Secondary battery and battery module, battery pack and electric device including same

By using lithium-containing phosphate with olivine structure and its modified compounds as the positive electrode film layer in the secondary battery, and adding specific organic solvents and additives to the electrolyte, the energy density and kinetic performance of the secondary battery are solved. The problem is that high energy density, good kinetic performance and low volume expansion rate are achieved.

CN118970191AActive Publication Date: 2024-11-15CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411013552.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2021-07-30
Publication Date
2024-11-15
Estimated Expiration
2041-07-30

AI Technical Summary

Technical Problem

While improving the energy density of existing secondary batteries, it is difficult to take into account both the dynamic performance and capacity retention rate, and the volume expansion rate is relatively high.

Method used

A secondary battery design is adopted that includes a positive electrode film layer and an electrolyte solution, where the positive electrode film layer is composed of lithium-containing phosphate with olivine structure and its modified compounds, and specific organic solvents and additives are added to the electrolyte solution to optimize the wetting of the electrolyte solution. and ensure stable transport of active ions by controlling the content of electrolyte and additives.

Benefits of technology

It achieves good kinetic performance, high capacity retention rate and low volume expansion rate while maintaining high energy density, improving the cycle performance and storage performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970191A_ABST
    Figure CN118970191A_ABST
Patent Text Reader

Abstract

The invention discloses a secondary battery, a battery module containing the secondary battery, a battery pack and an electric device. The secondary battery comprises a positive pole piece and an electrolyte, the positive pole piece comprises a positive pole current collector and a positive pole film layer arranged on at least one surface of the positive pole current collector; the positive pole film layer comprises one or more of lithium-containing phosphate with an olivine structure and a modified compound of the lithium-containing phosphate. The electrolyte comprises an organic solvent, and the organic solvent comprises a first solvent as shown in the formula 1. R < 11 > is one of hydrogen, an alkyl group with 1 to 4 carbon atoms and a halogenated alkyl group with 1 to 4 carbon atoms, and R < 12 > is one of an alkyl group with 1 to 4 carbon atoms and a halogenated alkyl group with 1 to 4 carbon atoms. Based on the mass of the electrolyte, the mass percentage of the first solvent is greater than or equal to 20%. The secondary battery satisfies the condition that the mass of the electrolyte / the rated capacity of the secondary battery is less than or equal to 3.6 g / Ah. The secondary battery provided by the invention can maintain high energy density, and has good dynamic performance, relatively high capacity retention rate and relatively low volume expansion rate at the same time. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with the application date of July 30, 2021, application number 202180006893.9 (international application number PCT / CN2021 / 109903), and invention name "Secondary battery and battery module, battery pack and electrical device containing the secondary battery". Technical Field

[0002] The present application belongs to the technical field of secondary batteries, and specifically relates to a secondary battery and a battery module, a battery pack and an electrical device containing the secondary battery. Background Art

[0003] Secondary batteries have the characteristics of good cycle performance, stable electrochemical performance, and low price, so they occupy a large market share. As customers' requirements for battery energy density become higher and higher, it is crucial to develop batteries with higher energy density and longer cycle life. At present, an effective way to improve battery energy density is to increase the internal space utilization of the battery, for example, to increase the coating weight and compaction density of the pole piece, but the disadvantage is that the transmission path of the active ions becomes longer and the diffusion rate of the active ions becomes slower, making it difficult for the active ions to be deintercalated between the positive and negative electrodes of the battery, and the battery's kinetic performance deteriorates. Summary of the invention

[0004] The purpose of the present application is to provide a secondary battery and a battery module, a battery pack and an electrical device containing the secondary battery, so as to enable the secondary battery to have good dynamic performance, a high capacity retention rate and a low volume expansion rate while maintaining a high energy density.

[0005] In a first aspect, the present application provides a secondary battery, which includes a positive electrode plate and an electrolyte. The positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, and the positive electrode film layer includes one or more of an olivine-structured lithium-containing phosphate and a modified compound thereof. The electrolyte includes an organic solvent, and the organic solvent includes a first solvent shown in Formula 1.

[0006]

[0007] In formula 1, R 11 and R 12 Each is independently one of a C1-C4 alkyl group and a C1-C4 halogenated alkyl group.

[0008] The secondary battery of the present application satisfies: the mass of the first solvent / rated capacity of the secondary battery ≥ 0.7 g / Ah, and the mass of the electrolyte / rated capacity of the secondary battery ≤ 3.5 g / Ah.

[0009] When the secondary battery of the present application satisfies the mass of the first solvent / rated capacity of the secondary battery ≥ 0.7g / Ah and the mass of the electrolyte / rated capacity of the secondary battery ≤ 3.5g / Ah, the electrolyte inside the battery can well infiltrate the positive electrode plate and the negative electrode plate, giving full play to the improvement effect of the first solvent on the battery kinetic performance, and the irreversible consumption of active ions inside the battery can also be controlled within a small range. Therefore, the secondary battery can have good kinetic performance, high capacity retention rate and low volume expansion rate while maintaining high energy density.

[0010] Optionally, the mass of the first solvent / rated capacity of the secondary battery is ≥ 1.0 g / Ah.

[0011] Optionally, the mass of the electrolyte / rated capacity of the secondary battery is 2.8 g / Ah-3.3 g / Ah.

[0012] In any embodiment of the present application, the secondary battery also satisfies: the content of the first solvent / (thickness of the positive electrode film layer×3+0.008 / porosity of the positive electrode film layer)≥1. The content of the first solvent refers to the mass percentage of the first solvent based on the total mass of the organic solvent; the thickness of the positive electrode film layer refers to the thickness of the single-sided positive electrode film layer on the positive electrode current collector in mm. At this time, the problem of poor battery kinetic performance caused by the increase in the coating weight and compaction density of the positive electrode film layer can be effectively solved.

[0013] Optionally, the secondary battery further satisfies: content of the first solvent / (thickness of the positive electrode film layer×3+0.008 / porosity of the positive electrode film layer)≥1.5.

[0014] In any embodiment of the present application, the electrolyte further includes an additive.

[0015] Optionally, the reduction potential of the additive is ≥ 0.8V (vs Li+ / Li). At this time, the additive can participate in the formation of the SEI film on the surface of the negative electrode active material by electrochemical reduction reaction in priority to the organic solvent, and promote the formation of a stable SEI film on the surface of the negative electrode active material, prevent the negative electrode active material from further reacting with the electrolyte, and reduce the degree of damage to the SEI film by protons generated by the reduction of the first solvent.

[0016] In any embodiment of the present application, the additive includes an organic additive, and the organic additive includes one or more of vinylene carbonate, fluoroethylene carbonate, vinyl carbonate, vinyl sulfate, and 1,3-propane sultone. The organic additive can be preferentially electrochemically reduced on the surface of the negative electrode active material to form an SEI film with excellent performance, reducing the degree of damage to the SEI film by the protons generated by the first solvent reduction. The reduction products of the organic additive are mainly organic components, which can improve the mechanical stability of the SEI film and help improve the cycle performance of the battery.

[0017] In any embodiment of the present application, the additive includes an inorganic additive, and the inorganic additive includes one or more of tris(trimethylsilyl)phosphate, lithium bis(oxalatoborate), lithium difluorobis(oxalatophosphate), lithium tetrafluorooxalatophosphate, lithium difluorooxalatoborate, and lithium difluorophosphate. The inorganic additive can be preferentially electrochemically reduced on the surface of the negative electrode active material to form an SEI film with excellent performance, thereby reducing the degree of damage to the SEI film by the protons generated by the reduction of the first solvent. The reduction products of the inorganic additive are mainly inorganic components, which can improve the thermal stability of the SEI film and are beneficial to improving the high temperature performance of the battery.

[0018] In any embodiment of the present application, based on the total mass of the additive, the mass percentage of the organic additive is ≥50%. Optionally, the mass percentage of the organic additive is 70%-100%.

[0019] In any embodiment of the present application, based on the total mass of the additives, the mass percentage of the inorganic additives is ≤50%. Optionally, the mass percentage of the inorganic additives is 0%-30%.

[0020] In any embodiment of the present application, the secondary battery further includes a negative electrode plate, and the negative electrode plate includes a negative electrode active material.

