Anti-flashover coating on aluminum oxide ceramic surface and preparation method of anti-flashover coating

The chromium trioxide coating is prepared by slurry coating, combined with feldspar powder and zirconium dioxide, and sintered at high temperature in a low oxygen environment, solving the problems of complex preparation process of chromium trioxide coating and poor coating quality. It achieves dense coating and voltage resistance enhancement, suitable for miniaturized vacuum electronic equipment.

CN118955178APending Publication Date: 2024-11-15XIAMEN FINE CERAMICS TECH CO LTD

Patent Information

Application Number
CN202411053678.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing chromium trioxide coating preparation process is complex, the coating quality is poor, and it is difficult to achieve sintering density and high temperature stability, which affects the voltage resistance of alumina ceramics.

Method used

Using slurry coating method, prepare a powder mixture containing chromium trioxide, feldspar powder, zirconium dioxide and silica, combines organic carriers with methyl cellulose and water, and sintered at high temperature after ball milling to form a dense The sintering temperature of the coating is between 1100°C and 1400°C and is carried out in a low oxygen environment.

Benefits of technology

It realizes high-temperature sintering and curing that can be completed by one coating, has good repeatability of coating performance, low cost, environmentally friendly, has an increase in flashover voltage by about 50%, and has strong adhesive force, which is suitable for miniaturized vacuum electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955178A_ABST
    Figure CN118955178A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-flashover coating on an aluminum oxide ceramic surface and a preparation method, the anti-flashover coating is prepared by a slurry coating method, the slurry is composed of mixed powder and an organic carrier, the mixed powder comprises 70%-90% of chromium sesquioxide, 5%-15% of feldspar powder, 0-5% of zirconium dioxide and 5%-15% of silicon dioxide; the organic carrier comprises 96%-99% of water, 0.2%-2.0% of methyl cellulose and 0%-2% of polyethylene glycol; the mixed powder and the organic carrier are uniformly stirred according to a certain weight ratio. The coating can be prepared by dip-coating or brush-coating and can be finished by one-time coating and sintering, the process is simple, the cost is low, the coating is sintered compactly, and the coating performance repeatability is good; meanwhile, water is used as a solvent, and is non-toxic, pollution-free and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of vacuum electronics and relates to an anti-flashover coating on the surface of an alumina ceramic and a preparation method thereof. Background Art

[0002] In the insulation system of vacuum electronics, the vacuum-solid insulation interface is the weakest link in voltage resistance in terms of electrical performance. 95 alumina ceramic is currently the most widely used insulating material. The secondary electron emission coefficient of alumina is large (about 6.0), and its surface flashover voltage is much lower than its solid breakdown voltage. In order to improve the voltage resistance reliability, it is often only possible to increase the volume, such as designing a corrugated surface to extend the surface distance, etc. The resulting increase in volume ultimately leads to a large device, which is not conducive to miniaturization.

[0003] To solve this problem, some scholars have increased the flashover voltage by doping alumina ceramics with oxides such as copper oxide and manganese oxide to reduce the resistance of the ceramic body. However, doping will affect other properties of the alumina ceramic itself. Since surface flashover only occurs on the surface, the best way is to apply a coating on the surface of the ceramic substrate to avoid affecting the overall alumina ceramic. The secondary electron emission coefficient of chromium trioxide is small (about 2.0), and adding a chromium trioxide coating on the ceramic surface is an effective way to increase the surface flashover voltage.

