Preparation method of multifunctional fiber
By evenly dispersing ginseng extract and far infrared negative ion powder into the fiber, the problems of ginseng fabric not lasting and uneven powder dispersion in the prior art are solved, and antioxidant, moisturizing and far infrared of multifunctional fibers are realized , the effects of negative ions and antibacterial and mite prevention are improved.
Patent Information
- Application Number
- CN202411197761.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ginseng-containing fabrics do not last long during use, and fall off with the increase in the number of washes, which deteriorates. The ginseng powder cannot be evenly dispersed when preparing multifunctional fibers, resulting in poor results.
First, the ginseng extract is micronized, then mixed with far-infrared negative ion powder, added dispersion solvent and stirred and dried, and then grinded to form a multifunctional ginseng powder, and then mixed with cellulose spinning liquid in one go to prepare a composite dispersion and then mix it with the remaining cellulose spinning liquid to form a uniform composite spinning glue to ensure that ginseng and far-infrared negative ion powder are evenly dispersed inside the fiber.
The fiber's antioxidant, moisturizing, far infrared, negative ion, antibacterial and anti-mites are combined, which improves the problem of short-lasting functions and single functions, and improves the performance stability and use effect of fibers.
Smart Images

Figure CN118957788A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of fiber manufacturing, and in particular, relates to a method for preparing a multifunctional fiber. Background Art
[0002] Currently, most of the ginseng-containing fabrics on the market have undergone post-finishing treatment, in which slurry or additives containing ginsenosides are impregnated or coated on the surface of the fabric. They have relatively simple functions, simple process operations, a hard feel, and poor comfort. Moreover, with the increase of usage time and the number of washings, there are defects of falling off and reduced functionality.
[0003] In the prior art, in the preparation of multifunctional fibers, ginseng powder and far-infrared negative ion powder are directly and simply stirred and mixed with cellulose spinning solution. The powder cannot be evenly dispersed in the cellulose spinning solution, and aggregation is serious, resulting in poor effect. Summary of the invention
[0004] The present application provides a method for preparing multifunctional fibers, which solves the problem that the functional materials of ginseng fibers fall off and the functions are reduced as the number of times they are washed increases, and the ginseng components cannot exert their effects.
[0005] The present invention provides a method for preparing a multifunctional fiber, which specifically comprises the following steps:
[0006] Step 1, micronizing the ginseng extract to obtain a micronized ginseng extract;
[0007] Step 2, filtering and grinding to prepare far-infrared negative ion powder;
[0008] Step 3, adding the micronized ginseng extract and the far-infrared negative ion powder into a dispersing solvent, stirring, drying, and grinding to obtain ginseng multifunctional powder;
[0009] Step 4: mixing the ginseng multifunctional powder with part of the cellulose spinning solution once to obtain a composite dispersion, and then mixing the composite dispersion with the remaining part of the cellulose spinning solution for a second time, and allowing to stand to obtain a composite spinning glue;
[0010] Step 5: Spinning to obtain multifunctional fibers.
[0011] In one embodiment,
[0012] Step 1: The ginseng extract is one of ginseng root extract, ginseng stem and leaf extract or ginseng adventitious root; the particle size of the micronized ginseng extract is 3 μm, the total ginsenoside content is 80.2%, and the drying loss is 1.6%.
[0013] In one embodiment,
[0014] In step 2, the far-infrared negative ion powder is one of microporous composite powder, silicate powder or seaweed; the microporous composite powder includes inorganic powder and plant residues, the inorganic powder is one or more of zinc oxide, aluminum oxide, zirconium oxide, tourmaline, germanium stone, diatomaceous earth or zeolite, and the plant residues are one or more of ginseng stems and leaves, bamboo chips, tea residues, and coffee residues; the silicate powder is one or more of feldspar, quartz, mica or talc, and the seaweed is one or more of sodium alginate or seaweed charcoal; preferably, the far-infrared negative ion powder is sodium alginate.
[0015] In one embodiment,
[0016] The mixing ratio of the inorganic powder to the plant residue is 1:5.
[0017] In one embodiment,
[0018] The microporous composite powder and seaweed charcoal need to be carbonized, and the carbonization temperature is 1000-1200° C. The particle size of the far-infrared negative ion powder is 300-500 nm, and the porosity is 40-50%.
