Method for quasi-in-situ tracking of trace element distribution of high-temperature alloy

Through surface treatment and micro-zone X-ray fluorescence analysis technology, combined with ion thinning, quasi-in-situ tracking of trace elements distribution in high-temperature alloys is achieved, solving the problem that the existing technology cannot track elements less than 10ppm, and improving the mechanical properties of the alloy and craft design.

CN118961777AActive Publication Date: 2024-11-15INST OF METAL RESEARCH - CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410973211.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-15
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The prior art cannot realize non-destructive quasi-in-situ tracking of trace elements with content less than 10 ppm in high-temperature alloys, and cannot effectively study and optimize the relative distribution changes of trace elements under high-temperature treatment conditions, affecting the mechanical properties of the alloy.

Method used

The surface treatment technology is used to mark the surface of high-temperature alloy samples, and the micro-zone X-ray fluorescence analysis combined with ion thinning technology is used to measure the distribution of trace elements before and after high-temperature treatment, and then analyze them again after the oxide layer is removed to achieve the relative distribution of trace elements. Change tracking.

Benefits of technology

Quasi-in-situ tracking of elements with content less than 10ppm in high-temperature alloys is achieved, and quantification and spatial resolution are accurately determined, the distribution position of trace elements is optimized, and the mechanical properties and process design of high-temperature alloys are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961777A_ABST
    Figure CN118961777A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of material component analysis, and particularly relates to a method for quasi-in-situ tracking of trace element distribution of a high-temperature alloy. Selecting a high-temperature alloy sample, and treating the surface of the sample into a mirror surface; performing target position pattern marking on the surface of the sample, and treating the surface of the sample into a mirror surface after marking; putting into a micro-area X-ray fluorescence analysis device, positioning and then carrying out micro-area X-ray fluorescence analysis; carrying out high-temperature treatment on the sample subjected to fluorescence analysis, and then determining the thickness of an oxide layer by utilizing a size measurement technology; removing an oxide layer by using an ion thinning device; after the sample without the oxide layer is positioned, the sample is put into a micro-area X-ray fluorescence analysis device for micro-area X-ray fluorescence analysis, and quasi-in-situ tracking of relative change of trace element distribution under the high-temperature treatment condition is achieved. On one hand, the content of the microelements in the high-temperature alloy can be accurately and quantitatively obtained, and on the other hand, the optimal distribution position of the microelements can be optimized and determined, so that the processing technology is determined.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material composition analysis, and in particular relates to a method for quasi-in-situ tracking of trace element distribution of high-temperature alloys. Background Art

[0002] High-temperature alloys refer to high-alloy iron-based, nickel-based and cobalt-based austenitic metal materials that can work at high temperatures above 600°C, withstand high and complex stresses, and have surface stability. They are irreplaceable key structural materials for high-temperature parts of aircraft engines and gas turbines, and are widely used in turbine blades, guide vanes, turbine disks, and combustion chambers. The quality of high-temperature alloys determines the performance of engines and gas turbines.

[0003] High-temperature alloys generally contain 10 to 20 elements. In high-temperature alloys, a variety of trace elements may segregate in dendrites or grain boundaries to form low-melting phases, or promote the precipitation of harmful phases, or even form inclusions, which become channels for crack generation and expansion. The local enrichment of these trace elements can have a significant effect on the mechanical properties of high-temperature alloys, such as reducing high-temperature tensile plasticity, high-temperature fatigue and creep properties. In directionally solidified columnar crystal high-temperature alloys and directionally solidified single crystal high-temperature alloys, the content control of elements such as P, Pb, Sb, As, Sn, Bi, Ag, Ga, Ti, Te, and Se is demanding, and it is often necessary to control one or more elements to less than 10ppm. This poses a challenge to the accuracy of alloy chemical composition analysis technology. Under the premise of keeping the trace element content unchanged, the high temperature heat treatment conditions are changed to study the relative distribution changes of trace elements at grain boundaries and within grains, the relative changes between dendrites, the relative changes between dendrite stems, primary dendrites, secondary dendrites and tertiary dendrites, and the relative changes between eutectic and non-eutectic structures at different heat treatment temperatures, so that the trace elements are distributed in the best position, thereby giving full play to the maximum potential of the alloy under the same composition and obtaining excellent comprehensive properties. These studies require some non-destructive quasi-in-situ tracking technology.