[0004] At present, the main methods of chromium trioxide coating are thermal spraying, plasma spraying, PVD deposition of metal chromium reoxidation, sol-gel coating and slurry coating. Among them, both spraying and PVD methods are difficult to prepare coatings with complex structures (especially inner holes), and the comprehensive cost is relatively high; the sol-gel method can adapt to complex structures, but the coating is thin and uneven after one coating, and the process is difficult to control, and multiple coatings are required to achieve the required thickness; slurry coating is an ideal preparation method for this occasion. Slurry coating has two methods: low-temperature curing with resin as an adhesive and high-temperature sintering directly combined with ceramic materials. The low-temperature cured adhesive resin cannot withstand the high temperature of 500°C, and it is difficult to withstand the arc burning caused by high voltage for a long time, and the application scenarios are limited; high-temperature sintering and curing slurry is the most ideal coating preparation method, in which the composition configuration and preparation process of the slurry are very critical; if chromium trioxide is used alone, its melting point is high and it is difficult to sinter densely, the coating is not firm, and the ideal effect cannot be obtained. If the composition and process are not suitable, it is difficult to apply, and the final coating thickness is uneven.

[0005] Publication No. CN113929501B discloses a flashover-resistant gradient composite coating on the surface of alumina ceramics, which controls the relative dielectric constant / surface resistivity of the coating by changing the content of chromium oxide in the coating. This method requires the preparation of slurries of different concentrations and repeated coating.

[0006] Therefore, the present invention is dedicated to solving the problems of complex preparation process and poor coating quality of chromium oxide coating. Summary of the invention

[0007] In view of the existing problems, the present invention provides an anti-flashover coating on the surface of alumina ceramics and a preparation method thereof. The coating is sintered densely and has good performance repeatability; the preparation process is simple and environmentally friendly.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] An anti-flashover coating on the surface of alumina ceramics comprises the following raw materials, by weight: 70% to 90% chromium oxide, 5% to 15% feldspar powder, 0% to 5% zirconium dioxide, and 5% to 15% silicon dioxide. Preferably, the powder particle size of the raw materials is 5 microns to 20 microns. The feldspar powder is preferably lithium feldspar powder.

[0010] Preferably, the thickness of the anti-flashover coating is 0.01 mm to 0.02 mm.

[0011] The present invention also provides a method for preparing the above-mentioned anti-flashover coating, which adopts a slurry coating method, (1) slurry preparation, the slurry consists of a mixed powder and an organic carrier, the mixed powder contains: 70% to 90% chromium trioxide, 5% to 15% feldspar powder, 0% to 5% zirconium dioxide, 5% to 15% silicon dioxide; the organic carrier contains 96% to 99% water, 0.2% to 2.0% methyl cellulose, and 0% to 2% polyethylene glycol; when the mixed powder and the organic carrier are mixed, the weight of the mixed powder accounts for 40% to 80%; (2) the prepared slurry is coated on the surface of the alumina ceramic, dried, sintered at high temperature, and cooled to obtain the obtained slurry. The polyethylene glycol is preferably PEG-1000.

[0012] Preferably, the methylcellulose is water-soluble methylcellulose, including but not limited to one or more of sodium methylcellulose, hydroxypropyl methylcellulose, and sodium carboxymethylcellulose.

[0013] Furthermore, step (1) also includes a ball milling step: first adding half of the amount of the organic carrier to the mixed powder, ball milling for 8h to 24h, and then adding the remaining half of the organic carrier after the ball milling is completed, stirring and mixing, and obtaining a paint-like slurry after mixing.

[0014] Furthermore, in step (2), the high temperature sintering temperature is between 1100°C and 1400°C.

[0015] Furthermore, the high temperature sintering in step (2) is carried out in a low oxygen environment, such as vacuum sintering, or sintering under a protective atmosphere of one or more of hydrogen, argon and nitrogen.

[0016] In one possible implementation scheme, the high temperature sintering in step (2) is performed in air by using a carbon buried sintering method.

[0017] Beneficial effects: The present invention provides a chromium oxide coating that is solidified by high-temperature sintering, which can be prepared by dipping and brushing, and can be completed by one-time coating and sintering. The process is simple and the cost is low. The coating is sintered densely and the coating performance has good repeatability. At the same time, water is used as a solvent, which is non-toxic, pollution-free and environmentally friendly.

[0018] Vacuum ceramics often require fine processing and brazing of alumina after firing to match the size. The present invention can apply the coating later and does not need to be co-fired with the alumina blank, so the application is more flexible.

