and x, y contain natural numbers from 2 to 8; R contains one or a combination of two or more of H, C1 to C5 alkane groups.

[0068] For example, the molecular formula of organic sodium supplement is Na2C x O y The type of sodium supplement needs to consider its decomposition into sodium ions and byproducts that are easy to escape from the battery during the first charge and discharge cycle of the sodium battery. The specific types include but are not limited to any one or a combination of two or more of Na2C3O3, Na2C4O4, Na2C5O5, Na2C6O6, Na2C2O4 (sodium oxalate), Na2C3O5, Na2C4O6, Na2C5O7, and Na2C6O8. x O y The byproducts generated by the decomposition of the sodium supplement during the first charge and discharge cycle of the sodium battery include carbon dioxide.

[0069] For another example, the type of sodium supplement with the molecular formula RCOONa in the organic sodium supplement also needs to consider that it decomposes into sodium ions and byproducts that are convenient to be removed from the battery during the first charge and discharge cycle of the sodium battery. The specific types include but are not limited to any one or a combination of two or more of sodium formate, sodium acetate, sodium propionate, sodium butyrate, sodium isobutyrate, sodium valerate, sodium isovalerate, and sodium pivalate. The types of organic sodium supplements listed in this application decompose into sodium ions and byproducts that are convenient to be removed from the battery during the first charge and discharge cycle of the sodium battery. The byproducts include carbon dioxide, small molecule alkanes, and a small amount of water, wherein the small molecule alkanes are gaseous or liquid at room temperature and pressure, and the boiling point of the liquid small molecule alkanes is less than or equal to 100°C. During the first charge and discharge cycle of the sodium battery, such as a certain temperature and pressure environment of the formation process, a part of the battery is removed, and the remaining part is also easily removed from the battery with the help of an external environment.

[0070] At the same time, the decomposition principle of the sodium supplement with the molecular formula RCOONa is the Korber reaction.

[0071]

[0072] and / or;

[0073]

[0074] In the above molecular formula, R, R1 and R2 include one or a combination of two or more of H and C1-C5 alkanes, and R1 and R2 are different.

[0075] In some of the following embodiments, this application lists in detail any one of the inorganic sodium supplement (sodium nitride) and organic sodium supplement (sodium oxalate, sodium formate, sodium acetate, sodium propionate, sodium butyrate, sodium isobutyrate) as a sodium supplement for preparing an isolation membrane, and explores the specific effects on battery performance.

[0076] According to some embodiments of the present application, the mass of the sodium supplementer accounts for 1% to 10% of the mass of the coating.

[0077] The content of the sodium supplement affects the effect of sodium supplementation. At the same time, it is also necessary to consider whether the decomposed by-products can be conveniently and promptly discharged from the battery, and whether it affects the function of the isolation membrane itself. The actual calculation method of the sodium supplement content is calculated according to the actual addition amount during the preparation of the isolation membrane. This application limits the mass of the sodium supplement to 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10% of the coating mass or any one of the above range values. When the mass proportion is less than 1%, the improvement of battery performance is not ideal. When the mass proportion is higher than 10%, the excess sodium supplement affects the function of the isolation membrane itself, such as reduced air permeability. The distribution form of the sodium supplement in the coating includes uniform and uneven distribution, and the uneven distribution includes gradient distribution, etc.

[0078] According to some embodiments of the present application, the mass of the sodium supplementer is limited to 3% to 6% of the mass of the coating. The isolation membrane prepared by the sodium supplementer containing this content has a relatively ideal effect on improving battery performance, and has a relatively small impact on the function of the isolation membrane itself, that is, the comprehensive performance evaluation of the isolation membrane is relatively excellent. For example, some of the following embodiments explore in detail the effect of the sodium supplementer on the air permeability and thermal shrinkage of the isolation membrane. The results of the exploration show that the sodium supplementer added in the present application has a small effect on the air permeability and thermal shrinkage of the isolation membrane, and can achieve a good performance of the isolation membrane's own function.

[0079] The air permeability here belongs to the performance test index of the isolation membrane, which can indirectly reflect the permeability of ions. The membrane industry usually uses the Gurley value as the evaluation standard, which refers to the time it takes for a certain volume of air to pass through a specified area of ​​the membrane under a certain pressure when the membrane is placed in an air permeability tester. The specific evaluation method includes any conventional form in this field, such as GB / T 1038-2000 "Plastic Film and Sheeting Gas Permeability Test Method Pressure Difference Method" and so on. Similarly, the thermal shrinkage rate is also a performance test index of the isolation membrane. Since the isolation membrane is prone to shrinkage and deformation at high temperatures, the thermal shrinkage rate can be used to characterize the dimensional stability of the isolation membrane at high temperatures. The test standard of this indicator includes any conventional form in this field, such as GB / T 13519-2016 "Polyethylene Heat Shrinkage Film for Packaging", ASTM D 2732-08 "Standard Test Method for Unrestrained Linear Thermal Shrinkage of Plastic Film and Sheeting" and so on.