[0019] In one embodiment,
[0020] Step 3: The preparation step of the dispersion solvent is as follows: add the hydrophilic solvent into deionized water and stir in a high-speed stirrer for 1 hour.
[0021] In one embodiment,
[0022] The hydrophilic solvent is one of polyvinyl pyrrolidone, N,N-di(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenediamide or a hydrophilic acrylic hyperbranched block copolymer. Preferably, the hydrophilic solvent is a hydrophilic acrylic hyperbranched block copolymer; the mass of the acrylic hyperbranched block copolymer is 25% of the deionized water.
[0023] In one embodiment,
[0024] The stirring time in step three is 4 hours; the particle size of the ginseng multifunctional powder is 3 μm; the mixing ratio of the micronized ginseng extract, the microporous composite powder and the dispersing solvent is 0.5%:19.5%:80%-22%:8%:70%, preferably, the mixing ratio is 10%:10%:80%.
[0025] In one embodiment,
[0026] In step 4, the cellulose spinning solution is one or more of viscose, modal, lyocell, and bamboo pulp fiber. The mass fraction ratio of ginseng multifunctional powder to cellulose spinning solution in the one mixing is 10%:90%-40%:60%, preferably, the mass fraction ratio is 30%:70%.
[0027] In one embodiment,
[0028] The specific steps of the secondary mixing described in step 4 are: secondary mixing the composite dispersion liquid and the remaining part of the cellulose spinning solution in a ratio of 1:3-50 through a diaphragm pump and a plunger pump, stirring with a high-speed stirrer for 0.5h, and standing for 2h to achieve a uniformly mixed and stable dispersion state; preferably, the ratio of the composite dispersion liquid to the remaining part of the cellulose spinning solution is 1:10.
[0029] The present application provides a method for preparing multifunctional fibers, which combines the antioxidant properties of ginsenosides with the far-infrared, negative ion, and antibacterial and anti-mite functions of far-infrared negative ion functional powders. A compounding process of first small mixing and then blending is adopted to first prepare a composite dispersion with extremely high dispersibility and stability, and then the composite dispersion is blended with a cellulose spinning solution to form a uniform and stable composite spinning glue, thereby ensuring that the ginseng powder and the far-infrared negative ion powder are uniformly dispersed inside the fibers, so that the prepared fibers have the functions of antioxidant, moisturizing, far-infrared, negative ion, and antibacterial and anti-mite, thereby improving the problems of the existing technology of short-lasting functions and single functions. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0031] Figure 1 This is a line graph showing changes in the amount of moisture in the skin keratin of Example 1;
[0032] Figure 2 This is a line graph showing changes in the amount of moisture in the skin keratin of Example 2;
[0033] Figure 3 This is a line graph showing the change in moisture content of skin keratin in Example 3. DETAILED DESCRIPTION
[0034] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clear, the present application is further described in detail. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0035] Example 1
[0036] A method for preparing a multifunctional fiber comprises the following steps:
[0037] Step 1, micronizing the 120-mesh ginseng root extract to obtain a particle size of 3 μm to obtain a micronized ginseng extract, wherein the total ginsenoside content of the micronized ginseng extract is 80.2% and the drying loss is 1.6%;
[0038] Step 2: Mix zinc oxide-germanium-diatomaceous earth with a particle size of less than 3 μm and ginseng stems and leaves-bamboo chips in a ratio of 1:5 and put them into a high-temperature furnace, carbonize them at a high temperature of 1000-1200°C, evaporate the ginseng stems and leaves and bamboo chips around the oxide, and form a microporous composite powder coated with carbon particles with a particle size of 300-500 nm after filtering and grinding, and the porosity is 40-50%; the ratio of zinc oxide:germanium:diatomaceous earth is 1:1:1, and the ratio of ginseng stems and leaves:bamboo chips is 1:1;