[0004] Existing technologies cannot achieve non-destructive high-temperature quasi-in-situ tracking of the distribution of elements with a content of less than 10ppm. The analysis accuracy of the energy dispersive system (EDS) of a scanning electron microscope is up to 100ppm; the analysis accuracy of an X-ray fluorescence instrument is up to 100ppm; the analysis accuracy of an electron probe (EPMA) is up to tens of ppm; the analysis accuracy of time-of-flight secondary ion mass spectrometry technology reaches the ppm level, but it is a destructive technology, and because only some ions are collected, the quantitative ability is seriously insufficient; the analysis accuracy of an inductively coupled plasma mass spectrometer (ICP-MAS) reaches the ppm level, which is also a destructive technology and cannot repeatedly measure and track the relative changes in the distribution of elements. For researchers, being able to analyze elements with a content of less than 10ppm and to achieve quasi-in-situ tracking of their relative distribution changes at high temperatures will help optimize the process, improve the mechanical properties of high-temperature alloys, and accelerate their application in engines and gas turbines. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a method for quasi-in-situ tracking of trace element distribution in high-temperature alloys. The method can be used to quasi-in-situ track the relative changes in the distribution of elements with a content less than 10 ppm under high-temperature treatment conditions.

[0006] The technical solution of the present invention is:

[0007] A method for quasi-in-situ tracking of trace element distribution in a high-temperature alloy comprises the following steps:

[0008] Step 1: Select a high-temperature alloy sample and use surface treatment technology to process the sample surface into a mirror surface;

[0009] Step 2: Mark the target position pattern on the mirror sample of step 1 using marking technology;

[0010] Step 3: Use surface treatment technology to process the marked sample surface into a mirror surface;

[0011] Step 4: Immediately place the sample obtained in step 3 into a micro-area X-ray fluorescence analysis device, use positioning technology to select a target area ROI in the marked area, perform micro-area X-ray fluorescence analysis, repeat the measurement multiple times, and obtain trace element distribution result 1;

[0012] Step 5: subjecting the sample after micro-area X-ray fluorescence analysis to high temperature treatment;

[0013] Step 6: Determine the thickness of the oxide layer of the sample after high temperature treatment using dimensional measurement technology;

[0014] Step 7: After determining the thickness of the oxide layer, use an ion thinning device to remove the oxide layer at the ROI;

[0015] Step 8: Place the sample with the oxide layer removed into a micro-area X-ray fluorescence analysis device, select the target area ROI in the marked area using positioning technology, perform micro-area X-ray fluorescence analysis, and repeat the measurement multiple times to obtain the element and trace element distribution result 2;

[0016] Step 9: Repeat steps 5 to 8 to obtain multiple element distribution results, and realize quasi-in-situ tracking of the relative changes of trace element distribution under high temperature treatment conditions.

[0017] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 1, the high-temperature alloy samples include various grades of high-temperature alloys that have been developed or are being developed at home and abroad.

[0018] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 1, the surface treatment technology is metallographic grinding and polishing technology, electrolytic polishing technology or ion cleaning technology.

[0019] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 2, the marking technology is hardness pit technology, laser marking technology, manual marking or ion processing technology; the marking pattern includes any easily identifiable figure among triangles, quadrilaterals, pentagons, flowers and cones.

[0020] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 4, the micro-area refers to a beam spot size less than 20 μm; the micro-area X-ray fluorescence analysis device includes a micro-area device based on a laboratory light source or a micro-area device based on a synchrotron radiation light source.