[0080] According to some embodiments of the present application, the coating includes a filler, and the filler includes one or a combination of two or more of an inorganic filler, an organic filler, and an organic-inorganic hybrid filler, and the mass of the filler accounts for 40-50% of the mass of the coating.

[0081] The filler includes but is not limited to conventional materials in the art that are easy to form a coating on the surface of the base film. The filler has the characteristics of good thermal stability and is not easy to decompose, and does not affect ion conductivity. The particle size of the filler includes any conventional particle size in the art. Inorganic fillers include but are not limited to boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, magnesium aluminum silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate, barium titanate, etc. Inorganic fillers also include their own modified products, and the modification method can be chemical modification and / or physical modification. Chemical modification methods include coupling agent modification (for example, using silane coupling agent, titanate coupling agent, etc.), surfactant modification, polymer grafting modification, etc. Physical modification methods can be mechanical dispersion, ultrasonic dispersion, high-energy treatment, etc. The modification treatment can reduce the agglomeration of inorganic particles; in addition, by selecting coupling agents, surfactants or polymers with specific functional groups to modify inorganic particles, it is also helpful to improve the coating's wetting properties for the electrolyte and improve the coating's adhesion.

[0082] The organic fillers include, but are not limited to, at least one of polyethylene particles, polypropylene particles, polystyrene particles, cellulose, cellulose modifiers (e.g., carboxymethyl cellulose), melamine resin particles, phenolic resin particles, polyester particles (e.g., polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate), silicone resin particles, polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles, polyaryletherketone particles, and copolymers of butyl acrylate and ethyl methacrylate (e.g., cross-linked polymers of butyl acrylate and ethyl methacrylate).

[0083] The inorganic hybrid filler includes, but is not limited to, a mixture of at least one of the inorganic fillers and at least one of the organic fillers.

[0084] According to some embodiments of the present application, the coating further includes a binder, and the binder includes one or a combination of two of polyacrylate, acrylic resin, polystyrene butadiene copolymer, and fluorine-containing olefin monomer homopolymer or copolymer.

[0085] The binder is used to bond the coating to the surface of the base film so that it is not easy to fall off. The fluorine-containing olefin monomer homopolymer or copolymer includes polyvinylidene fluoride and the like.

[0086] According to some embodiments of the present application, the mass of the binder accounts for 30% to 60% of the mass of the coating, preferably 40% to 50%. An appropriate amount of binder can bond the sodium supplement to the surface of the base film without affecting the performance of the isolation film.

[0087] According to some embodiments of the present application, the coating further includes a wetting agent, the wetting agent includes one or a combination of two or more of alcohols and nitrogen-containing amines, the alcohol includes one or a combination of two or more of methanol, ethanol, propanol, ethylene glycol, glycerol, and 1,3-propylene glycol, and the nitrogen-containing amine includes one or a combination of two or more of dimethylformamide, methylpyrrolidone, and ethylpyrrolidone.

[0088] According to some embodiments of the present application, the mass of the wetting agent accounts for 2% to 10% of the mass of the coating, preferably 3% to 8%.

[0089] According to some embodiments of the present application, when the coating is mainly composed of a sodium supplement, an inorganic filler, a binder and a wetting agent, the mass ratio of the sodium supplement, the inorganic filler, the binder and the wetting agent is (3-6): (40-50): (40-50): (3-8). At this mass ratio, the coating can be relatively friendly bonded to the surface of the base film, which is conducive to the sodium supplement to play a sodium supplement effect, and can alleviate the impact of temperature changes on the isolation membrane, and can also improve the interface fit between the isolation membrane and the positive and negative electrode sheets.

[0090] According to some embodiments of the present application, the base film material includes but is not limited to any conventional material in the art, such as a polyethylene single-layer film, a polypropylene single-layer film, or a polyethylene, polypropylene composite multi-layer microporous film, etc. And the preparation process of the base film includes but is not limited to any conventional form in the art, such as a dry method or a wet method, etc.

[0091] According to some embodiments of the present application, the base film has a thickness of 10 μm to 30 μm.

[0092] According to some embodiments of the present application, the relationship between the base film and the coating thickness satisfies that the coating thickness does not exceed half of the base film thickness.

[0093] According to some embodiments of the present application, the coating thickness is 0.5 μm to 6 μm.