[0039] Step 3: Add the hydrophilic acrylic acid hyperbranched block copolymer to deionized water and stir in a high-speed stirrer for 1 hour to obtain a dispersion solvent, then add the micronized ginseng extract and the microporous composite powder to the dispersion solvent, continue stirring and mixing for 4 hours, the mixing ratio of the micronized ginseng extract, the microporous composite powder and the dispersion solvent is 10%:10%:80%, and then vacuum dry and grind into ginseng multifunctional powder with a particle size of 3 μm; the mass of the hydrophilic acrylic acid hyperbranched block copolymer is 25% of the deionized water;
[0040] Step 4: Add the ginseng multifunctional powder and a portion of viscose in a ratio of 30%:70% by mass into a stirring kettle and stir for 2 hours to obtain a composite dispersion, then mix the composite dispersion with the remaining viscose in a ratio of 1:10 through a diaphragm pump and a plunger pump, stir for 0.5 hours with a high-speed stirrer, and let stand for 2 hours to allow the composite dispersion and viscose to be evenly mixed and stably dispersed to obtain a composite spinning glue;
[0041] Step 5, spinning to obtain multifunctional fiber ginseng fiber 1#; the specific steps of spinning include: pulp impregnation, pressing, crushing, aging, yellowing, dissolving, maturation, filtering, coagulation bath, and degassing; wherein, the composite spinning adhesive obtained in step 4 is introduced after the maturation step, the composite spinning adhesive is pumped into the filter, filtered through a poplin filter cloth, pumped into the spinneret by a metering pump, discharged from the metering pump, enters the curved tube, and finally sprayed out from the spinneret hole, solidified in the coagulation bath to become primary filaments, the filaments pass through an acid scraping rod, a spinning disk, a coagulation roller, and a deacidifying roller, and finally enter a centrifugal tank to be wound into a silk cake, the silk cake is refined and degassed (through alkali washing, acid washing, water washing, oiling and other processes), and then dried and humidified, and then beaten into a bobbin, and finally graded and packaged.
[0042] The cellulose dissolving system adopted in this embodiment is an alkalization and sulfonation dissolving system widely used in current industrial production. The cellulose used for spinning ginseng regenerated cellulose fiber is prepared from cotton pulp and wood pulp raw materials. The semi-continuous spinning conventional process conditions are the basic conditions for spinning ginseng regenerated cellulose fiber. The spinning step in step five is a spinning method in the prior art, so it will not be repeated here.
[0043] The basic process conditions are shown in Tables 1-1, 1-2, 1-3 and 1-4.
[0044] Table 1-1 Cellulose spinning solution indicators
[0045] Element index Fiber content 7.70-8.30% NaOH 5.60-5.80% Viscosity 26-45s (20℃, ball drop) Maturity <![CDATA[7.8-9.0mL(10%NH4CL)]]>
[0046]
[0047] Element Indicator parameters <![CDATA[H2SO4]]> 128.0-136.0g / L <![CDATA[Na2SO4]]> 260.0-270.0g / L <![CDATA[ZnSO4]]> 10.0-12.0g / L Bath temperature 48.0-53.0℃
[0048] Table 1-3 Spinning conditions
[0049] Spinning conditions Indicator parameters Product Specifications 1.2D Spinning speed 82m / min Bath length 355mm Silk bath length 450mm Drafting rate of drafting disc 25% Tension stretch 4.12% Solidification roller wire turns 26-30 laps Number of deacidification roller wire turns Lap 80-85
[0050] Table 1-4 Silk cake elution treatment conditions
[0051] Element concentration temperature time Desulfurization: NaOH 5.4-5.8g / L 73-77℃ 120min Pickling: HCL 4.8-5.2g / L normal temperature 40min oil 1.4-1.8g / L 38-42℃ 40min
[0052] Example 2
[0053] The difference between this embodiment and embodiment 1 is that the microporous composite powder in step 2 is replaced with feldspar, and carbonization is not required. The other steps are the same to obtain ginseng fiber 2#.
[0054] Example 3
[0055] The difference between this embodiment and embodiment 1 is that the microporous composite powder in step 2 is replaced with sodium alginate, and carbonization is not required. The other steps are the same to obtain ginseng fiber 3#.
[0056] Example 4
[0057] The difference between this embodiment and embodiment 1 is that the hydrophilic acrylic hyperbranched block copolymer in step 3 is replaced by polyvinyl pyrrolidone, and the other steps are the same.
[0058] Example 5
[0059] The difference between this embodiment and embodiment 1 is that the hydrophilic acrylic hyperbranched block copolymer in step 3 is replaced by N,N-di(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenediamide, and the other steps are the same.