[0021] In any embodiment of the present application, the secondary battery also satisfies: (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of first solvent × 0.03) ≥ 1. At this time, the additive can effectively protect the negative electrode interface, inhibit the aggravation of the negative electrode interface side reaction caused by the instability of the first solvent, and the capacity retention rate of the secondary battery during use is higher and the volume expansion rate is lower. The liquid retention coefficient refers to the ratio of the mass of the electrolyte to the rated capacity of the secondary battery, measured in g / Ah; the content of the additive refers to the mass percentage of the additive based on the total mass of the electrolyte; the relative mass of the negative electrode refers to the ratio of the mass of the negative electrode active material in the negative electrode sheet to the rated capacity of the secondary battery, measured in g / Ah; the specific surface area of ​​the negative electrode active material is measured in m 2 / g.

[0022] Optionally, the secondary battery further satisfies: (liquid retention coefficient×content of additive) / (negative electrode relative mass×specific surface area of ​​negative electrode active material×0.012+liquid retention coefficient×content of first solvent×0.03)≥2.

[0023] In any embodiment of the present application, the thickness of the positive electrode film layer is ≥ 0.07 mm. Optionally, the thickness of the positive electrode film layer is 0.07 mm-0.14 mm. The thickness of the positive electrode film layer is moderate, the transmission path of active ions in the positive electrode film layer is moderate, and the battery can maintain good dynamic performance without excessively sacrificing the energy density of the battery.

[0024] In any embodiment of the present application, the porosity of the positive electrode film layer is ≤50%. Optionally, the porosity of the positive electrode film layer is 5%-50%. The porosity of the positive electrode film layer is moderate, the transmission resistance of active ions in the positive electrode film layer is moderate, and the battery can maintain good dynamic performance without excessively sacrificing the energy density of the battery.

[0025] In any embodiment of the present application, the negative electrode relative mass is ≤2.1 g / Ah. Optionally, the negative electrode relative mass is 1.2 g / Ah-2.1 g / Ah.

[0026] In any embodiment of the present application, the specific surface area of ​​the negative electrode active material is 0.5 m 2 / g-6.0m 2 / g. Optionally, the specific surface area of ​​the negative electrode active material is 1.0m 2 / g-3.2m 2 / g.

[0027] In any embodiment of the present application, the content of the first solvent is ≥ 10%. Optionally, the content of the first solvent is 10%-80%. The moderate content of the first solvent can fully exert the effect of improving the battery kinetics performance on the one hand, and avoid excessive damage to the negative electrode interface on the other hand.

[0028] In any embodiment of the present application, the content of the additive is ≥ 3%. Optionally, the content of the additive is 3%-9%. The moderate content of the additive can fully play the protective effect on the negative electrode interface on the one hand, and on the other hand, it can avoid the formation of an excessively thick SEI film on the surface of the negative electrode active material, thereby increasing the negative electrode film formation impedance.

[0029] In any embodiment of the present application, in Formula 1, R 11 and R 12 Each of R is independently selected from the group consisting of methyl, ethyl, propyl, butyl, fluoromethyl, fluoroethyl, fluoropropyl and fluorobutyl. 11 and R 12 When selected from the above groups, the viscosity of the electrolyte can be maintained within an appropriate range and the electrolyte has a higher conductivity.

[0030] In any embodiment of the present application, the first solvent represented by Formula 1 is selected from one or more of the following compounds:

[0031]

[0032] In any embodiment of the present application, the organic solvent further comprises one or more of the second solvent shown in Formula 2 and the third solvent shown in Formula 3. In Formula 2, R 21 is one of H, methyl, and ethyl. In formula 3, R=, R 32 Each is independently one of methyl, ethyl and propyl.

[0033]

[0034] In any embodiment of the present application, based on the total mass of the organic solvent, the mass percentage of the second solvent is ≥10%. Optionally, the mass percentage of the second solvent is 10%-80%. The second solvent has a high dielectric constant, which is conducive to the dissociation of the lithium salt. Adding the second solvent to the electrolyte is conducive to increasing the conductivity of the electrolyte.

[0035] In any embodiment of the present application, based on the total mass of the organic solvent, the mass percentage of the third solvent is ≥ 0%. Optionally, the mass percentage of the third solvent is 5%-80%. The third solvent has a small dielectric constant and a weak ability to dissociate lithium salts, but has a small viscosity and good fluidity. After adding the third solvent to the electrolyte, the conductivity of the electrolyte can be increased by increasing the migration rate of active ions.

[0036] In any embodiment of the present application, the second solvent represented by Formula 2 is selected from one or two of the following compounds:

[0037]

[0038] In any embodiment of the present application, the third solvent represented by Formula 3 is selected from one or more of the following compounds:

[0039]

[0040] In any embodiment of the present application, the olivine-structured lithium-containing phosphate includes one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.

[0041] A second aspect of the present application provides a battery module, which includes the secondary battery of the first aspect of the present application.

[0042] A third aspect of the present application provides a battery pack, which includes the secondary battery of the first aspect of the present application and one of the battery modules of the second aspect of the present application.

[0043] A fourth aspect of the present application provides a device comprising at least one of the secondary battery of the first aspect of the present application, the battery module of the second aspect of the present application, and the battery pack of the third aspect of the present application.

[0044] The battery module, battery pack and electric device of the present application include the secondary battery provided by the present application, and thus have at least the same advantages as the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0046] Figure 1 It is a schematic diagram of one embodiment of the secondary battery of the present application.

[0047] Figure 2 It is an exploded schematic diagram of one embodiment of the secondary battery of the present application.

[0048] Figure 3 It is a schematic diagram of an embodiment of a battery module of the present application.

[0049] Figure 4 It is a schematic diagram of an embodiment of the battery pack of the present application.

[0050] Figure 5 yes Figure 4 Exploded diagram of .

[0051] Figure 6 It is a schematic diagram of an embodiment of an electric device using the secondary battery of the present application as a power source. DETAILED DESCRIPTION

[0052] Below, the secondary battery of the present application and the battery module, battery pack and electric device containing the secondary battery are described in detail with appropriate reference to the accompanying drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0053] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0054] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0055] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0056] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0057] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0058] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0059] Secondary battery

[0060] Secondary batteries, also known as rechargeable batteries or storage batteries, refer to batteries that can continue to be used by recharging the active materials after the battery is discharged.

[0061] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, and at the same time allow active ions to pass through. The electrolyte plays the role of conducting active ions between the positive electrode sheet and the negative electrode sheet.

[0062] In the secondary battery of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0063] In the secondary battery of the present application, the positive electrode film layer includes a positive electrode active material. As an example, the positive electrode active material may include one or more of a lithium transition metal oxide, a lithium-containing phosphate with an olivine structure, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds. These positive electrode active materials may be used alone or in combination of two or more.

[0064] In some embodiments, the positive electrode active material may include at least one or more of an olivine-structured lithium-containing phosphate and a modified compound thereof.

[0065] In some embodiments, the positive electrode active material may be only one or more of olivine-structured lithium-containing phosphates and modified compounds thereof.

[0066] In the secondary battery of the present application, the modified compound of each positive electrode active material may be a compound that performs doping modification, surface coating modification, or doping and surface coating modification on the positive electrode active material.

[0067] In the secondary battery of the present application, the positive electrode film layer generally comprises a positive electrode active material and an optional binder and an optional conductive agent. The positive electrode film layer is generally formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is generally formed by dispersing the positive electrode active material, the optional conductive agent, the optional binder and any other components in a solvent and stirring evenly. The solvent may be N-methylpyrrolidone (NMP), but is not limited thereto. As an example, the binder for the positive electrode film layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. As an example, the conductive agent for the positive electrode film layer may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0068] In the secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may be selected from one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0069] In the secondary battery of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0070] The negative electrode active material may be a negative electrode active material for a secondary battery known in the art. As an example, the negative electrode active material may include one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloy materials. Tin-based materials may include one or more of elemental tin, tin oxide, and tin alloy materials. The present application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials for secondary batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0071] In the secondary battery of the present application, the negative electrode film layer generally comprises a negative electrode active material, an optional binder, an optional conductive agent and other optional additives. The negative electrode film layer is generally formed by coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing. The negative electrode slurry coating is generally formed by dispersing the negative electrode active material, the optional conductive agent, the optional binder, and other optional additives in a solvent and stirring evenly. The solvent may be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto. As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. As an example, the binder may include styrene-butadiene rubber (SBR), a water-soluble unsaturated resin SR-1B, an aqueous acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). Other optional additives may include thickeners (eg, sodium carboxymethyl cellulose CMC-Na), PTC thermistor materials, and the like.