[0094] Since the isolation film protected by the present application includes a base film + coating structure, wherein the base film performs the conventional function of the isolation film, and the coating is mainly used to improve the function of the isolation film, the coating is formed on the base film in a manner including but not limited to any conventional form in the art, such as a coating process, which includes roller coating, spray coating, etc., and the roller coating includes gravure roller coating, etc. The coating thickness or base film thickness can be measured directly, such as using a conventional measuring instrument such as a micrometer to measure the distance between the upper and lower surfaces.

[0095] The present application limits the coating thickness to any one of 0.5μm, 1.0μm, 1.5μm, 2.0μm, 2.5μm, 3.0μm, 3.5μm, 4.0μm, 4.5μm, 5.0μm, 5.5μm, 6.0μm or any one of the values ​​in the above range, which is beneficial to achieving the effect of not affecting the function of the isolation membrane itself and effectively improving the sodium replenishment effect of the isolation membrane.

[0096] Secondary battery

[0097] The secondary battery comprises a positive electrode sheet, a negative electrode sheet, an electrolyte and the above-mentioned separator. The secondary battery decomposes into sodium ions and byproducts that are easy to remove during the first charge and discharge cycle. Since the byproducts are removed from the sodium battery as much as possible, the byproduct content remaining in the battery is limited and / or basically has no adverse effect on the positive and negative electrode materials or the electrolyte, and the decomposed sodium ions are used to compensate for the active sodium ions lost in the first charge and discharge cycle, thereby achieving the technical purpose of increasing the capacity and cycle life of the battery.

[0098] [Positive electrode]

[0099] According to some embodiments of the present application, the positive electrode sheet constituting the secondary battery includes a positive electrode active material, and the positive electrode active material is at least one of a sodium transition metal oxide, a polyanion compound, and a Prussian blue compound. Among them, in the sodium transition metal oxide, the transition metal can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. The sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1. Polyanionic compounds include one or more of sodium vanadium trifluorophosphate Na3V2(PO4)2F3, sodium vanadium fluorophosphate NaVPO4F, sodium vanadium phosphate Na3V2(PO4)3, Na4Fe3(PO4)2P2O7, NaFePO4, Na3V2(PO4)3. Prussian blue compounds are Na x M1M2(CN)6, wherein M1 and M2 are one or more of Fe, Mn, Co, Ni, Cu, Zn, Cr, Ti, V, Zr, and Ce, and 0<x≤2.

[0100] A binder and / or a conductive agent may also be added to the positive electrode active material, and the types of the binder and the conductive agent are not limited, and those skilled in the art may select them according to actual needs. For example, the binder may be one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid (PAA), polyvinyl alcohol (PVA), and styrene-butadiene rubber (SBR), and the conductive agent may be one or more of graphite, superconducting carbon, acetylene black, carbon black, carbon nanotubes, graphene, and carbon nanofibers.

[0101] [Negative electrode]

[0102] According to some embodiments of the present application, the negative electrode plates constituting the secondary battery are carbon-based negative electrode materials, titanium-based oxide negative electrode materials, metal and alloy negative electrode materials, and non-metallic elements, among which the carbon-based negative electrode materials include hard carbon and soft carbon, the titanium-based oxide negative electrode materials include titanium dioxide and other optimized materials, the metal and alloy negative electrode materials can be tin, antimony, germanium and lead, etc., and the non-metallic elements include carbon elements, etc.

[0103] [Electrolyte]

[0104] According to some embodiments of the present application, the electrolyte constituting the secondary battery includes a sodium salt and an organic solvent. Specifically, there is no particular restriction on the organic solvent in the electrolyte, and the organic solvent may be an organic solvent commonly used in the art for electrolytes. As an example, the organic solvent may be selected from at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, propylene carbonate, methyl acetate, ethyl propionate, fluoroethylene carbonate, ethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and methyl tert-butyl ether, preferably an ether solvent, which is used to adjust the sodium ion deposition morphology, thereby inhibiting the massive growth of sodium dendrites. In the electrochemical device of the present application, there is no particular restriction on the sodium salt in the electrolyte, and the sodium salt may be a sodium salt commonly used in the art for electrolytes. As an example, the sodium salt may include but is not limited to at least one of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate, and sodium chloride.

[0105] [Preparation of Secondary Battery]

[0106] According to some embodiments of the present application, according to some embodiments of the present application, the preparation method of the secondary battery includes overlapping the positive electrode sheet, the negative electrode sheet and the isolation film according to the lamination process or the winding process, and then baking, injecting, standing, forming, secondary injection, aging, shaping, etc. to obtain the secondary battery. Among them, the lamination process, the winding process, baking, injecting, standing, forming, secondary injection, aging, shaping, etc. all include any conventional form in the art, and the injection includes connecting the battery injection hole to the vacuum system by using a multi-station rotary liquid injection machine, a vacuum reverse suction liquid injection machine or manual liquid injection, and vacuuming to form a negative pressure in the battery, and the electrolyte enters the battery under the negative pressure environment, wherein the multi-station rotary liquid injection machine, the vacuum reverse suction liquid injection machine or the vacuum system includes any conventional machine or system in the art, and for a fixed battery system, such as a battery capacity is determined, the injection amount can also be calculated based on the battery capacity.