[0060] Example 6
[0061] The difference between this embodiment and embodiment 1 is that the ratio of zinc oxide-germanium stone-diatomaceous earth to ginseng stems and leaves-bamboo chips in step 2 is changed to 1:1, and the other steps are the same.
[0062] Example 7
[0063] The difference between this embodiment and embodiment 1 is that the ratio of zinc oxide-germanium stone-diatomaceous earth to ginseng stems and leaves-bamboo chips in step 2 is changed to 1:10, and the other steps are the same.
[0064] Example 8
[0065] The difference between this embodiment and embodiment 1 is that the zinc oxide-germanium stone-diatomaceous earth in step 2 is replaced by aluminum oxide-zirconium oxide-tourmaline, and the other steps are the same.
[0066] Example 9
[0067] The difference between this embodiment and embodiment 1 is that the zinc oxide-germanium stone-diatomaceous earth in step 2 is replaced by aluminum oxide-zirconium oxide-zeolite, and the other steps are the same.
[0068] Example 10
[0069] The difference between this embodiment and embodiment 1 is that the zinc oxide-germanium stone-diatomaceous earth in step 2 is replaced by zinc oxide, and the other steps are the same.
[0070] Embodiment 11
[0071] The difference between this embodiment and embodiment 1 is that the ginseng stems and leaves-bamboo chips in step 2 are replaced with tea dregs-coffee dregs, and the other steps are the same.
[0072] Example 12
[0073] The difference between this embodiment and embodiment 1 is that the ginseng stems and leaves-bamboo chips in step 2 are replaced with tea ginseng stems and leaves-coffee grounds, and the other steps are the same.
[0074] Embodiment 13
[0075] The difference between this embodiment and embodiment 1 is that the ginseng stems and leaves-bamboo chips in step 2 are replaced with ginseng stems and leaves, and the other steps are the same.
[0076] Embodiment 14
[0077] The difference between this embodiment and embodiment 1 is that the ginseng root extract in step 2 is replaced by ginseng stem and leaf extract, and the other steps are the same.
[0078] Embodiment 15
[0079] The difference between this embodiment and embodiment 1 is that the ginseng root extract in step 2 is replaced by ginseng adventitious root, and the other steps are the same.
[0080] Example 16
[0081] The difference between this embodiment and embodiment 2 is that feldspar is replaced by quartz stone, and carbonization is not required. The other steps are the same.
[0082] Embodiment 17
[0083] The difference between this embodiment and embodiment 2 is that feldspar is replaced by mica, and carbonization is not required, and the other steps are the same.
[0084] Embodiment 18
[0085] The difference between this embodiment and embodiment 2 is that feldspar is replaced by talc, carbonization is not required, and the other steps are the same.
[0086] Embodiment 19
[0087] The difference between this embodiment and embodiment 1 is that the microporous composite powder is replaced with seaweed charcoal, and the other steps are the same.
[0088] Embodiment 20
[0089] The difference between this embodiment and embodiment 1 is that the mixing ratio of the micronized ginseng extract, the microporous composite powder and the dispersing solvent in step 3 is changed to 0.5%:19.5%:80%, and the other steps are the same.
[0090] Embodiment 21
[0091] The difference between this embodiment and embodiment 1 is that the mixing ratio of the micronized ginseng extract, the microporous composite powder and the dispersing solvent in step 3 is changed to 22%:8%:70%, and the other steps are the same.
[0092] Embodiment 22
[0093] The difference between this embodiment and embodiment 1 is that the ratio of ginseng multifunctional powder to viscose in step 4 is changed to 10%:90%, and the other steps are the same.
[0094] Embodiment 23
[0095] The difference between this embodiment and embodiment 1 is that the ratio of ginseng multifunctional powder to viscose in step 4 is changed to 40%:60%, and the other steps are the same.
[0096] Embodiment 24
[0097] The difference between this embodiment and embodiment 1 is that the ratio of the composite dispersion to the remaining viscose in step 4 is changed to 1:3, and the other steps are the same.
[0098] Embodiment 25
[0099] The difference between this embodiment and embodiment 1 is that the ratio of the composite dispersion to the remaining viscose in step 4 is changed to 1:50, and the other steps are the same.
[0100] Embodiment 26
[0101] The difference between this embodiment and embodiment 1 is that the ratio of the composite dispersion to the remaining viscose in step 4 is changed to 1:25, and the other steps are the same.