[0072] In the secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may be selected from one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may be selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0073] In the field of batteries, the electrolyte can be selected from at least one of a solid electrolyte, a gel electrolyte, and a liquid electrolyte (ie, an electrolyte). The secondary battery of the present application uses a liquid electrolyte, ie, an electrolyte.

[0074] In the secondary battery of the present application, the electrolyte may include an organic solvent and an optional additive. The organic solvent of the present application is a non-aqueous organic solvent, and the organic solvent may include a first solvent as shown in Formula 1.

[0075]

[0076] In formula 1, R 11 and R 12 are independently C1-C4 alkyl or C1-C4 halogenated alkyl, R 11 and R 12 The alkyl and haloalkyl substituents may be straight-chain or branched. The number of halogen atoms in the haloalkyl substituent may be one or more; when the haloalkyl substituent contains multiple halogen atoms, these halogen atoms may be the same or different.

[0077] Generally, the high energy density of the battery and good kinetic performance cannot be taken into account at the same time. Increasing the coating weight and compaction density of the positive electrode film layer can improve the energy density of the battery, but at the same time it will lead to poor battery kinetic performance. Adding the first solvent shown in Formula 1 to the electrolyte can improve the kinetic performance of the electrolyte and the kinetic performance of the battery. This is because the first solvent shown in Formula 1 has the advantages of low viscosity and high dielectric constant, which can greatly improve the conductivity of the electrolyte.

[0078] Generally speaking, the higher the electrolyte content in the battery, the better the battery performance. However, the inventors found that when the positive electrode plate includes an olivine-structured lithium-containing phosphate and its modified compound, within a certain range, the electrolyte injection amount increases, the electrolyte wettability inside the battery improves, and the battery's dynamic performance also improves; but continuing to increase the electrolyte injection amount has little effect on improving the battery's dynamic performance; and continuing to increase the electrolyte injection amount will also increase the content of organic solvents inside the battery, and some organic solvents will consume active ions, resulting in accelerated battery capacity decay and increased battery gas production.

[0079] The inventors also found that in a battery with lithium-containing phosphates and modified compounds of olivine structure as positive electrode active materials, when the mass of the first solvent / rated capacity of the secondary battery is ≥ 0.7 g / Ah and the mass of the electrolyte / rated capacity of the secondary battery is ≤ 3.5 g / Ah, the battery can maintain high energy density while having good kinetic performance, high capacity retention rate and low volume expansion rate. The possible reason is that the energy density of the battery with lithium-containing phosphates and modified compounds of olivine structure as positive electrode active materials is low. In order to further improve the energy density of the battery, an effective way is to improve the internal space utilization of the battery, for example, to increase the coating weight and compaction density of the pole piece. At this time, the residual space inside the battery becomes very small. When the content of the electrolyte increases, the gas production inside the battery is also easy to increase. Therefore, batteries with lithium-containing phosphates and modified compounds of olivine structure as positive electrode active materials are more sensitive to the content of the electrolyte. At the same time, in order to improve the kinetic performance of the electrolyte and the kinetic performance of the battery, the electrolyte often uses the above-mentioned first solvent. However, the first solvent has poor oxidation resistance and is easily oxidized and decomposed, resulting in increased gas production inside the battery. Therefore, for batteries that mainly use olivine-structured lithium-containing phosphates and their modified compounds as positive electrode active materials, the content of the electrolyte and the first solvent inside must be strictly controlled.

[0080] After extensive research, the inventors found that when the battery meets the conditions that the mass of the first solvent / rated capacity of the secondary battery is ≥ 0.7 g / Ah and the mass of the electrolyte / rated capacity of the secondary battery is ≤ 3.5 g / Ah, the electrolyte inside the battery can well infiltrate the positive electrode and the negative electrode, giving full play to the improvement of the battery kinetic performance by the first solvent, and the irreversible consumption of active ions inside the battery can also be controlled within a small range. Therefore, the secondary battery can have good kinetic performance, high capacity retention rate and low volume expansion rate while maintaining high energy density.

[0081] “Battery mainly using olivine-structured lithium-containing phosphates and their modified compounds as positive electrode active materials” means that the positive electrode active materials may be only olivine-structured lithium-containing phosphates and their modified compounds, or the positive electrode active materials may be a combination of olivine-structured lithium-containing phosphates and their modified compounds and other positive electrode active materials, that is, the positive electrode active materials include other positive electrode active materials, such as lithium transition metal oxides and their modified compounds, in addition to olivine-structured lithium-containing phosphates and their modified compounds. In some embodiments, based on the total mass of the positive electrode active materials, the mass percentage of olivine-structured lithium-containing phosphates and their modified compounds is ≥50%. Optionally, the mass percentage of olivine-structured lithium-containing phosphates and their modified compounds is 80%-100%.

[0082] In the secondary battery of the present application, the quality of the electrolyte refers to the quality of the electrolyte inside the finished battery, rather than the quality of the electrolyte injected during the battery preparation process.

[0083] In the secondary battery of the present application, the rated capacity of the secondary battery refers to the capacity released when a fully charged battery is discharged at a current of 1 / 3×I1(A) at room temperature and reaches the termination voltage, where I1 represents the 1-hour rate discharge current. For details, please refer to the national standard GB / T 31484-2015 Cycle performance requirements and test methods for power batteries for electric vehicles.

[0084] In the secondary battery of the present application, the ratio of the mass of the electrolyte to the rated capacity of the secondary battery may also be referred to as the electrolyte retention coefficient.

[0085] In some embodiments, the mass of the first solvent / rated capacity of the secondary battery may be ≥0.7 g / Ah, >0.8 g / Ah, ≥0.9 g / Ah, ≥1.0 g / Ah, ≥1.1 g / Ah, ≥1.2 g / Ah, ≥1.3 g / Ah, ≥1.4 g / Ah, ≥1.5 g / Ah, ≥1.6 g / Ah, ≥1.7 g / Ah, ≥1.8 g / Ah, or ≥1.9 g / Ah.

[0086] In some embodiments, the mass of the first solvent per rated capacity of the secondary battery may be 0.7 g / Ah-2.0 g / Ah, 0.8 g / Ah-2.0 g / Ah, 0.9 g / Ah-2.0 g / Ah, 1.0 g / Ah-2.0 g / Ah, 1.1 g / Ah-2.0 g / Ah, 1.2 g / Ah-2.0 g / Ah, 1.5 g / Ah-2.0 g / Ah, 0.7 g / Ah-1.9 g / Ah, 0.8 g / Ah-1.9 g / Ah, 0.9 g / Ah-1. 9g / Ah, 1.0g / Ah-1.9g / Ah, 1.1g / Ah-1.9g / Ah, 1.2g / Ah-1.9g / Ah, 1.5g / Ah-1.9g / Ah, 0.7g / Ah-1.6g / Ah, 0.8g / Ah-1.6g / Ah, 0.9g / Ah-1.6g / Ah, 1.0g / Ah-1.6g / Ah, 1.1g / Ah-1.6g / Ah, 1.2g / Ah-1.6g / Ah, or 1.5g / Ah-1.6g / Ah.

[0087] In some embodiments, the mass of the electrolyte / rated capacity of the secondary battery may be ≤3.5 g / Ah, ≤3.4 g / Ah, ≤3.3 g / Ah, ≤3.2 g / Ah, ≤3.1 g / Ah, ≤3.0 g / Ah, ≤2.9 g / Ah, ≤2.8 g / Ah, ≤2.7 g / Ah, ≤2.6 g / Ah, ≤2.5 g / Ah, ≤2.4 g / Ah, ≤2.3 g / Ah, ≤2.2 g / Ah, ≤2.1 g / Ah, or ≤2.0 g / Ah.

[0088] In some embodiments, the mass of the electrolyte / rated capacity of the secondary battery may be 2.4 g / Ah-3.5 g / Ah, 2.5 g / Ah-3.5 g / Ah, 2.6 g / Ah-3.5 g / Ah, 2.7 g / Ah-3.5 g / Ah, 2.8 g / Ah-3.5 g / Ah, 2.9 g / Ah-3.5 g / Ah, 3.0 g / Ah-3.5 g / Ah, 3.1 g / Ah-3.5g / Ah, 2.4g / Ah-3.3g / Ah, 2.5g / Ah-3.3g / Ah, 2.6g / Ah-3.3g / Ah, 2.7g / Ah-3. 3g / Ah, 2.8g / Ah-3.3g / Ah, 2.9g / Ah-3.3g / Ah, 3.0g / Ah-3.3g / Ah, or 3.1g / Ah-3.3g / Ah.