[0107] The formation includes the first charge and discharge of the battery. The chemical process may include high-temperature formation, low-temperature formation, high-current formation, low-current formation, open-mouth formation, closed-mouth formation, negative pressure formation, etc. Among them, high-temperature formation is to keep the battery in a high-temperature environment all the time, and the formation time is short. However, due to the fast reaction rate, the SEI film formed has high consistency, but is loose and unstable; low-temperature formation is to keep the battery in a low-temperature environment all the time, and the formation time is long. However, due to the slow reaction rate, a dense and stable SEI film is easily formed; high-current formation is to keep the charge and discharge current of the battery at a relatively large current such as 0.5C, 1C, and 2C. The large current can increase the electrochemical reaction rate and the SEI film formation rate, but the formed SEI film has low consistency, is loose and unstable; low-current formation is to charge and discharge the battery The flow is always at a small current such as 0.02C, 0.05C, etc. The SEI film formed in the small current process is dense and stable, but the reduction in reaction rate will prolong the formation time; open formation means that the battery filling port is always open at normal pressure, and the gas generated by the electrochemical reaction can be removed in time, which improves the consistency of SEI film formation, but the formation equipment is simple and low-cost, but the static time is long, and the environmental humidity conditions are high; closed formation means that the battery filling port is always in a sealed state, and there is no environmental humidity condition requirement during the formation process, but the formation equipment process is complex, and the battery shell has the risk of plastic deformation; negative pressure formation includes vacuuming the battery from the filling port, such as to -80KPa. Negative pressure formation can remove the generated gas in time, ensuring the stability and consistency of the SEI film. However, the formation equipment is complex and has high requirements for airtightness. In addition, electrolyte loss will occur during the vacuuming process. The formation process of the present application includes charging to 30% SOC at a small rate of 0.05C at a negative pressure of -80KPa at 45±5°C, and then charging the battery to 70% SOC at a rate of 0.33C. Under the formation process of the present application, the gaseous substances in the decomposition byproducts of the sodium supplement are easier to escape from the sodium battery, and part of the liquid substances, such as alkanes with low boiling points, are also escaped, and the remaining part needs to be escaped with the help of external force. The length, width and thickness of the sodium battery of the present application are any conventional form in the art.

[0108] At the same time, the present application provides a method for replenishing sodium in a secondary battery, which includes heating up after the formation process of the secondary battery is completed to further remove the byproducts of the decomposition of the sodium replenisher from the sodium battery. The heating includes a certain temperature, at which the remaining byproducts that have not been removed in the formation process are also removed from the sodium battery. Since the byproducts are removed from the sodium battery as much as possible, the byproduct content remaining in the battery is limited and / or basically has no adverse effects on the positive and negative electrode materials or electrolytes, and the decomposed sodium ions are used to compensate for the active sodium ions lost in the first charge and discharge cycle, thereby achieving the technical purpose of increasing the capacity and cycle life of the battery.

[0109] According to some embodiments of the present application, heating includes heating at a rate of 0.5°C / min to 2°C / min, and then maintaining the temperature for a period of time after heating to 50°C to 100°C.

[0110] The heating rate, insulation temperature and insulation time of the present application affect not only the rate and degree of by-product release, but also the performance of the electrolyte and the isolation membrane. If the heating rate is lower than 0.5°C / min and the insulation temperature is lower than 50°C, the by-product release rate is slow, and the by-product cannot be removed quickly and as much as possible within the effective time. If the heating rate is higher than 2°C / min and the insulation temperature is higher than 100°C, the electrolyte may be released and the isolation membrane may be adversely affected.

[0111] The temperature increase includes using a charge-discharge box used in the formation process, and setting a temperature increase program for the charge-discharge box to control the temperature increase of the secondary battery. The temperature increase process designed in the present application has little effect on the electrolyte and the positive and negative electrode sheets. The charge-discharge box includes any conventional model of equipment in the art.

[0112] According to some embodiments of the present application, heating includes heating at a rate of 0.8°C / min to 1.8°C / min, and after heating to 55°C to 90°C, keeping the temperature for 1h to 5h.

[0113] Under this temperature rising procedure, the present application can reduce the impact on the electrolyte and the isolation membrane, and at the same time can remove the by-products quickly and as much as possible within the effective time.

[0114] According to some embodiments of the present application, the heating is performed under an environment not higher than standard atmospheric pressure.