[0102] Embodiment 27
[0103] The difference between this embodiment and embodiment 1 is that the ratio of the composite dispersion to the remaining viscose in step 4 is changed to 1:40, and the other steps are the same.
[0104] Embodiment 28
[0105] The difference between this embodiment and embodiment 1 is that the viscose in step 4 is replaced by modal, and the other steps are the same.
[0106] Embodiment 29
[0107] The difference between this embodiment and embodiment 1 is that the viscose in step 4 is replaced by lyocell, and the other steps are the same.
[0108] Embodiment 30
[0109] The difference between this embodiment and embodiment 1 is that the viscose in step 4 is replaced by bamboo pulp fiber, and the other steps are the same.
[0110] Embodiment 31
[0111] The difference between this embodiment and embodiment 1 is that the viscose in step 4 is replaced by modal and viscose, and the other steps are the same.
[0112] Test Example 1 Ginsenoside content test
[0113] The ginsenoside content of the ginseng fibers prepared in Example 1, Example 2 and Example 3 was tested by high performance liquid chromatography.
[0114] Test method:
[0115] 1. Pretreatment method: crush the sample and pass through an 80-mesh sieve; accurately weigh 0.5g of the sample, add deionized water at a ratio of 1g:100ml, ultrasonically extract, adjust the extract to a fixed volume, pass through a 0.22μm organic membrane, and wait for liquid spectrum analysis. 2. Chromatographic condition setting: a. Mobile phase: acetonitrile-water, b. Flow rate: 1.0mL / min, c. Column temperature: 30℃, d. Detection wavelength: 203nm; 3. Sample injection determination: a. Inject the prepared sample solution through an automatic sampler, b. Record the chromatogram and observe the chromatographic peak shape and retention time of ginsenosides. 4. Peak area calculation: a. Use a chromatographic workstation or data processing software to calculate the peak area of each chromatographic peak, b. According to the standard curve, convert the peak area to the corresponding concentration; 5. Content calculation and result analysis: According to the sample injection volume and the converted concentration, calculate the content of ginsenosides in the sample. The test results are shown in Table 1-5.
[0116] Table 1-5 Ginsenoside content
[0117] Sample name Test results (mg / kg) Ginseng Fiber 1# 108.6 Ginseng Fiber 2# 47 Ginseng Fiber 3# 99.1
[0118] Test Example 2 Antioxidant Performance Test
[0119] The ginseng fibers prepared in Example 1, Example 2, and Example 3 were tested according to the standard T / CCTA20102-2023 "DPPH method for determination and evaluation of antioxidant capacity of textiles". DPPH is a dark purple prismatic crystal, which is dark purple in anhydrous ethanol solution. The DPPH free radical has a strong absorption peak at 517nm in the visible light region. This method provides a stable DPPH free radical through DPPH and pairs it with an electron provided by the antioxidant textile, so that the characteristic purple color of the DPPH free radical disappears and becomes colorless or light yellow. The absorbance after the reaction is determined by a visible spectrophotometer, and the antioxidant capacity of the sample is expressed by the free radical scavenging rate. The evaluation criteria are: ≥70 samples have extremely strong antioxidant capacity, 40~<70 samples have good antioxidant capacity, 30~<40 samples have antioxidant capacity, and <30 samples have no antioxidant capacity. The test results are shown in Tables 1-6.
[0120] Table 1-6 Antioxidant capacity test
[0121] Sample name Test results (%) Ginseng Fiber 1# 44.8 Ginseng Fiber 2# 30.1 Ginseng Fiber 3# 89.1
[0122] Test Example 3 Moisturizing Performance Test
[0123] The single-sided sweat cloth made of ginseng fiber and the sweat cloth made of ordinary non-functional fiber were applied to the inner arm of the same test subject symmetrically on both sides to test the skin moisture content; this test method refers to the "QBT4256-2011 Cosmetic Moisturizing Efficacy" in the cosmetics industry, and the cosmetics testing instrument CM825 Skin Moisture Tester was used to test 30 test subjects aged 18-65; the moisture content of the skin was tested before wearing the fabric, and after wearing the fabric for 15 minutes, 30 minutes, 45 minutes, and 60 minutes. Test environment: 23.0±1℃, 50±2% RH, test instrument: CM825 Skin Moisture Tester; Sample test state: dry state, without washing, without controlling the moisture content, and directly tested after humidification; Sample preparation: cut a 5cm*5cm sample.