[0089] In some embodiments, in Formula 1, R 11 and R 12 can be independently selected from the group consisting of methyl, ethyl, propyl, butyl, fluoromethyl, fluoroethyl, fluoropropyl, and fluorobutyl, R 11 and R 12 The number of fluorine atoms can be one or more. 11 and R 12 When selected from the above groups, the viscosity of the electrolyte can be maintained within an appropriate range and the electrolyte has a higher conductivity.

[0090] In some embodiments, as an example, the first solvent shown in Formula 1 can be selected from one or more of the following compounds:

[0091]

[0092] The first solvent shown in Formula 1 has the advantages of low viscosity and high dielectric constant, which can improve the conductivity of the electrolyte, and thus improve the problem of poor battery kinetic performance caused by the increase in the coating weight and compaction density of the positive electrode film layer to a certain extent. However, the inventors also found that the first solvent shown in Formula 1 is unstable at the negative electrode and is easily reduced to generate protons and other products, increasing the gas production of the battery. The protons generated by the reduction of the first solvent shown in Formula 1 will also decompose components such as lithium carbonate and alkoxy lithium in the SEI membrane, making the stability of the SEI membrane worse; in this way, the SEI membrane needs to be continuously repaired during the use of the battery. This repair process will consume more active ions, increase the irreversible consumption of active ions, and cause the battery capacity to decay rapidly. In addition, the product after the reduction of the first solvent shown in Formula 1 accumulates on the surface of the negative electrode active material, which will also extend the transmission path of the active ions and reduce the transmission speed of the active ions, thereby deteriorating the kinetic performance of the negative electrode sheet and the kinetic performance of the battery.

[0093] The inventors have discovered solutions to the above problems through extensive research work, which not only ensures high energy density and good kinetic performance of the battery, but also ensures that the battery has good cycle performance and storage performance.

[0094] In order to improve the energy density of the battery, the coating weight and compaction density of the positive electrode film layer are usually increased. One problem brought about by this is that the positive electrode film layer has an increasing demand for the kinetic performance of the electrolyte. The thicker the positive electrode film layer, the longer the transmission path of the active ions, and the higher the demand for the kinetic performance of the electrolyte; the smaller the porosity of the positive electrode film layer, the greater the resistance in the transmission process of the active ions, and the higher the demand for the kinetic performance of the electrolyte. Therefore, the above two parameters of the positive electrode film layer are independent of each other, and both have certain requirements for the kinetic performance of the electrolyte. The inventor obtained the coefficients of these two independent requirements through a large number of studies and experiments, and used the sum of the two to represent the total demand for the kinetic performance of the electrolyte. The content of the first solvent is strongly correlated with the kinetic performance of the electrolyte. The higher the content of the first solvent, the better the kinetic performance of the electrolyte. The inventor found that the content of the first solvent can be used to characterize the kinetic performance level of the electrolyte. And only when the kinetic performance level of the electrolyte is ≥ the total demand of the positive electrode film layer for the kinetic performance of the electrolyte, can the problem of poor battery kinetic performance caused by the increase in the coating weight and compaction density of the positive electrode film layer be effectively improved.

[0095] Through extensive research, the inventors found that when the secondary battery also satisfies: the content of the first solvent / (thickness of the positive electrode film layer×3+0.008 / porosity of the positive electrode film layer)≥1, the problem of poor battery kinetic performance caused by the increase in the coating weight and compaction density of the positive electrode film layer can be effectively solved.

[0096] In some embodiments, the secondary battery may satisfy: the content of the first solvent / (the thickness of the positive electrode film layer × 3 + 0.008 / the porosity of the positive electrode film layer) ≥ 1.1, the content of the first solvent / (the thickness of the positive electrode film layer × 3 + 0.008 / the porosity of the positive electrode film layer) ≥ 1.2, the content of the first solvent / (the thickness of the positive electrode film layer × 3 + 0.008 / the porosity of the positive electrode film layer) ≥ 1.3, the content of the first solvent / (the thickness of the positive electrode film layer × 3 + 0.008 / the porosity of the positive electrode film layer) porosity) ≥ 1.4, content of the first solvent / (thickness of the positive electrode film layer × 3 + 0.008 / porosity of the positive electrode film layer) ≥ 1.5, content of the first solvent / (thickness of the positive electrode film layer × 3 + 0.008 / porosity of the positive electrode film layer) ≥ 1.6, content of the first solvent / (thickness of the positive electrode film layer × 3 + 0.008 / porosity of the positive electrode film layer) ≥ 1.7, or content of the first solvent / (thickness of the positive electrode film layer × 3 + 0.008 / porosity of the positive electrode film layer) ≥ 1.8.

[0097] The content of the first solvent refers to the mass percentage of the first solvent based on the total mass of the organic solvent.

[0098] The thickness of the positive electrode film layer represents the thickness of the single-sided positive electrode film layer on the positive electrode current collector in mm. When the positive electrode film layer is arranged on any one of the two opposite surfaces of the positive electrode current collector, the thickness of the positive electrode film layer = the thickness of the positive electrode pole piece - the thickness of the positive electrode current collector; when the positive electrode film layer is arranged on two opposite surfaces of the positive electrode current collector at the same time, the thickness of the positive electrode film layer = (the thickness of the positive electrode pole piece - the thickness of the positive electrode current collector) / 2. In the present application, the thickness can be measured using a micrometer, for example, a micrometer with a model of Mitutoyo293-100 and an accuracy of 0.1μm can be used. In the present application, the "thickness of the positive electrode film layer" refers to the thickness of the single-sided positive electrode film layer, and the "total thickness of the positive electrode film layer" means the sum of the thicknesses of each positive electrode film layer when the positive electrode film layer is arranged on two opposite surfaces of the positive electrode current collector at the same time.

[0099] The porosity of the positive electrode film layer is expressed as the ratio of the pore volume of the positive electrode sheet (i.e., the true volume of the positive electrode sheet) to the apparent volume of the positive electrode sheet. The porosity of the positive electrode film layer can be tested with reference to GB / T24586-2009 Determination of apparent density, true density and porosity of iron ore. The test method includes the following steps: 30 small discs with a diameter of 14 mm are cut from the positive electrode sheet, and based on the principle of gas adsorption, an inert gas (e.g., helium or nitrogen) is used as a medium to test the true volume of the 30 small discs with a diameter of 14 mm; the apparent volume of the positive electrode sheet is calculated based on the area, thickness and number of the small discs, and the ratio of the true volume to the apparent volume is the porosity of the positive electrode film layer.

[0100] The surfaces of lithium-containing phosphates with olivine structure and their modified compounds contain polar functional groups and have a large specific surface area, making them very easy to absorb water. However, the drying process before battery filling cannot completely remove the moisture therein. During the use of the battery, this part of the moisture will gradually diffuse into the electrolyte and react with the electrolyte. At the same time, the presence of moisture will also destroy the SEI film (Solid Electrolyte Interface Membrane) on the surface of the negative electrode active material, affecting the stability of the negative electrode interface.

[0101] The thickness of the positive electrode film layer decreases, the transmission path of active ions therein becomes shorter, and the kinetic performance of the secondary battery becomes better; at the same time, the moisture in the positive electrode film layer is easier to remove in the drying process, and the degree of damage to the negative interface by moisture becomes smaller. However, as the thickness of the positive electrode film layer decreases, the energy density of the secondary battery will also decrease. In some embodiments, the thickness of the positive electrode film layer may be ≥0.07mm. For example, the thickness of the positive electrode film layer may be ≥0.075mm, ≥0.08mm, ≥0.085mm, ≥0.09mm, ≥0.10mm, ≥0.11mm, ≥0.12mm, ≥0.13mm, ≥0.14mm, or ≥0.15mm.

[0102] In some embodiments, optionally, the thickness of the positive electrode film layer may be 0.07 mm-0.14 mm. More specifically, the thickness of the positive electrode film layer may be 0.09 mm-0.12 mm.

[0103] The porosity of the positive electrode film layer increases, the electrolyte is easier to infiltrate the positive electrode film layer, the transmission resistance of active ions in the positive electrode film layer becomes smaller, and the kinetic performance of the secondary battery becomes better; at the same time, the moisture in the positive electrode film layer is easier to remove in the drying process, and the degree of damage to the negative electrode interface by moisture becomes smaller. However, as the porosity of the positive electrode film layer increases, the energy density of the secondary battery will decrease. In some embodiments, the porosity of the positive electrode film layer may be ≤50%. For example, the porosity of the positive electrode film layer may be ≤48%, ≤45%, ≤42%, ≤40%, ≤38%, ≤37%, ≤35%, ≤32%, or ≤30%.