[0115] According to some embodiments of the present application, the environment not higher than the standard atmospheric pressure includes a negative pressure of 0.01MPa to 0.1MPa. Heating the temperature in an environment not higher than the standard atmospheric pressure can improve the rate and degree of release. If the pressure is too low, the electrolyte will also be drawn out, which is not conducive to the sodium supplementation process.

[0116] In the secondary battery provided by the present application, during the battery charging and discharging process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The isolation membrane is arranged between the positive electrode sheet and the negative electrode sheet, mainly playing the role of preventing the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0117] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape.

[0118] Battery Module

[0119] The present application provides a battery module, which includes the secondary battery described above. Secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module. The secondary batteries can be arranged along the length direction of the battery module, or in any other arbitrary manner, and the multiple secondary batteries can be fixed by fasteners. At the same time, the battery module can also include a housing with a storage space, and multiple secondary batteries are accommodated in the storage space.

[0120] Battery Pack

[0121] The present application provides a battery pack, which includes the battery modules described above. The number of battery modules contained in the battery pack can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack. The battery pack may include a battery box and a plurality of battery modules arranged in the battery box, and the battery box includes an upper box body and a lower box body, and the upper box body can be covered on the lower box body to form a closed space for accommodating the battery modules, and the plurality of battery modules can be arranged in the battery box in any manner.

[0122] Electrical devices

[0123] The present application provides an electrical device, which includes the isolation membrane of the first aspect, the secondary battery of the second aspect, the secondary battery made by the sodium supplementation method of the third aspect, the battery module of the fourth aspect, or the battery pack of the fifth aspect.

[0124] The electric device can be used as a power source or as an energy storage unit. The electric device has good application prospects in the power field, such as two-wheeled electric vehicles, low-speed electric vehicles, electric ships, buses / coaches, etc., and / or energy storage fields, such as household / industrial energy storage, 5G communication base stations, data centers, renewable energy access, etc., but is not limited to the above fields. As the electric device, a secondary battery, a battery module or a battery pack can be selected according to its use requirements. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the high power and high energy density requirements of the electric device for secondary batteries, a battery pack or a battery module can be used.

[0125] To make the purpose, technical solution and advantages of this application clearer, the sodium battery separator and sodium replenishment method protected by this application are described in detail below in conjunction with specific examples. The chemical substances, reagents, etc. used in the following examples are all conventional models and manufacturers in the field.

[0126] Example 1

[0127] A method for preparing an isolation film is provided, comprising the following steps:

[0128] S1 provides a base film: a polyethylene monolayer film with a thickness of 13 μm;

[0129] S2: preparing a coating slurry: mixing sodium nitride, submicron-grade Al2O3, polyvinylidene fluoride and a wetting agent 1,3-propylene glycol in a mass ratio of 5:45:45:5, adding the mixture into a solvent of deionized water and stirring evenly to obtain a coating slurry having a solid content of about 60%, wherein the solid content is measured by weight;

[0130] S3 coating preparation: The coating slurry of S2 is coated on one side of the base film of S1 by micro-gravure coating, and an isolation film is obtained through drying, slitting and other processes. The coating thickness is 3 μm, wherein the drying temperature is 50°C ± 5°C, and the drying time is 30s.

[0131] Example 2

[0132] Provided is a method for preparing an isolation membrane, wherein the sodium supplement is sodium oxalate, the mass ratio of the components of the coating slurry is: sodium oxalate, submicron Al2O3, polystyrene butadiene copolymer (styrene butadiene rubber), and a wetting agent are mixed in a mass ratio of 4:40:50:6, and the coating thickness is 4 μm.

[0133] Example 3

[0134] Provided is a method for preparing an isolation film, wherein the sodium supplement is sodium formate, the mass ratio of the components of the coating slurry is: sodium formate, submicron Al2O3, polyacrylate, and wetting agent are mixed in a mass ratio of 3.5:50:44.5:2, and the coating thickness is 5 μm.

[0135] Example 4

[0136] A method for preparing an isolation membrane is provided, wherein the sodium supplement is sodium acetate, the mass ratio of the components of the coating slurry is: sodium acetate, submicron Al2O3, polystyrene butadiene copolymer (styrene butadiene rubber), and a wetting agent are mixed in a mass ratio of 6:45:45:4, and the coating thickness is 0.5 μm.

[0137] Example 5

[0138] Provided is a method for preparing an isolation membrane, wherein the sodium supplement is sodium propionate, the mass ratio of the components of the coating slurry is: sodium propionate, submicron Al2O3, polystyrene butadiene copolymer (styrene butadiene rubber), and a wetting agent are mixed in a mass ratio of 3:45:45:7, and the coating thickness is 0.8 μm.