[0124] Test process: Before wearing the sample, use the CM825 skin moisture tester to test the initial moisture content at the biceps brachii of the arm, then place the sample at the biceps brachii of the arm, and use tape to fix the sample on the arm. After wearing it for 15 minutes, remove the sample and immediately use the instrument to test the moisture content of the human skin surface. After the test is completed, stick the sample to the arm again and test the moisture content of the skin surface at 30 minutes, 45 minutes, and 60 minutes. The instrument test position should be kept consistent as much as possible, and the test distance deviation should not exceed ±1cm. The width of the tape used each time should be consistent, and the method of fixing the fabric with tape should be consistent.
[0125] Finally, the test results are expressed by the change in the moisture content of the skin's keratin. The results of ginseng fiber 1# are shown in Table 1-7, and the line chart is as follows: Figure 1 shown.
[0126] Table 1-7 Changes in moisture content of skin keratin in ginseng fiber 1#
[0127] Project Description Ginseng fiber 1#(%) Ordinary viscose fiber(%) Before wearing 44.76 40.78 After wearing for 15 minutes 41.08 36.10 After wearing for 30 minutes 38.46 38.80 After wearing for 45 minutes 38.88 38.40 After wearing for 60 minutes 40.86 37.14 After wearing for 60 minutes 44.76 40.78
[0128] The results of ginseng fiber 2# are shown in Table 1-8, and the line chart is as follows Figure 2 shown.
[0129] Table 1-8 Changes in moisture content of skin keratin in ginseng fiber 2#
[0130] Project Description Ginseng fiber 2#(%) Ordinary viscose fiber(%) Before wearing 30.3 31.2 After wearing for 15 minutes 35.6 31.8 After wearing for 30 minutes 32.5 28.8 After wearing for 45 minutes 34.8 31.3 After wearing for 60 minutes 32.6 28.8 After wearing for 60 minutes 30.3 31.2
[0131] The results of ginseng fiber 3# are shown in Table 1-9, and the line chart is as follows Figure 3 shown.
[0132] Table 1-9 Changes in moisture content of skin keratin of ginseng fiber 3#
[0133] Project Description Ginseng fiber 3#(%) Ordinary viscose fiber(%) Before wearing 40.10 34.42 After wearing for 15 minutes 41.92 35.34 After wearing for 30 minutes 39.72 34.16 After wearing for 45 minutes 47.96 40.56 After wearing for 60 minutes 44.08 35.72 After wearing for 60 minutes 40.10 34.42
[0134] Ginseng contains a variety of active ingredients, such as ginsenosides, polysaccharide compounds, amino acids, vitamins and minerals. Ginseng extract has good permeability and can penetrate deep into the skin, replenish and lock the moisture needed by the skin, and enhance the skin's own water retention capacity; the ginsenosides and polysaccharides therein help to form a moisturizing film, reduce water evaporation, and regulate moisture balance. From the above experiments, it can be seen that the moisturizing performance of the skin wearing ginseng fiber fabrics is better than that of ordinary viscose fiber fabrics, among which sodium alginate has the best effect.
[0135] Test Example 4 Far infrared performance test
[0136] The ginseng fibers prepared in Example 1, Example 2 and Example 3 were tested according to GB / T30127-2013 Testing and Evaluation of Far-Infrared Performance of Textiles. According to the provisions of GB / T30127-2013 Testing and Evaluation of Far-Infrared Performance of Textiles, for general samples, if the far-infrared emissivity of the sample is not less than 0.88, and the far-infrared radiation temperature rise is not less than 1.4°C, the sample has far-infrared function; for loose samples such as flakes, non-wovens, and plush, if the far-infrared emissivity of the sample is not less than 0.83, and the far-infrared radiation temperature rise is not less than 1.7°C, the sample has far-infrared function. According to the measured data, they are all higher than the national standard, indicating that the three ginseng fibers have far-infrared function. The results are shown in Tables 1-10.