[0104] In some embodiments, optionally, the porosity of the positive electrode film layer may be 5%-50%. More specifically, the porosity of the positive electrode film layer may be 20%-40%.

[0105] In some embodiments, the single-sided coating weight of the positive electrode film layer may be ≥20 mg / cm 2 Optionally, the single-sided coating weight of the positive electrode film layer may be 23 mg / cm 2 -29mg / cm 2 More specifically, the single-sided coating weight of the positive electrode film layer may be 25 mg / cm 2 -29mg / cm2 .

[0106] In some embodiments, the compaction density of the positive electrode film layer may be ≥2.1 g / cm 3 Optionally, the compaction density of the positive electrode film layer may be 2.1 g / cm 3 -2.8g / cm 3 More specifically, the compaction density of the positive electrode film layer may be 2.3 g / cm 3 -2.6g / cm 3 .

[0107] In some embodiments, based on the total mass of the organic solvent, the mass percentage of the first solvent (i.e., the content of the first solvent) may be ≥10%. For example, the content of the first solvent may be ≥15%, ≥20%, ≥25%, ≥30%, ≥35%, ≥40%, ≥45%, ≥50%, ≥55%, or ≥60%.

[0108] In some embodiments, the content of the first solvent may be 10%-80%, 15%-80%, 20%-80%, 25%-80%, 30%-80%, 35%-80%, 40%-80%, 45%-80%, 50%-80%, 10%-75%, 15%-75%, 20%-75%, 25%-75%, 30%-75%, 35%-75%, 40%-75%, 45%-75%, 50%-75%, 10%-70%, 1 5%-70%, 20%-70%, 25%-70%, 30%-70%, 35%-70%, 40%-70%, 45%-70%, 50%-70%, 10%-65%, 15%-65%, 20%-65%, 25%-65%, 30%-65%, 35%-65%, 40%-65%, 45%-65%, 50%-65%, 1 0%-60%, 15%-60%, 20%-60%, 25%-60%, 30%-60%, 35%-60%, 40%-60%, 45%-60%, 50%-60%, 10%-55%, 15%-55%, 20%-55%, 25%-55%, 30%-55%, 35%-55%, 40%-55%, 45%-55%, or 50%-55%.

[0109] In some embodiments, the organic solvent may further include one or more of the second solvent shown in Formula 2 and the third solvent shown in Formula 3. In Formula 2, R 21 is one of H, methyl, and ethyl; in Formula 3, R 31 , R 32 are independently one of methyl, ethyl and propyl, R 31 and R 32Can be the same or different.

[0110]

[0111] In the secondary battery of the present application, the organic solvent may include, in addition to the first solvent shown in Formula 1, a second solvent shown in Formula 2, or a third solvent shown in Formula 3, or may include both the second solvent shown in Formula 2 and the third solvent shown in Formula 3. In some embodiments, the organic solvent may include, in addition to the first solvent shown in Formula 1, a second solvent shown in Formula 2.

[0112]

[0113] In some embodiments, as an example, the second solvent shown in Formula 2 can be selected from one or two of the following compounds:

[0114]

[0115] In some embodiments, as an example, the third solvent shown in Formula 3 can be selected from one or more of the following compounds:

[0116]

[0117] The second solvent has a high dielectric constant, which is conducive to the dissociation of the lithium salt. In some embodiments, based on the total mass of the organic solvent, the mass percentage of the second solvent may be ≥10%. Optionally, the mass percentage of the second solvent may be 10%-80%. More specifically, the mass percentage of the second solvent may be 20%-50%.

[0118] The third solvent has a smaller dielectric constant and a weaker ability to dissociate lithium salts, but has a lower viscosity and better fluidity, which can increase the migration rate of active ions. In some embodiments, based on the total mass of the organic solvent, the mass percentage of the third solvent may be ≥ 0%. Optionally, the mass percentage of the third solvent may be 5%-80%. More specifically, the mass percentage of the third solvent may be 5%-20%.

[0119] In the secondary battery of the present application, the electrolyte may further include an additive, and the additive may be a film-forming additive. In some embodiments, the reduction potential of the additive may satisfy ≥0.8V (vs Li + / Li).

[0120] The SEI film on the surface of the negative electrode active material is insulated from electrons, while allowing active ions to freely enter and exit, and can also prevent the negative electrode active material from further reacting with the electrolyte. Therefore, the properties of the SEI film on the surface of the negative electrode active material will affect the performance of the negative electrode sheet and the performance of the battery, such as the cycle performance and storage performance of the battery. The reduction potential of the additive of the present application is ≥0.8V (vs Li + / Li), can participate in the formation of SEI film on the surface of negative electrode active material by electrochemical reduction reaction in priority to organic solvent, and promote the formation of stable SEI film on the surface of negative electrode active material, prevent the negative electrode active material from further reacting with electrolyte, and reduce the degree of damage to SEI film by protons generated by reduction of the first solvent.

[0121] In some embodiments, the additive may include one or more of an organic additive and an inorganic additive.

[0122] In the secondary battery of the present application, the additive may also include only organic additives.

[0123] In some embodiments, as an example, the organic additive may include one or more of vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VEC), ethylene sulfate (DTD), and 1,3-propane sultone (PS). The organic additive is an electrochemical reduction additive, and its reduction potential is higher than that of the organic solvent. Therefore, it can be electrochemically reduced on the surface of the negative electrode active material to form an SEI film with excellent performance, thereby reducing the degree of damage to the SEI film by the protons generated by the reduction of the first solvent. The reduction products of the organic additive are mainly organic components, which can improve the mechanical stability of the SEI film, thereby helping to improve the cycle performance of the battery.

[0124] In some embodiments, as an example, the inorganic additive may include one or more of tris(trimethylsilyl)phosphate (TMSP), lithium bis(oxalate)borate (LiBOB), lithium bis[ethanedioato(2-)-KO1,κO2]difluorophosphate(1-), LiDFOP, lithium tetrafluorooxalatophosphate (LiTFOP), lithium difluorooxalatoborate (LiDFOB), and lithium difluorophosphate (LiPO2F2). The inorganic additive is an electrochemical reduction additive, and its reduction potential is higher than that of the organic solvent. Therefore, it can be preferentially electrochemically reduced on the surface of the negative electrode active material to form an SEI film with excellent performance, thereby reducing the degree of damage to the SEI film by the protons generated by the reduction of the first solvent. The reduction products of inorganic additives are mainly inorganic components, which can improve the thermal stability of the SEI film, thereby helping to improve the high-temperature performance of the battery.

[0125] In some embodiments, optionally, the additive includes one or more of vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, lithium difluorophosphate, and tris(trimethylsilyl)phosphate. Among them, the reduction products of vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, and vinyl sulfate can be used as organic components in the SEI film to improve the mechanical stability of the SEI film and the tolerance of the SEI film to the volume change of the negative electrode active material during the battery cycle. The reduction products of lithium difluorophosphate and tris(trimethylsilyl)phosphate can be used as inorganic components in the SEI film to improve the thermal stability of the SEI film, so that the SEI film is not easy to decompose even in a high temperature environment.

[0126] In some embodiments, the mass percentage of the organic additive may be ≥50% based on the total mass of the additive. For example, the mass percentage of the organic additive may be ≥55%, ≥60%, ≥65%, ≥70%, ≥75%, ≥80%, ≥85%, ≥90%, ≥95%, or 100%.

[0127] In some embodiments, the mass percentage of the organic additive may be 50%-100%, 55%-100%, 60%-100%, 65%-100%, 70%-100%, 75%-100%, 80%-100%, 85%-100%, 90%-100%, or 95%-100%.

[0128] In some embodiments, the mass percentage of the inorganic additive may be ≤50% based on the total mass of the additive. For example, the mass percentage of the inorganic additive may be ≤45%, ≤40%, ≤35%, ≤30%, ≤25%, ≤20%, ≤15%, ≤10%, ≤5%, or 0%.

[0129] In some embodiments, the mass percentage of the inorganic additive may be 0%-50%, 0%-45%, 0%-40%, 0%-35%, 0%-30%, 0%-25%, 0%-20%, 0%-15%, 0%-10%, or 0%-5%.