[0139] Example 6

[0140] Provided is a method for preparing an isolation membrane, wherein the sodium supplement is sodium butyrate, the mass ratio of the components of the coating slurry is: sodium butyrate, submicron Al2O3, polystyrene butadiene copolymer (styrene butadiene rubber), and a wetting agent are mixed in a mass ratio of 5.5:45:45:4.5, and the coating thickness is 1 μm.

[0141] Example 7

[0142] Provided is a method for preparing an isolation membrane, wherein the sodium supplement is sodium isobutyrate, the mass ratio of the components of the coating slurry is: sodium isobutyrate, submicron Al2O3, polystyrene butadiene copolymer (styrene butadiene rubber), and a wetting agent are mixed in a mass ratio of 6:42:42:10, and the coating thickness is 6 μm.

[0143] Example 8

[0144] Provided is a method for preparing an isolation membrane, wherein the sodium supplement is sodium formate, the mass ratio of the components of the coating slurry is: sodium formate, submicron Al2O3, and polystyrene butadiene copolymer (styrene butadiene rubber) are mixed in a mass ratio of 1:49:50, and the coating thickness is 5.2 μm.

[0145] Example 9

[0146] Provided is a method for preparing an isolation membrane, wherein the sodium supplement is sodium formate, the mass ratio of the components of the coating slurry is: sodium formate, polyimide particles, and polystyrene butadiene copolymer (styrene butadiene rubber) are mixed in a mass ratio of 3:47:50, and the coating thickness is 5.5 μm.

[0147] Example 10

[0148] Provided is a method for preparing an isolation membrane, wherein the sodium supplement is sodium formate, the mass ratio of the components of the coating slurry is: sodium formate, polyaramid particles, and polystyrene butadiene copolymer (styrene butadiene rubber) are mixed in a mass ratio of 10:45:45, and the coating thickness is 6 μm.

[0149] Embodiment 11

[0150] A method for preparing an isolation film is provided, wherein the method is different from Example 1 in that the base film is a polypropylene single-layer film and the coating thickness is 3 μm.

[0151] Comparative Example 1

[0152] A method for preparing an isolation membrane is provided, which is different from Example 1 in that no sodium supplement is added.

[0153] Comparative Example 2

[0154] A separation film is provided. The separation film is the polyethylene single-layer film in Example 1 and has a thickness of 13 μm.

[0155] The specific parameters of the isolation membranes of Examples 1 to 11 are shown in Table 1.

[0156] Table 1 Parameter list of isolation membranes of Examples 1 to 11

[0157]

[0158]

[0159] Isolation film related performance test:

[0160] 1. Air permeability test: Cut the isolation film sample, the sample size must be greater than 40×40mm. Place the sample on the sample test platform, the sample must cover the entire sample area, tighten the knob, select the measurement area to ensure that the diaphragm can cover the test platform. First press the RESET key (the screen will display "TIMER SEEKING STARTING MARK"), then release the slide to start the test. After the measurement is completed, slowly loosen the plug until the slide drops to the lowest position. Take out the sample, slowly lift the slide, and prepare for the next measurement. The test results are shown in Table 2.

[0161] 2. Heat shrinkage test: Cut the isolation film sample to a size of 15mm×130mm. Place the sample on the sample test platform. The sample must cover the entire sample area. Use the FST-02 film heat shrinkage tester and heat treat it at 130°C for 30 minutes in accordance with ISO 14616-1997 "Heat-shrinkable films of polyethylene, ethylene copolymers and their mixtures - Determination of shrinkage stress". The test results are shown in Table 2.

[0162] Table 2 Performance list of isolation films of Examples 1 to 11 and Comparative Examples 1 to 2

[0163]

[0164]

[0165] As can be seen from Table 1 above, the air permeability of the membrane after adding the sodium supplement to the isolation membrane of the present application is comparable to that of the base membrane of Comparative Example 2, which indicates that the sodium supplement will not have a significant impact on the air permeability of the membrane itself. At the same time, after adding fillers to the isolation membrane of the present application, the thermal shrinkage of the membrane is comparable to that of Comparative Example 1, which indicates that the thermal shrinkage of the membrane is mainly affected by the fillers. At the same time, no wetting agent is added to the isolation membranes of Examples 8, 9, and 10, and the impact on the membrane itself is not significant.

[0166] In addition, after the sodium supplement decomposes, holes will be left in the coating of the isolation membrane, which will help to accommodate part of the electrolyte and buffer the deformation effect of the expansion of the positive and negative electrode sheets on the isolation membrane.

[0167] Secondary batteries were prepared using the separators of Examples 1 to 11 and Comparative Examples 1 to 2 according to the following general preparation method.