[0019] The coating of the present invention has strong bonding force with alumina ceramics and can be applied by dipping. Due to the film-forming components in the slurry (methylcellulose plays a leading role), the slurry can be closely attached to the alumina ceramic substrate after drying and forming a film.

[0020] The key to strong adhesion after sintering the coating is that the silica component of the coating is the same as the glass phase component in the alumina matrix, and they fuse together during the sintering process; on the other hand, the feldspar powder and silica melt to form a liquid phase, and the liquid phase dissolves to form a glass phase, which fills the gaps in the unmelted chromium trioxide, thereby fixing the chromium trioxide and playing a bonding role. Zirconium dioxide is a synergistic component that is conducive to liquid phase diffusion and accelerates the densification of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the process flow of the present invention;

[0022] Figure 2 This is a macroscopic photograph of the anti-flashover coating on the surface of the alumina ceramic obtained in Example 1 after the performance test. The green anti-flashover coating prepared on the outer surface and the inner hole surface of the alumina ceramic has strong bonding strength and does not fall off.

[0023] Figure 3 This is an enlarged view of coating A in Example 1, with a magnification of 4 times. DETAILED DESCRIPTION

[0024] In order to better understand the technical solution of the present invention, the embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. It should be clear that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Unless otherwise specified, the test materials and equipment used in the examples are common commercial products and can be purchased in the market.

[0026] like Figure 1 The process flow shown in the figure, the anti-flashover coating on the surface of alumina ceramic includes the following steps:

[0027] (1) Slurry preparation.

[0028] The slurry consists of two parts: a mixed powder and an organic carrier: the mixed powder contains: 70% to 90% chromium oxide, 5% to 15% feldspar powder, 0 to 5% zirconium dioxide, and 5% to 15% silicon dioxide, and the proportion is by weight. Among them, chromium oxide is the main and functional component, which plays a role in reducing the secondary electron emission rate and improving the flashover voltage resistance; feldspar powder, zirconium dioxide, and silicon dioxide are sintering aids. Since pure chromium oxide has a high melting point and is difficult to sinter, the addition of sintering aids can reduce the overall melting point and make the coating dense. The sintering aid will melt to form a liquid phase during the sintering process, filling the gaps in the unmelted chromium oxide, thereby fixing the chromium oxide, and at the same time the liquid phase and the alumina substrate form a bond. The powder particle size is micron-level, preferably 5 to 20 microns. Feldspar powder is preferably lithium feldspar.

[0029] More specifically, the synergistic effect between the mixed powders is as follows: lithium feldspar and silicon dioxide are key components (lithium feldspar is more key), which lower the melting point. The liquid phases of the two melts dissolve into a glass phase, which plays a bonding role. Silicon dioxide also helps the glass of the coating and the base ceramic to combine and increase the bonding strength; while zirconium dioxide is a synergistic component, which is conducive to liquid phase diffusion and accelerates the densification of the coating. Titanium dioxide is also used as a sintering aid in the prior art, but the sintering temperature of titanium dioxide is relatively high, which needs to reach 1600°C. At the sintering temperature of this patent, the bonding strength is insufficient if titanium dioxide is used.

[0030] At the same time, the organic carrier contains: 96% to 99% water, 0.2% to 2.0% methyl cellulose, and 0% to 2% polyethylene glycol; the ratio is weight ratio. The organic carrier is used to carry and disperse the powder during coating to obtain a slurry for easy operation, wherein water is the main solvent component; methyl cellulose increases the overall viscosity of the carrier, making it difficult for the powder to settle; polyethylene glycol is a dispersant, which controls the dispersion of the powder without agglomeration and prolongs the operability time of the slurry.

[0031] Among them, the methylcellulose can be water-soluble, such as sodium methylcellulose, hydroxypropyl methylcellulose, sodium carboxymethylcellulose, etc., which does not chemically react with the powder.