[0021] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 4, the positioning technology refers to optical microscope positioning, laser positioning or X-ray positioning technology.

[0022] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 4, trace elements refer to elements with a content of less than 10 ppm.

[0023] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 5, high-temperature treatment refers to various heat treatments performed at a temperature above 600°C.

[0024] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 6, the dimension measurement technology refers to a screw micrometer, a scanning electron microscope, an X-ray imaging instrument or a laser rangefinder.

[0025] In the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, in step 7, the ion thinning device includes various devices that use ion beams to perform micro-nano processing and surface treatment.

[0026] The design concept of the present invention is:

[0027] In view of the problems of low precision and sample destruction of existing chemical composition analysis technology, and aimed at the demand for trace element control in high-temperature alloys, a method for quasi-in-situ tracking of trace element distribution in high-temperature alloys was invented to solve the bottleneck problems of optimal position of trace element distribution and process optimization in the field of high-temperature alloys.

[0028] The advantages and beneficial effects of the present invention are:

[0029] The present invention can be used to quasi-in-situ track the relative changes in the distribution of elements with a content of less than 10ppm under high-temperature treatment conditions. The present invention focuses on the control and optimization of elements with a content of 10ppm or lower. On the one hand, the content of trace elements in high-temperature alloys can be accurately and quantitatively obtained. On the other hand, under the premise that the total content of the same trace element remains unchanged, its optimal distribution position can be optimized and determined, thereby determining the processing and treatment process, improving mechanical properties such as high-temperature creep, fatigue and tensile plasticity, and opening up new directions for research in related fields. The present invention is not only suitable for high-temperature alloy samples, but can also be extended to various types of metals, ceramics, composite materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of the method for quasi-in-situ tracking of trace element distribution in high-temperature alloys.

[0031] Figure 2 The optical microscope image (a) and the surface distribution image (b) of the Bi element with a content of about 0.5 ppm by micro-area X-ray fluorescence analysis. DETAILED DESCRIPTION

[0032] like Figure 1 As shown, in the specific implementation process, the quasi-in-situ tracking method of trace element distribution of high-temperature alloy includes the following steps: selecting a high-temperature alloy sample and processing the sample surface into a mirror surface; marking the target position pattern on the sample surface, and then processing the sample surface into a mirror surface after marking; placing it in a micro-area X-ray fluorescence analysis device, positioning it, and performing micro-area X-ray fluorescence analysis (μXRF), with an analysis accuracy of sub-ppm level, and the micro area refers to a beam spot size of less than 20μm, which can reach 5-10μm; high-temperature treatment of the sample after fluorescence analysis, and then determining the thickness of the oxide layer using size measurement technology; using an ion thinning device to remove the oxide layer; positioning the sample without the oxide layer, placing it in a micro-area X-ray fluorescence analysis device, and performing micro-area X-ray fluorescence analysis to achieve quasi-in-situ tracking of the relative changes in the distribution of trace elements under high-temperature treatment conditions, and high-temperature treatment refers to various heat treatments performed at 600-1500°C, such as: long-term creep, long-term aging, long-term durability, high-temperature fatigue, and solution treatment with a heat preservation time of 1-100 hours.

[0033] The present invention is described in detail below in conjunction with specific embodiments.

[0034] Embodiment 1:

[0035] In this embodiment, DZ640M cobalt-based precipitation-strengthened directionally solidified columnar superalloy is selected to perform quasi-in-situ tracking of the distribution of trace element Bi, and the steps are as follows:

[0036] Step 1: Use metallographic grinding and polishing technology to process the sample surface into a mirror surface;

[0037] Step 2: Using laser marking technology, an isosceles triangle pattern is etched on the surface of the mirror sample of step 1;

[0038] Step 3: After the pattern is etched, the sample surface is processed into a mirror surface by using ion cleaning technology;