[0168] Preparation of secondary batteries:

[0169] (1) Preparation of positive electrode sheet: Na3V2(PO4)2F3 material was used as positive electrode (gram capacity 128.3 mAh / g), polyvinylidene fluoride (PVDF) was used as binder, and conductive carbon black (Super-P) was used as conductive agent. The mixture was uniformly mixed in N-methylpyrrolidone (NMP) solvent at a mass ratio of 90%:5%:5% to prepare positive electrode slurry. The positive electrode active material unit area mass was 360 mg / 1540.25 cm using an extrusion coater. 2 It is required to coat the positive electrode slurry on the surface of the aluminum foil and dry it, and then use a cold press to press the coated electrode at 2.57g / cm 3 The design is compacted and cold pressed.

[0170] (2) Preparation of negative electrode sheets: artificial graphite as an active material, carbon black as a conductive agent, styrene-butadiene rubber as a binder, and sodium hydroxymethyl cellulose as a thickener are dissolved in deionized water as a solvent at a weight ratio of 97.2:0.8:0.8:1.2, and mixed evenly to prepare a negative electrode slurry, wherein the solid content of the negative electrode slurry is 66.5%; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and the negative electrode sheets are obtained after drying, cold pressing, and slitting.

[0171] (3) Preparation of electrolyte: The mass percentage concentration is 12.5%, and NaPF6 is dissolved in a mixed solvent of ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7 to prepare the electrolyte.

[0172] (4) Sodium battery assembly: The positive electrode sheet, negative electrode sheet and isolation film are overlapped together according to the winding process to form a square bare cell. The bare cell is baked at 100°C to remove water, and then the electrolyte is injected and sealed. After that, the secondary battery is obtained through the processes of static standing, hot and cold pressing, formation, secondary liquid injection, aging, shaping, and capacity testing.

[0173] In the process of preparing secondary batteries using the separators of Examples 1 to 11 and Comparative Examples 1 to 2, the temperature is increased after the formation using the process parameters shown in Table 3 to allow the byproducts of the decomposition of the sodium supplement to escape from the battery.

[0174] Comparative Example 3

[0175] A secondary battery is provided, the secondary battery comprising the separator of comparative example 2, wherein a sodium supplement is added to the positive electrode plate, and the mass ratio of the Na3V2(PO4)2F3 material, the polyvinylidene fluoride binder, the conductive carbon black and the sodium formate sodium supplement is 88%:4.8%:4.8%:2.4%. The process parameters of the heating are shown in Table 3.

[0176] Comparative Example 4

[0177] A secondary battery is provided, which includes the isolation membrane of Example 1, and the process parameters of heating are shown in Table 3.

[0178] Comparative Example 5

[0179] A secondary battery is provided, which includes the isolation membrane of Example 1, and the process parameters of heating are shown in Table 3.

[0180] Comparative Example 6

[0181] A secondary battery is provided, which includes the isolation membrane of Example 1, and the process parameters of heating are shown in Table 3.

[0182] Table 3 List of process parameters for heating program of secondary batteries of Examples 1 to 11 and Comparative Examples 1 to 6

[0183]

[0184] Battery performance test:

[0185] (1) Capacity retention after 200 cycles at 25°C: At 25°C, the first charge and discharge were performed. The battery was first charged to 4.3 V at a charging current of 1 / 3C. Then, the battery was charged at a constant voltage of 4.3 V to a current of 0.05C. The test capacity was the first charge capacity. After standing for 5 min, the battery was discharged to 2.8 V at 1 / 3C. The obtained capacity was recorded as the discharge capacity of the first cycle. The charge and discharge cycles were then repeated, and the discharge capacity of the 200th cycle was recorded.

[0186] According to the formula: cycle capacity retention rate = (discharge capacity of the 200th cycle / discharge capacity of the first cycle) × 100%, the capacity retention rate of the battery before and after cycling is calculated, as shown in Table 4;

[0187] (2) First cycle discharge specific capacity and first cycle charge specific capacity at 25°C: according to the method of test (1);

[0188] Table 4 Performance list of secondary batteries of Examples 1 to 11 and Comparative Examples 1 to 6

[0189]

[0190] Combined with Table 4, it can be seen that the first cycle coulomb efficiency (first cycle discharge specific capacity / first cycle charge specific capacity) of Examples 1 to 11 of the present application is first calculated, which are 56.19%, 55.29%, 54.15%, 53.17%, 52.71%, 52.24%, 54.19%, 51.79%, 52.53%, 53.77%, and 55.92%, respectively, which are higher than 49.14% of Comparative Example 1, 49.13% of Comparative Example 2, 48.96% of Comparative Example 3, 51.35% of Comparative Example 4, 50.53% of Comparative Example 5, and 50% of Comparative Example 6. Therefore, compared with the comparative example, the design scheme of the present application improves the problem of capacity loss and cycle performance attenuation. Among them, in comparative example 3, a sodium supplement is added to the positive electrode plate. The design of the present application has significantly improved the problems of capacity loss and cycle performance attenuation. This may be because the sodium supplement is located in the isolation membrane and has little effect on the positive and negative electrode plates. In comparative example 4, the heating procedure is completed under a relatively low vacuum degree. The capacity loss of the battery is improved to a certain extent, but the cycle performance is not ideal. It is speculated that the possible reason is that a certain amount of electrolyte is extracted at a relatively low vacuum degree, and the secondary liquid replenishment effect is not ideal.