[0032] When the mixed powder and the organic carrier are mixed, the weight of the mixed powder accounts for 40% to 80%. When the mixed powder accounts for 60%, brush coating can meet most needs. When the structure is complex and dip coating is required, the powder ratio is reduced and the slurry fluidity is increased. When a thick coating is required, the mixed powder ratio can be increased. The proportion of the mixed powder is directly related to the product to be coated and is adjusted according to the actual product.

[0033] It should be noted that in the slurry prepared by the present invention, if the ratio of feldspar powder to silicon dioxide is too high, the coating performance will be reduced because the amount of the effective ingredient chromium trioxide is reduced; if the ratio of feldspar powder to silicon dioxide is too low, the coating bonding strength is poor, and the liquid phase after sintering is too small to completely enclose the chromium trioxide, and granular peeling is prone to occur. The inventors found in the research and development process that feldspar powder, zirconium dioxide, and silicon dioxide are sintering aids. When the content of this sintering aid is less than 7% of the weight of the mixed powder, the bonding strength between the coating and the substrate begins to deteriorate. (2) The slurry is coated and dried, and sintered at high temperature to form a coating.

[0034] The slurry is coated on the surface of 95 alumina ceramics, dried under natural conditions, and then sintered at high temperature. The sintering atmosphere needs to be a low-oxygen environment, such as protective gases such as hydrogen, argon, and nitrogen, or vacuum sintering. Carbon sintering should be used in the air, otherwise it will not be successful and the thin coating will evaporate directly.

[0035] The preferred sintering temperature is 1100°C to 1400°C. When sintering is performed at a temperature lower than 1000°C, the sintering is incomplete and the bonding strength is poor; when sintering is performed at a temperature higher than 1400°C, the coating is firmly sintered, but as the temperature rises, chromium oxide and aluminum oxide are mutually dissolved and strengthened, and the coating appearance gradually changes from green to dark green and then to pink.

[0036] It is preferred to sinter in wet hydrogen or vacuum atmosphere. The oxygen partial pressure of sintering in air atmosphere is too high, and chromium trioxide is easy to volatilize. The sintering atmosphere needs to be a low-oxygen environment, such as hydrogen, argon and other protective gases or vacuum sintering. Carbon buried sintering should be used in air, otherwise it will not be successful and the thin coating will evaporate directly.

[0037] It should be noted that: 1. Chromium oxide itself is volatile during sintering (all +2-valent / +4-valent oxides except chromium trioxide are volatile. Chromium trioxide is easy to react with oxygen at high temperature during sintering to become other volatile oxides), and it is not easy to sinter densely. It is necessary to find a suitable sintering aid, and the coating must be fired at a temperature lower than 95 alumina ceramic firing temperature (1600℃), otherwise the alumina ceramic will be deformed, resulting in changes in the size of the substrate and the product will be scrapped; and when the sintering temperature exceeds 1400℃, chromium oxide will begin to dissolve into the alumina lattice in large quantities, causing the porcelain body to turn pink. 2. The organic carrier is the key to the final coating operability of the slurry and the uniformity of the final coating. Find a suitable carrier solvent to evenly disperse chromium trioxide and other powders, and create conditions for the coating process. It is necessary to meet the requirements of proper fluidity, uniform film formation after coating, and decomposition during firing that does not affect the final coating.

[0038] Example 1

[0039] (1) Slurry preparation

[0040] Prepare an organic carrier by weighing 0.2% methylcellulose, 2% polyethylene glycol and 97.8% water according to the weight ratio, stirring and mixing thoroughly for use. The polyethylene glycol is PEG-1000, and the methylcellulose is hydroxypropyl methylcellulose with a viscosity of 200,000. The polyethylene glycol can be of other molecular weights. The methylcellulose can also be a product with a viscosity that meets the water solubility and does not chemically react with the powder.

[0041] The following powders are weighed and mixed according to the weight ratio: 70% chromium oxide, 15% feldspar powder, 5% zirconium dioxide, and 10% silicon dioxide to obtain a mixed powder. The powder particle size is micron-grade, preferably 5 to 20 microns. For example, 20 microns, 10 microns, or 5 microns are all acceptable.