[0130] As the content of the additive increases, the amount of additive available for consumption in the secondary battery formation process increases, the SEI film formed on the surface of the negative electrode active material becomes thicker, and the negative electrode film formation impedance increases; however, the thickening of the SEI film will strengthen the protective effect of the negative electrode active material, improve the stability of the negative electrode interface, and increase the tolerance of the SEI film to the side effects caused by the first solvent. In some embodiments, based on the total mass of the electrolyte, the mass percentage of the additive (i.e., the content of the additive) may be ≥3%. For example, the additive content may be ≥3.5%, ≥4%, ≥4.5%, ≥5%, ≥5.5%, ≥6%, ≥6.5%, ≥7%, ≥7.5%, ≥8%, ≥9%, ≥10%, ≥11%, or ≥12%.

[0131] In the secondary battery of the present application, “the content of the additive” refers to the sum of the content of the organic additive and the content of the inorganic additive.

[0132] In some embodiments, optionally, the content of the additive may be 3%-9%. More specifically, the content of the additive may be 5%-8%.

[0133] The present application has no specific restrictions on the type of lithium salt, which can be selected according to actual needs. In some embodiments, as examples, the lithium salt may include LiPF6, LiBF4, LiAsF6, Li(FSO2)2N, LiCF3SO3, LiClO4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2), wherein x and y are positive integers.

[0134] The smaller the mass percentage of lithium salt (for example, less than 10%), the fewer active ion transfer units inside the battery. When charging at a high rate, the negative electrode potential drops rapidly, and dendrites are easily grown on the surface of the negative electrode, increasing the irreversible consumption of active ions; the continuous growth of dendrites may also pierce the separator, causing internal short circuits between the positive and negative electrodes. The smaller the mass percentage of lithium salt, the more free organic solvent (especially the first solvent) in the electrolyte, which will also make the SEI film on the surface of the negative electrode active material unstable, and the SEI film will be easily decomposed by protons. In some embodiments, based on the total mass of the electrolyte, the mass percentage of the lithium salt may be ≥10%. For example, the mass percentage of the lithium salt may be ≥11%, ≥12%, ≥13%, ≥14%, ≥15%, ≥16%, ≥17%, or ≥18%.

[0135] The conductivity of the electrolyte is affected by the total number of mobile active ions and the migration rate of the active ions. As the mass percentage of the lithium salt increases, the total number of mobile active ions increases, but at the same time the viscosity of the electrolyte also increases, and the migration rate of the active ions slows down. Therefore, there is an optimal value for the mass percentage of the lithium salt. In some embodiments, the mass percentage of the lithium salt may be 10%-20%. Optionally, the mass percentage of the lithium salt may be 12%-17%.

[0136] Additives promote the formation of a stable SEI film on the surface of the negative electrode active material. The larger the specific surface area of ​​the negative electrode active material, the greater the demand for additives; the first solvent will also consume additional additives. After a lot of research and experiments, the inventors obtained the coefficients of the consumption behavior of these two additives, and used the sum of these two consumption behaviors to represent the demand level of additives; and the retention level of additives can be expressed by the liquid retention coefficient × the content of additives. Only when the retention level of additives is ≥ the demand level of additives can a good negative electrode interface be guaranteed, thereby effectively suppressing side reactions at the negative electrode interface.

[0137] The inventors have found through extensive research that when the secondary battery also satisfies the following conditions: (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of first solvent × 0.03) ≥ 1, the additive can effectively protect the negative electrode interface and inhibit the aggravation of the negative electrode interface side reaction caused by the instability of the first solvent. Therefore, the capacity retention rate of the secondary battery during use is higher and the volume expansion rate is lower.

[0138] The electrolyte retention coefficient refers to the ratio of the mass of the electrolyte to the rated capacity of the secondary battery, measured in g / Ah; the content of the additive refers to the mass percentage of the additive based on the total mass of the electrolyte; the negative electrode relative mass refers to the ratio of the mass of the negative electrode active material in the negative electrode sheet to the rated capacity of the secondary battery, measured in g / Ah; the specific surface area of ​​the negative electrode active material is measured in m2 / g.

[0139] In some embodiments, the secondary battery may also satisfy: (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of first solvent × 0.03) ≥ 1.2, (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of first solvent × 0.03) ≥ 1.4, (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of first solvent × 0.03) ≥ 1.6, (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of first solvent × 0.03) ≥ 1.8, (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of first solvent × 0.03) ≥ 1.8 × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of the first solvent × 0.03) ≥ 2, (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of the first solvent × 0.03) ≥ 2.2, (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of the first solvent × 0.03) ≥ 2.4, (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of the first solvent × 0.03) ≥ 2.8, or (liquid retention coefficient × content of additive) / (relative mass of negative electrode × specific surface area of ​​negative electrode active material × 0.012 + liquid retention coefficient × content of the first solvent × 0.03) ≥ 3.2.

[0140] In some embodiments, the negative electrode relative mass may be ≤2.1 g / Ah. For example, the negative electrode relative mass may be ≤2.08 g / Ah, ≤2.05 g / Ah, ≤2.0 g / Ah, ≤1.95 g / Ah, ≤1.9 g / Ah, ≤1.85 g / Ah, ≤1.8 g / Ah, ≤1.75 g / Ah, ≤1.7 g / Ah, ≤1.65 g / Ah, ≤1.6 g / Ah, ≤1.55 g / Ah, or ≤1.5 g / Ah.

[0141] In some embodiments, optionally, the negative electrode relative mass may be 1.2 g / Ah-2.1 g / Ah. More specifically, the negative electrode relative mass may be 1.5 g / Ah-1.8 g / Ah.

[0142] In the secondary battery of the present application, the specific surface area of ​​the negative electrode active material may be 0.5 m 2 / g-6.0m 2 / g. For example, the specific surface area of ​​the negative electrode active material may be 1.0 m 2 / g-5.0m 2 / g,1.0m 2 / g-4.0m 2 / g,1.0m 2 / g-3.2m 2 / g,1.0m 2 / g-2.8m 2 / g, 1.2m 2 / g-5.0m 2 / g, 1.2m 2 / g-4.0m 2 / g, 1.2m 2 / g-3.0m 2 / g, 1.2m 2 / g-2.8m 2 / g, 1.5m 2 / g-5.0m 2 / g, 1.5m 2 / g-4.0m 2 / g, 1.5m 2 / g-3.0m 2 / g, 2.0m 2 / g-5.0m 2 / g, 2.0m 2 / g-4.0m 2 / g, or 2.0m 2 / g-3.0m 2 / g.

[0143] The secondary battery of the present application also includes an isolation membrane. The isolation membrane is arranged between the positive electrode plate and the negative electrode plate to play an isolation role. The present application has no particular restrictions on the type of isolation membrane, and any known porous structure isolation membrane with good chemical stability and mechanical stability can be selected. In some embodiments, the material of the isolation membrane can be selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different. In some embodiments, a ceramic coating or a metal oxide coating can also be provided on the isolation membrane.

[0144] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0145] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0146] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0147] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.

[0148] In some embodiments, reference Figure 2 , the outer package may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are enclosed to form a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to needs.

[0149] In some embodiments, secondary batteries may be assembled into a battery module. The battery module may contain multiple secondary batteries, and the specific number may be adjusted according to the application and capacity of the battery module.

[0150] Figure 3 4 is an example of a battery module. Figure 3 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0151] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0152] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0153] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and Figure 5The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3, wherein the upper box body 2 is used to cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0154] Method for preparing secondary battery

[0155] In some embodiments, the method for preparing a secondary battery of the present application may include the following steps:

[0156] S10, assembling a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte to form a secondary battery;

[0157] S20, testing the secondary batteries, and selecting the secondary batteries that meet the conditions of mass of the first solvent / rated capacity of the secondary battery ≥ 0.7 g / Ah and mass of the electrolyte / rated capacity of the secondary battery ≤ 3.5 g / Ah.

[0158] The secondary batteries obtained by the method of the present application can have good kinetic performance, high capacity retention rate and low volume expansion rate while maintaining high energy density.

[0159] In some embodiments, in step S10, as an example, the positive electrode sheet, the isolation membrane, and the negative electrode sheet can be formed into an electrode assembly through a winding process or a stacking process, the electrode assembly is placed in an outer package, and the electrolyte is injected after drying. After vacuum packaging, standing, forming, shaping and other processes, a secondary battery is obtained.

[0160] In some embodiments, in step S20, optionally, secondary batteries satisfying the following condition: mass of the first solvent / rated capacity of the secondary battery ≥ 1.0 g / Ah are screened out.