[0191] The above-mentioned embodiments and comparative examples only explore the addition of the sodium supplement agent on the surface of one side of the isolation membrane, but the sodium supplement agent can also be added to the surfaces of both sides of the isolation membrane at the same time.

[0192] In summary, the isolation membrane provided in the present application achieves the technical purpose of improving the capacity and cycle life of the battery.

[0193] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A separation film, characterized in that: The isolation film comprises: Basement membrane; A coating layer, located on at least one side surface of the base film; The coating contains a sodium supplement, which decomposes into sodium ions and byproducts that can escape from the isolation membrane during the battery charge and discharge cycle.

2. The isolation film according to claim 1, characterized in that: The sodium supplement is decomposed into sodium ions and byproducts that can escape from the isolation membrane during the first charge and discharge cycle of the battery.

3. The isolation film according to any one of claims 1 to 2, characterized in that: The by-products include gas at normal temperature and pressure and / or liquid with a boiling point of less than or equal to 100°C.

4. The isolation film according to claim 3, characterized in that: The gas comprises one or a combination of two or more of nitrogen, carbon dioxide, gaseous alkanes, hydrogen sulfide, and hydrogen fluoride; The liquid comprises water, liquid alkane, or a combination of two or more thereof.

5. The isolation film according to any one of claims 1 to 2, characterized in that: The sodium supplement comprises one or a combination of two or more inorganic sodium supplements or organic sodium supplements.

6. The isolation film according to claim 5, characterized in that: The inorganic sodium supplement comprises one or a combination of two or more of sodium nitride, sodium azide, sodium sulfide, sodium oxide, sodium peroxide, sodium fluoride or sodium carbonate; The organic sodium supplement comprises Na2C x O y , RCOONa; and x, y include natural numbers from 2 to 8; R includes one or a combination of two or more of H, C1 to C5 alkane groups.

7. The isolation film according to claim 6, characterized in that: The Na2C x O y Here x is 2 and y is 4; In the RCOONa, R includes one or a combination of two or more of H, methyl, ethyl, n-propyl, and isopropyl.

8. The isolation film according to any one of claims 1 to 2, characterized in that: The mass of the sodium supplement accounts for 1% to 10% of the mass of the coating, preferably 3% to 6%.

9. A secondary battery, characterized in that: The secondary battery comprises a positive electrode sheet, a negative electrode sheet, an electrolyte and the separator according to any one of claims 1 to 8.

10. A sodium supplementation method for a secondary battery according to claim 9, characterized in that: The sodium supplementation method includes raising the temperature after the formation process of the secondary battery is completed so that the byproducts of the decomposition of the sodium supplementation agent can be removed from the battery.

11. The method for supplementing sodium according to claim 10, characterized in that: The heating includes heating at a rate of 0.5°C / min to 2°C / min, heating to 50°C to 100°C and then keeping the temperature for a period of time.

12. The method for supplementing sodium according to claim 10 or 11, characterized in that: The heating includes heating at a rate of 0.8°C / min to 1.8°C / min, heating to 55°C to 90°C, and then keeping the temperature for 1h to 5h.

13. The method for supplementing sodium according to claim 10 or 11, characterized in that: The heating is carried out under an environment not higher than the standard atmospheric pressure; Preferably, the environment not higher than the standard atmospheric pressure includes a negative pressure of 0.01 MPa to 0.1 MPa.

14. A battery module, characterized in that: The battery module comprises the secondary battery according to claim 9 or the secondary battery made by the sodium supplementation method according to any one of claims 10 to 13.

15. A battery pack, characterized in that: The battery pack comprises the battery module according to claim 14.

16. An electrical device, characterized in that: The electrical device comprises the isolation membrane described in any one of claims 1 to 8, or the secondary battery described in claim 9, or the secondary battery made by the sodium supplementation method described in any one of claims 10 to 13, or the battery module described in claim 14, or the battery pack described in claim 15.

Citation Information

Cited By

  • Sodium supplementing method of sodium ion battery and sodium ion battery supplemented with sodium

    CN119601786A

  • A sodium supplement method of a sodium ion battery and a sodium ion battery after sodium supplement

    CN119601786B

  • Asymmetric functional sodium battery diaphragm as well as preparation method and application thereof

    CN119833880A

  • An asymmetric functional sodium battery separator, a preparation method and application thereof