[0042] Mix according to the ratio of mixed powder: organic carrier = 60:40 (weight ratio). First add half of the amount of organic carrier to the above mixed powder, and ball mill for 24 hours. After the ball milling is completed, add the remaining half of the organic carrier and stir and mix. After mixing, a slurry similar to paint is obtained. It is better to prepare it before use. It needs to be sealed and stored after use, and fully stirred again before the next use. The lithium feldspar component in the sintering aid lowers the melting point of the entire sintering aid to form a liquid phase. Ball milling is mainly for the uniformity of the powder particle level. The ball milling time can be adjusted according to the actual situation. It can be within 8 hours to 24 hours. In this embodiment, 24 hours is taken to more fully and evenly disperse the mixed powder.

[0043] (2) Drying slurry and high temperature sintering

[0044] Apply the slurry (by brushing or spraying) on ​​the surface of 95 alumina ceramics, dry it naturally, and then dry it at 100℃ for 30 minutes. If it is the inner surface of a tubular alumina ceramic or an alumina ceramic with a complex structure such as an inner hole, the alumina ceramic can also be immersed in the slurry, taken out, dried naturally, and then dried. There are no special requirements for the coating process, and it can be operated at room temperature and pressure.

[0045] After drying, sintering was carried out in a vacuum environment at 1250°C for 1 hour with a vacuum degree of 10 -3 Pa~10 -6 Pa. Cool naturally with the furnace. The thickness of the obtained coating is 0.01 mm to 0.02 mm. The high-temperature sintering process of the present invention has no special requirements for the heating rate. Because the organic content is very small, the water as a solvent has basically volatilized during drying, so there is no need for a dwelling temperature for organic decomposition like an organic solvent slurry. If the organic content is high, it needs to stay at the decomposition temperature and decompose thoroughly before further sintering to prevent the decomposition during sintering to produce gaseous substances that cause the coating to become loose. The coating of this patent has very little organic matter and does not have this problem.

[0046] (3) Performance testing

[0047] Surface resistance test: Use a surface resistance tester to test 3 times and take the middle value as the test result.

[0048] Thermal shock test: Place the product in a 200℃ resistance furnace for 30 minutes, take it out and quickly throw it into room temperature water for rapid cooling for 2 minutes. The above is one cycle. Perform a total of 25 thermal shock cycles and visually inspect the coating.

[0049] Flashover voltage test: in vacuum degree 10 -4 Under the condition of Pa, a DC voltage is applied to both ends of the product through the copper plate, with an initial voltage of 8kVDC, maintained for 1min, and a leakage current greater than 1mA is considered to be a breakdown. If there is no breakdown, the voltage is increased by 1kVDC intervals until the test product flashes over and breaks down, and the final voltage without breakdown is the withstand voltage test result (for example: if a breakdown occurs at 10kVDC, the withstand voltage test result is 9kVDC).

[0050] The test results are shown in Table 2. After the coating is applied, the flashover withstand voltage is increased by about 50%.

[0051] In Example 2-5, the steps of Example 1 are followed, and the composition, content and preparation conditions of the slurry are shown in Table 1. The mixed powder and the organic carrier are mixed in a weight ratio of 60:40.

[0052] Example 6, the steps are the same as Example 1-5, and the difference from Example 5 is that the organic carrier does not contain polyethylene glycol. When polyethylene glycol is not added, the main effect is to reduce the storage time of the slurry, because the powder is easy to precipitate and agglomerate, and there is no effect on coating within a short time after the slurry is prepared. Specific data are shown in Table 2.