[0161] In some embodiments, in step S20, optionally, secondary batteries that meet the requirement of electrolyte mass / rated capacity of secondary battery of 2.8 g / Ah-3.3 g / Ah are screened out.

[0162] In some embodiments, the preparation method further comprises the step: S30, screening out secondary batteries that satisfy the content of the first solvent / (thickness of the positive electrode film layer×3+0.008 / porosity of the positive electrode film layer)≥1. At this time, not only is the high energy density and good kinetic performance of the battery guaranteed, but also a good negative electrode interface is guaranteed, so that the battery of the present application can have good cycle performance and storage performance.

[0163] In some embodiments, the preparation method further includes the step: S40, screening out secondary batteries that satisfy the following conditions: content of the first solvent / (thickness of the positive electrode film layer×3+0.008 / porosity of the positive electrode film layer)≥1 and (liquid retention coefficient×content of additive) / (relative mass of negative electrode×specific surface area of ​​negative electrode active material×0.012+liquid retention coefficient×content of the first solvent×0.03)≥1. At this point, the problems of poor battery kinetics performance caused by increased coating weight and compaction density of the positive electrode film layer and negative electrode interface damage caused by the first solvent can be effectively solved.

[0164] Electrical devices

[0165] The present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack of the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0166] The electrical device may select a secondary battery, a battery module or a battery pack according to its usage requirements.

[0167] Figure 6 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the power consumption device for high power and high energy density, a battery pack or a battery module can be used.

[0168] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a secondary battery may be used as a power source.

[0169] Example

[0170] The following examples more specifically describe the disclosure of the present application, which are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations are possible within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0171] Example 1

[0172] Preparation of positive electrode

[0173] The positive electrode active material lithium iron phosphate, the binder polyvinylidene fluoride, and the conductive agent acetylene black are mixed in a mass ratio of 96:2:2, and then the solvent N-methylpyrrolidone (NMP) is added to adjust the viscosity, and the positive electrode slurry is fully stirred according to the method known in the art; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained after drying and cold pressing. Among them, the porosity of the positive electrode film layer is 30%, and the thickness of the positive electrode film layer is 0.1mm.

[0174] Preparation of negative electrode

[0175] The negative electrode active material graphite (specific surface area 2m 2 / g), conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are mixed in a mass ratio of 97:1:1:1, and then solvent deionized water is added, and the mixture is fully stirred into a negative electrode slurry according to a method known in the art; the negative electrode slurry is evenly coated on the negative electrode collector copper foil, and the negative electrode sheet is obtained after drying and cold pressing.

[0176] Preparation of electrolyte

[0177] In an argon atmosphere glove box with a water content of less than 10ppm, the first solvent compound 1-1, the second solvent compound 2-1, and the third solvent compound 3-1 are uniformly mixed in a mass ratio of 50:30:20 to obtain an organic solvent; 15% by mass of lithium hexafluorophosphate (LiPF6) is slowly added as a lithium salt and stirred until it is completely dissolved; after the mixed solution returns to room temperature, 3% of vinylene carbonate (VC), 2% of fluoroethylene carbonate (FEC), 0.5% of 1,3-propane sultone (PS), and 0.5% of lithium difluorobis(oxalate) phosphate (LiDFOP) are added in sequence to obtain an electrolyte.

[0178] Preparation of isolation membrane

[0179] A polyethylene (PE) film coated with nano-aluminum oxide was used as the separator.

[0180] Preparation of secondary batteries

[0181] The positive electrode sheet, the separator, and the negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is added to the outer packaging aluminum plastic film, and the electrolyte is injected after drying, and the secondary battery is obtained through the processes of packaging, standing, formation, aging, secondary packaging, and capacity. The rated capacity of the first solvent / secondary battery is 1.6g / Ah, the liquid retention coefficient of the secondary battery is 3.1g / Ah, and the relative mass of the negative electrode is 1.7g / Ah.

[0182] Examples 2 to 30 and Comparative Examples 1 to 8

[0183] The preparation methods of Examples 2 to 30 and Comparative Examples 1 to 8 are similar to those of Example 1, except that the relevant parameters in the preparation of the positive electrode sheet, the negative electrode sheet and the electrolyte are adjusted. The specific parameters are detailed in Tables 1 and 2.

[0184]

[0185]

[0186] Table 2

[0187]

[0188] Test Section

[0189] (1) Initial DC internal resistance (DCR) test

[0190] At room temperature, the battery is charged to 3.65V at 0.5C constant current, and then charged to 0.05C at constant voltage; the battery is discharged at 0.5C constant current for 30 minutes to adjust the battery to 50% SOC, at which time the battery voltage is recorded as U1; the battery is discharged at 4C constant current for 30 seconds, with 0.1 second sampling, and the voltage at the end of discharge is recorded as U2. The discharge DCR of the battery at 50% SOC represents the initial DCR of the battery, and the initial DCR of the battery = (U1-U2) / 4C.

[0191] (2) 60℃ Cyclic Performance Test

[0192] At 60°C, charge the battery at a constant current of 0.5C to 3.65V, and then charge at a constant voltage to a current of 0.05C; let the battery stand for 5 minutes, and discharge it at a constant current of 1 / 3C to 2.5V; this is the first charge and discharge cycle of the battery, and the discharge capacity of this time is recorded as the discharge capacity of the first cycle of the battery. Perform 1000 cycles of charge and discharge on the battery according to the above method, and record the discharge capacity of the battery after 1000 cycles. The capacity retention rate (%) of the battery after 1000 cycles at 60°C = (discharge capacity of the battery after 1000 cycles / discharge capacity of the first cycle of the battery) × 100%.

[0193] (3) 60℃ volume expansion test

[0194] At 60°C, the battery is charged to 3.65V at a constant current of 0.5C, and then charged to a current of 0.05C at a constant voltage. At this time, the volume of the battery is tested by the water displacement method and recorded as V0; the battery is placed in a 60°C constant temperature box, and after storage for 30 days, it is taken out and the volume of the battery is tested by the water displacement method and recorded as V1. The volume expansion rate of the battery after storage at 60°C for 30 days = [(V1-V0) / V0]×100%.

[0195] The specific parameters of Examples 1-30 and Comparative Examples 1-8 are shown in Tables 1 and 2, and the test results are shown in Table 3.

[0196] In Table 3, Formula I = content of the first solvent / (thickness of the positive electrode film layer × 3 + 0.008 / porosity of the positive electrode film layer), Formula II = (liquid retention coefficient × content of additive) / (relative mass of the negative electrode × specific surface area of ​​the negative electrode active material × 0.012 + liquid retention coefficient × content of the first solvent × 0.03).

[0197] Table 3

[0198]

[0199] By comparing Examples 1-30 and Comparative Examples 1-8, it can be found that only when the battery simultaneously satisfies the mass of the first solvent / rated capacity of the secondary battery ≥ 0.7 g / Ah and the mass of the electrolyte / rated capacity of the secondary battery ≤ 3.5 g / Ah, the secondary battery can have a lower initial DCR, a higher high-temperature cycle capacity retention rate, and a lower high-temperature storage volume expansion rate while maintaining a high energy density. When the mass of the first solvent / rated capacity of the secondary battery does not meet ≥ 0.7 g / Ah, the content of the first solvent inside the battery is too small, and the kinetic performance of the battery cannot be effectively improved, and the initial DCR of the battery is high. When the mass of the electrolyte / rated capacity of the secondary battery does not meet ≤ 3.5 g / Ah, part of the organic solvent in the electrolyte will continue to consume active ions, and the irreversible consumption of active ions will continue to increase. The battery cannot simultaneously have a lower initial DCR, a higher high-temperature cycle capacity retention rate, and a lower high-temperature storage volume expansion rate.

[0200] By comparing Examples 1-7, it can be found that the initial DCR of the battery is low, the high-temperature cycle capacity retention rate is high, and the high-temperature storage volume expansion rate is low. In addition, the above-mentioned performance of the battery will vary slightly depending on the type of the first solvent in the electrolyte, which is due to the characteristics of the different first solvents themselves. Among these first solvents, compound 1-1 has the lowest viscosity and the highest dielectric constant, so the initial DCR of the prepared battery is also the lowest. However, among these first solvents, compound 1-1 has the worst stability at the negative electrode, and is more likely to destroy the stability of the negative electrode interface, causing continuous film formation on the surface of the negative electrode active material, and the most irreversible consumption of lithium ions; the products generated by the reduction and decomposition of compound 1-1 at the negative electrode are accumulated at the negative electrode interface, and the lithium ion transmission path is extended and the lithium ion transmission rate is slowed down; therefore, in Examples 1-7, the negative electrode interface condition of Example 1 is the worst, the battery high-temperature cycle capacity decays the fastest, and the battery high-temperature storage volume expansion rate is the largest.