[0039] Step 4: The sample obtained in step 3 is immediately placed in the Attomap micro-area X-ray fluorescence analysis device produced by SIGRAY, USA, and the sample cavity is evacuated; using the optical microscope in the optical path, the ROI area is selected at the vertex of the isosceles triangle pattern, and the area size is 0.6mm×0.6mm; the Mo target with an energy of 17.4keV is selected, the beam spot size is adjusted to 8μm, and the micro-area X-ray fluorescence analysis is performed using a step-scan method. After 3 repeated measurements, the distribution results of the trace element Bi are obtained1, see Figure 2 ;

[0040] Step 5: Heat the sample after fluorescence analysis to 1150°C and keep it warm for 10 hours;

[0041] Step 6: Using a scanning electron microscope to determine the oxide layer thickness of the sample obtained in step 5 is about 1 μm;

[0042] Step 7: After determining the thickness of the oxide layer, use a precision ion etching device, adjust the voltage to 5kV, adjust the current to 2mA, and the etching time to 30min to completely remove the oxide layer;

[0043] Step 8: Immediately place the sample with the oxide layer removed into the Attomap micro-area X-ray fluorescence analysis device, and use positioning technology to select the target area for fluorescence analysis in step 4 in the marked area, and perform micro-area X-ray fluorescence analysis. After three repeated measurements, the distribution result 2 of the trace element Bi is obtained, realizing the quasi-in-situ tracking of the relative changes in the distribution of the trace element Bi under high-temperature treatment conditions.

[0044] In this embodiment, the Bi element content is about 0.5ppm, which is very difficult to detect. The surface treatment requirements are very high, and the requirements for oxide layer removal are also very high. Any surface contamination will affect the detection signal and fluorescence analysis results. The present invention breaks the limitations of conventional chemical composition analysis technology and innovatively achieves high spatial resolution, high precision and non-destructive quasi-in-situ tracking of the relative change of Bi element distribution under high temperature processing conditions.

[0045] Embodiment 2:

[0046] In this embodiment, DD406 nickel-based directionally solidified single crystal high-temperature alloy is selected to perform quasi-in-situ tracking of the distribution of trace element Pb, and the steps are as follows:

[0047] Step 1: Use metallographic grinding and polishing technology to process the sample surface into a mirror surface;

[0048] Step 2: Using the hardness pit technology, mark the mirror sample of step 1 with a triangular pyramid pattern on the sample surface;

[0049] Step 3: Use ion cleaning technology to process the sample surface after marking the pattern into a mirror surface;

[0050] Step 4: Place the sample obtained in step 3 into the BL15U1 hard X-ray microfocusing and application beamline station of Shanghai Light Source; use the X-ray positioning technology in the optical path to select the ROI area at the vertex of the triangular pyramid pattern, with an area size of 0.2 mm×0.2 mm; adjust and use monochromatic light with an energy of 5.4 keV, adjust the beam spot size to 10 μm, and use a 10×10 equally spaced point array scanning method to perform micro-area X-ray fluorescence analysis. After 5 repeated measurements, the distribution result 1 of the trace element Pb is obtained;

[0051] Step 5: Heat the sample after fluorescence analysis to 1200°C and keep it at this temperature for 16 hours;

[0052] Step 6: Using X-ray three-dimensional imaging technology to determine that the oxide layer thickness of the sample obtained in step 5 is about 1.8 μm;

[0053] Step 7: After determining the thickness of the oxide layer, use a precision ion etching device, adjust the voltage to 5kV, adjust the current to 2mA, and the etching time to 54min to completely remove the oxide layer;

[0054] Step 8: The sample with the oxide layer removed is immediately placed in the BL15U1 hard X-ray microfocusing and application beamline station of the Shanghai Synchrotron Radiation Facility. Using positioning technology, the target area for fluorescence analysis in step 4 is selected in the marked area, and micro-area X-ray fluorescence analysis is performed. After 5 repeated measurements, the distribution result 2 of the trace element Pb is obtained, realizing the quasi-in-situ tracking of the relative changes in the distribution of the trace element Pb under high-temperature treatment conditions.