[0137] Table 1-10 Far infrared performance test results
[0138]
[0139] Test Example 5 Negative ion performance test
[0140] The single-sided jersey woven with ginseng fiber prepared in the three schemes of Example 1, Example 2 and Example 3 was tested according to GB / T30128-2013 Detection and evaluation of negative ion generation of textiles. The evaluation of negative ion generation in GB / T30128-2013 Detection and evaluation of negative ion generation of textiles is as follows: >1000 negative ion generation is relatively high; 550-1000 negative ion generation is medium; <550 negative ion generation is relatively low. According to the measured data, the negative ion generation of ginseng fiber is relatively high. The results are shown in Tables 1-11.
[0141] Table 1-11 Negative ion performance test results
[0142]
[0143]
[0144] Test Example 6 Antibacterial Performance Test
[0145] The single-sided jersey made of ginseng fiber prepared in Example 1, Example 2 and Example 3 was tested according to "FZ / T 73023-2006 Antibacterial Knitwear". According to the standard, the number of times the antibacterial knitwear can withstand water washing and the different test bacteria species are divided into three antibacterial levels: A, AA and AAA. The antibacterial rate index requirements for the test bacteria species are shown in Table 1-12. According to the test results, the antibacterial rates of the three fibers meet the AAA standard requirements of "FZ / T 73023-2006 Antibacterial Knitwear", indicating that the three fibers have good antibacterial properties. The results are shown in Table 1-13.
[0146] Table 1-12 Antibacterial rate index of antibacterial knitwear
[0147]
[0148] Table 1-13 Antibacterial performance test results
[0149]
[0150] Test Example 7 Anti-mite performance test
[0151] The single-sided jersey woven with ginseng fibers prepared in Example 1, Example 2 and Example 3 were tested according to the repellency method 9.1 of "GB / T 24253-2009 Evaluation of anti-mite performance of textiles". The dust mite sample was pretreated by drying at 65°C for 10 minutes and washed 20 times according to "GB / T 12490-2007 Textiles - Colour fastness test - Colour fastness to household and commercial washing". The evaluation criteria of this standard are as follows: repellency rate ≥ 95%, the sample has an extremely strong anti-mite effect; repellency rate ≥ 80%, the sample has a relatively strong anti-mite effect; repellency rate ≥ 60%, the sample has an anti-mite effect. According to the test results, the mite repellency rate of ginseng fiber 1# is 60.13%, the mite repellency rate of ginseng fiber 2# is 62.11%, and the mite repellency rate of ginseng fiber 3# is 78.18%. The three ginseng fabric samples have different degrees of anti-mite effects.
[0152] Test Example 8 Physical and Mechanical Properties Test
[0153] The specification of ginseng fiber prepared in Example 1, Example 2 and Example 3 was made into 1.2D×38mm. The three kinds of ginseng viscose fibers were tested in accordance with GBT14463-2022 Viscose Staple Fibers. All indicators met the standard requirements. The results are shown in Table 1-14.
[0154] Table 1-14 Physical and mechanical properties test results
[0155]
[0156]
[0157] The present application provides a method for preparing multifunctional fibers, which specifically includes the following steps: micronizing ginseng extract to obtain micronized ginseng extract; carbonizing far-infrared negative ion powder, filtering and grinding to obtain microporous composite powder; adding the micronized ginseng extract and the microporous composite powder to a dispersion solvent, stirring, drying and grinding to obtain ginseng multifunctional powder; mixing the ginseng multifunctional powder with part of cellulose spinning solution once to obtain a composite dispersion liquid, and then mixing the composite dispersion liquid with the remaining part of cellulose spinning solution for a second time, and allowing to stand to obtain a composite spinning adhesive; spinning to obtain To multifunctional fiber; the technical scheme combines the antioxidant properties of ginsenosides with the far-infrared, negative ion, and antibacterial and anti-mite functions of far-infrared negative ion functional powders, and adopts a compounding process of first small mixing and then blending to first prepare a composite dispersion with extremely high dispersibility and stability, and then blend the composite dispersion with the cellulose spinning solution to form a uniform and stable composite spinning glue, thereby ensuring that the ginseng powder and the far-infrared negative ion powder are evenly dispersed inside the fiber, so that the prepared fiber has the functions of antioxidant, moisturizing, far-infrared, negative ion, antibacterial and anti-mite, which improves the problems of short-lasting functions and single functions in the prior art.