[0053] Table 1 Examples 1-6

[0054]

[0055] The coating products prepared in Examples 1-6 were subjected to surface resistance test, thermal shock test and flashover voltage resistance test, respectively. The coating performance results are shown in Table 2. In the thermal shock test, the coatings did not peel off or crack. The flashover voltage resistance was 14kVDC to 16kVDC, which was about 50% higher than that without coating. Figure 2 This is a macroscopic photograph of the anti-flashover coating on the surface of the alumina ceramic obtained in Example 1 after the performance test. Figure 3 This is a partial enlarged view of the coating of Example 1, with a magnification of 4 times. After the thermal shock test, the green anti-flashover coating on the outer surface of the alumina ceramic and the inner hole surface of the coating prepared by the present invention has no peeling, cracking, or falling off, and the coating has a strong bonding force with the substrate.

[0056] Table 2 Coating performance test results

[0057]

[0058] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention still fall within the protection scope of the present invention.

Claims

1. An anti-flashover coating on the surface of alumina ceramics, characterized in that: The invention comprises the following raw materials, calculated by weight: 70% to 90% of chromium trioxide, 5% to 15% of feldspar powder, 0% to 5% of zirconium dioxide, and 5% to 15% of silicon dioxide.

2. The anti-flashover coating on the surface of alumina ceramic according to claim 1, characterized in that: The feldspar powder is lithium feldspar powder.

3. The anti-flashover coating on the surface of alumina ceramic according to claim 1, characterized in that: The coating thickness is 0.01 mm to 0.02 mm.

4. The method for preparing an anti-flashover coating on the surface of an alumina ceramic according to any one of claims 1 to 3, characterized in that: The slurry coating method includes the following steps: (1) Slurry preparation, the slurry consists of two parts: mixed powder and organic carrier, the mixed powder contains: 70% to 90% chromium oxide, 5% to 15% feldspar powder, 0% to 5% zirconium dioxide, 5% to 15% silicon dioxide; the organic carrier contains 96% to 99% water, 0.2% to 2.0% methyl cellulose, and 0% to 2% polyethylene glycol; when the mixed powder and the organic carrier are mixed, the weight of the mixed powder accounts for 40% to 80%; (2) the prepared slurry is coated on the surface of the alumina ceramic, dried, sintered at high temperature, and cooled to obtain the product.

5. The method for preparing an anti-flashover coating on the surface of an alumina ceramic according to claim 4, characterized in that: The methylcellulose is water-soluble methylcellulose, including but not limited to one or more of sodium methylcellulose, hydroxypropyl methylcellulose, and sodium carboxymethylcellulose.

6. The method for preparing an anti-flashover coating on the surface of an alumina ceramic according to claim 4, characterized in that: Step (1) also includes a ball milling step, wherein half of the organic carrier is added to the mixed powder and ball milled for 8 to 24 hours. After the ball milling is completed, the remaining half of the organic carrier is added and stirred to obtain a paint-like slurry.

7. The method for preparing an anti-flashover coating on the surface of an alumina ceramic according to claim 4, characterized in that: The high-temperature sintering temperature in step (2) is 1100°C to 1400°C.

8. The method for preparing an anti-flashover coating on the surface of an alumina ceramic according to claim 4, characterized in that: The high-temperature sintering in step (2) is carried out in a low-oxygen environment, including but not limited to vacuum sintering or sintering under a protective atmosphere of one or more of hydrogen, argon, and nitrogen.

9. The method for preparing an anti-flashover coating on the surface of an alumina ceramic according to claim 4, characterized in that: The high-temperature sintering in step (2) is carried out in air using a carbon-buried sintering method.

Citation Information

Patent Citations

  • A flashover-resistant gradient composite coating for alumina ceramic surface and its preparation method

    CN113929501B

  • Oxide ceramic material with high thermal conductivity and preparation method thereof

    CN104276815A

  • Ceramic X-ray pipe inner surface coating composition and sintering method thereof

    CN108395280A

  • Flashover-resistant gradient composite coating layer on aluminum oxide ceramic surface and preparation method of flashover-resistant gradient composite coating layer

    CN113929501A

  • Ceramic coating

    US4988538A

Cited By

  • Alumina ceramic for an electric vacuum device and method for manufacturing the same

    CN122853938A