[0055] In this embodiment, the Pb element content is about 5ppm, which is difficult to detect and requires very high surface treatment and oxide layer removal. Any surface contamination will affect the detection signal and fluorescence analysis results. The present invention breaks the limitations of conventional chemical composition analysis technology and innovatively achieves high spatial resolution, high precision and non-destructive quasi-in-situ tracking of the relative change of Pb element distribution under high temperature treatment conditions.

Claims

1. A method for quasi-in-situ tracking of trace element distribution in high-temperature alloys, characterized in that: The steps include: Step 1: Select a high-temperature alloy sample and use surface treatment technology to process the sample surface into a mirror surface; Step 2: Mark the target position pattern on the mirror sample of step 1 using marking technology; Step 3: Use surface treatment technology to process the marked sample surface into a mirror surface; Step 4: Immediately place the sample obtained in step 3 into a micro-area X-ray fluorescence analysis device, use positioning technology to select a target area ROI in the marked area, perform micro-area X-ray fluorescence analysis, repeat the measurement multiple times, and obtain trace element distribution result 1; Step 5: subjecting the sample after micro-area X-ray fluorescence analysis to high temperature treatment; Step 6: Determine the thickness of the oxide layer of the sample after high temperature treatment using dimensional measurement technology; Step 7: After determining the thickness of the oxide layer, use an ion thinning device to remove the oxide layer at the ROI; Step 8: Place the sample with the oxide layer removed into a micro-area X-ray fluorescence analysis device, select the target area ROI in the marked area using positioning technology, perform micro-area X-ray fluorescence analysis, and repeat the measurement multiple times to obtain the element and trace element distribution result 2; Step 9: Repeat steps 5 to 8 to obtain multiple element distribution results, and realize quasi-in-situ tracking of the relative changes of trace element distribution under high temperature treatment conditions.

2. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 1, the high-temperature alloy samples include various grades of high-temperature alloys that have been developed or are being developed at home and abroad.

3. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 1, the surface treatment technology is metallographic grinding and polishing technology, electrolytic polishing technology or ion cleaning technology.

4. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 2, the marking technology is hardness pit technology, laser marking technology, manual marking or ion processing technology; the marking pattern includes any easily recognizable shape such as triangle, quadrilateral, pentagon, flower, cone.

5. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 4, the micro area refers to a beam spot size less than 20 μm; the micro area X-ray fluorescence analysis device includes a micro area device based on a laboratory light source or a micro area device based on a synchrotron radiation light source.

6. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 4, the positioning technology refers to optical microscope positioning, laser positioning or X-ray positioning technology.

7. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 4, trace elements refer to elements with a content less than 10 ppm.

8. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 5, high temperature treatment refers to various heat treatments performed at a temperature above 600°C.

9. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 6, the dimension measurement technique refers to a micrometer screw, a scanning electron microscope, an X-ray imaging instrument or a laser rangefinder.

10. The method for quasi-in-situ tracking of trace element distribution in high-temperature alloys according to claim 1, characterized in that: In step 7, the ion thinning device includes various devices that use ion beams to perform micro-nano processing and surface treatment.

Citation Information

Patent Citations

  • In-situ analysis method for characterizing high-temperature alloy component distribution by using X-ray fluorescence spectrum

    CN110865092A

  • Aluminum alloy structure microscopic segregation quantitative characterization method based on micro-beam X-ray fluorescence

    CN114594118A

  • Method, apparatus and marking substance kit for multi-parameter x-ray fluorescence imaging

    CN114667447A

  • In-situ statistical distribution characterization method of precipitated phase particles in high-temperature alloy

    CN117147390A

  • Solid material characterization with x-ray spectra in both transmission and fluoresence modes

    US20120321039A1

Cited By

  • Online steel component automatic analysis method based on X-ray fluorescence spectrometer

    CN119985579A