[0158] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0159] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a multifunctional fiber, characterized in that: The specific steps include:
1. micronizing the ginseng extract to obtain a micronized ginseng extract; 2. Prepare far-infrared negative ion powder after filtering and grinding; 3. adding the micronized ginseng extract and the far-infrared negative ion powder into a dispersing solvent, stirring, drying, and grinding to obtain ginseng multifunctional powder; Fourth, the ginseng multifunctional powder is mixed with part of the cellulose spinning solution to obtain a composite dispersion, and the composite dispersion is mixed with the remaining part of the cellulose spinning solution for a second time, and the composite spinning glue is obtained after standing; 5. Multifunctional fibers are obtained by spinning.
2. The method for preparing a multifunctional fiber according to claim 1, characterized in that: Step 1: The ginseng extract is one of ginseng root extract, ginseng stem and leaf extract or ginseng adventitious root; the particle size of the micronized ginseng extract is 3 μm, the total ginsenoside content is 80.2%, and the drying loss is 1.6%.
3. The method for preparing a multifunctional fiber according to claim 1, characterized in that: In step 2, the far-infrared negative ion powder is one of microporous composite powder, silicate powder or seaweed; the microporous composite powder includes inorganic powder and plant residues, the inorganic powder is one or more of zinc oxide, aluminum oxide, zirconium oxide, tourmaline, germanium stone, diatomaceous earth or zeolite, the plant residue is one or more of ginseng stems and leaves, bamboo chips, tea residues, coffee residues; the silicate powder is one or more of feldspar, quartz, mica or talc, and the seaweed is one or more of sodium alginate or seaweed charcoal.
4. The method for preparing a multifunctional fiber according to claim 3, characterized in that: The mixing ratio of the inorganic powder to the plant residue is 1:
5.
5. The method for preparing a multifunctional fiber according to claim 3, characterized in that: The microporous composite powder and seaweed charcoal need to be carbonized, and the carbonization temperature is 1000-1200° C. The particle size of the far-infrared negative ion powder is 300-500 nm, and the porosity is 40-50%.
6. The method for preparing a multifunctional fiber according to claim 1, characterized in that: Step 3: The preparation step of the dispersion solvent is as follows: add the hydrophilic solvent into deionized water and stir in a high-speed stirrer for 1 hour.
7. The method for preparing a multifunctional fiber according to claim 6, characterized in that: The hydrophilic solvent is one of polyvinyl pyrrolidone, N,N-di(2,2,6,6-tetramethyl-4-piperidinyl)-1,3-benzenediamide or a hydrophilic acrylic acid hyperbranched block copolymer; the mass of the acrylic acid hyperbranched block copolymer is 25% of the deionized water.
8. The method for preparing a multifunctional fiber according to claim 1, characterized in that: The stirring time in step three is 4 hours; the particle size of the ginseng multifunctional powder is 3 μm; the mixing ratio of the micronized ginseng extract, the microporous composite powder and the dispersing solvent is 0.5%:19.5%:80%-22%:8%:70%.
9. The method for preparing a multifunctional fiber according to claim 1, characterized in that: In step 4, the cellulose spinning solution is one or more of viscose, modal, lyocell, bamboo pulp fiber, etc., and the mass fraction ratio of ginseng multifunctional powder to cellulose spinning solution in the first mixing is 10%:90%-40%:60%.
10. The method for preparing a multifunctional fiber according to claim 1, characterized in that: The specific steps of the secondary mixing in step 4 are: secondary mixing the composite dispersion and the remaining part of the cellulose spinning solution at a ratio of 1:3-50 through a diaphragm pump and a plunger pump, stirring for 0.5 hours with a high-speed stirrer, and standing for 2 hours.
Citation Information
Patent Citations
Multifunctional composite lyocell fiber and preparation method thereof
CN103590125A
Plant-based cellulose fibers with antibacterial, health-care and skin-care functions and preparation method thereof
CN107761183A
Multifunctional composite additive, viscose with functions of resisting bacteria and mites and generating negative ions as well as preparation method of viscose
CN109321991A
Composite functional regenerated cellulose fiber and preparation method thereof
CN110373734A
Multifunctional regenerated cellulose fibers and preparation method thereof
CN110791828A
Cited By
Inorganic-organic material structure bidirectional-effect high-sensitivity fiber and preparation method thereof
CN121653863A