[0201] By comparing Examples 8-9, it can be found that the lower the content of the first solvent, the smaller the degree of damage to the negative electrode interface, the higher the high-temperature cycle capacity retention rate of the battery, and the smaller the high-temperature storage volume expansion rate. However, at the same time, the lower the content of the first solvent, the weaker the improvement in the kinetic performance of the battery, and the larger the initial DCR of the battery.

[0202] By comparing Examples 10-11, it can be found that the thickness of the positive electrode film layer is reduced, the initial DCR of the battery is reduced, the high-temperature cycle capacity retention rate is increased, and the high-temperature storage volume expansion rate is reduced. This is mainly because, after the thickness of the positive electrode film layer is reduced, the transmission path of lithium ions in it becomes shorter, the kinetic performance of the battery becomes better, and the initial DCR is reduced. The surface of the lithium-containing phosphate with an olivine structure used in the positive electrode film layer contains polar functional groups and has a large specific surface area, which is very easy to absorb water, and the drying process before the battery is injected cannot completely remove the moisture in the positive electrode film layer. During the use of the battery, the moisture in the positive electrode film layer will gradually diffuse into the electrolyte and react with the electrolyte; at the same time, the presence of moisture will also destroy the SEI film on the surface of the negative electrode active material, affecting the stability of the negative electrode interface. Therefore, when the thickness of the positive electrode film layer is reduced, the moisture in the positive electrode film layer is easier to remove in the drying process, and the degree of damage to the negative interface by moisture is reduced, thereby slowing down the high-temperature cycle capacity decay of the battery and reducing the gas production of high-temperature storage.

[0203] By comparing Examples 12-13, it can be found that the porosity of the positive electrode film layer increases, the initial DCR of the battery decreases, the high-temperature cycle capacity retention rate increases, and the high-temperature storage volume expansion rate decreases. After the porosity of the positive electrode film layer increases, the electrolyte is easier to infiltrate the positive electrode film layer, and the transmission resistance of lithium ions in the positive electrode film layer decreases. Therefore, the kinetic performance of the battery improves and the initial DCR decreases. After the porosity of the positive electrode film layer increases, the moisture in the positive electrode film layer is easier to remove in the drying process, and the degree of damage to the negative electrode interface by moisture is reduced. Therefore, the high-temperature cycle capacity of the battery decays slower and the high-temperature storage gas production is reduced.

[0204] By comparing Examples 16-17, it can be found that increasing the content of additives increases the initial DCR of the battery, increases the high-temperature cycle capacity retention rate, and decreases the high-temperature storage volume expansion rate. This is mainly because, after the content of additives in the battery increases, the amount of additives consumed in the formation process increases, the SEI film formed on the surface of the negative electrode active material is thicker, and the negative electrode film formation impedance increases, so the initial DCR of the battery increases. Correspondingly, after the content of additives in the battery increases, the SEI film has a stronger protective effect on the negative electrode active material, the negative electrode interface stability is better, and the tolerance to the side effects caused by the first solvent is also higher. Therefore, the high-temperature cycle capacity of the battery decays slower and the high-temperature storage gas production is reduced.

[0205] By comparing Examples 18-21, it can be found that by reducing the relative mass of the negative electrode and the specific surface area of ​​the negative electrode active material, the initial DCR of the battery increases, the high-temperature cycle capacity retention rate increases, and the high-temperature storage volume expansion rate decreases. This is mainly because, after the relative mass of the negative electrode in the battery is reduced and the specific surface area of ​​the negative electrode active material is reduced, the amount of additives required to form the SEI film on the surface of the negative electrode active material is reduced, and the battery's demand for additives will be greatly reduced, and the number of additives inside the battery will be more sufficient. Therefore, the battery's high-temperature cycle capacity decay slows down and the high-temperature storage gas production decreases. The reduction in the battery's demand for additives will also cause the internal additives of the battery to be excessive. When the SEI film is formed on the surface of the negative electrode active material during the formation process, the amount of additives available for consumption increases, and the SEI film formed is thicker. Therefore, the initial DCR of the battery will increase.

[0206] By comparing Examples 22-25, it can be found that the level of electrolyte kinetic performance can meet the total demand of the positive electrode film layer for electrolyte kinetic performance, and the initial DCR of the battery is not large. However, when certain parameters change, the retention level of the additive is less than the required level of the additive, the additive does not fully protect the negative electrode interface, and the first solvent reacts side effects at the negative electrode interface, which consumes a certain number of lithium ions. Therefore, the high-temperature cycle capacity decay of the battery will become faster. The first solvent will also destroy the SEI film on the surface of the negative electrode active material, so that the SEI film needs to be continuously repaired during the use of the battery. A certain amount of gas will be generated during the repair of the SEI film. Therefore, the high-temperature storage volume expansion rate of the battery will increase.

[0207] After the specific surface area of ​​the negative electrode active material increases, the amount of additives required to form the SEI film on the surface of the negative electrode active material increases. Since the total amount of additives is constant, the SEI film formed on the surface of the negative electrode active material will become relatively thinner, so the initial DCR of the battery will decrease. However, in Example 22, due to the increase in the specific surface area of ​​the negative electrode active material, the retention level of the additive is less than the required level of the additive, and the additive cannot fully form the SEI film on the surface of the negative electrode active material and cannot fully protect the negative electrode interface. Therefore, the high-temperature cycle capacity decay of the battery becomes significantly faster and the high-temperature storage volume expansion rate becomes significantly larger.

[0208] After the content of the additive is reduced, the number of additives that can participate in forming the SEI film on the surface of the negative electrode active material is relatively reduced, and the negative electrode film formation impedance becomes lower, so the initial DCR of the battery is also reduced. However, in Example 23, due to the reduction in the content of the additive, the retention level of the additive is less than the required level of the additive, and the additive cannot fully form the SEI film on the surface of the negative electrode active material and cannot fully protect the negative electrode interface. Therefore, the high-temperature cycle capacity decay of the battery becomes significantly faster and the high-temperature storage volume expansion rate becomes significantly larger.

[0209] After the battery liquid retention coefficient is reduced, the number of additives that can participate in the formation of SEI film on the surface of the negative electrode active material is relatively reduced, and the negative electrode film formation impedance becomes lower, so the initial DCR of the battery is also reduced. However, in Example 24, due to the reduction of the liquid retention coefficient, the retention level of the additive is less than the required level of the additive. At this time, the additive can no longer fully protect the negative electrode interface. Therefore, the high-temperature cycle capacity decay of the battery becomes significantly faster and the high-temperature storage volume expansion rate becomes significantly larger.

[0210] After the relative mass of the negative electrode increases, the SEI film formed on the surface of the negative electrode active material will become relatively thinner due to the constant total amount of additives, so the initial DCR of the battery will decrease. However, in Example 25, due to the increase in the relative mass of the negative electrode, the retention level of the additive is less than the required level of the additive, and the additive cannot fully form an SEI film on the surface of the negative electrode active material and cannot fully protect the negative electrode interface. Therefore, the high-temperature cycle capacity decay of the battery becomes significantly faster and the high-temperature storage volume expansion rate becomes significantly larger.

[0211] By comparing Examples 26-28, it can be found that when the retention level of the additive is greater than the required level of the additive, even if the electrolyte contains the first solvent, the negative electrode interface can still be effectively protected, so the battery still has a high high-temperature cycle capacity retention rate and a low high-temperature storage volume expansion rate. However, when certain parameters change so that the electrolyte kinetic performance level does not meet the total requirement of the positive electrode film layer for the electrolyte kinetic performance, the initial DCR of the battery will increase significantly.

[0212] In Example 26, due to the reduction in the content of the first solvent, the kinetic performance level of the electrolyte cannot meet the total requirement of the positive electrode film layer for the kinetic performance of the electrolyte, and the kinetic performance of the electrolyte and the battery cannot be effectively improved, and the initial DCR of the battery will increase significantly.

[0213] The thickness of the positive electrode film layer increases, and the energy density of the battery increases. However, in Example 27, due to the increase in the thickness of the positive electrode film layer, the electrolyte kinetic performance level cannot meet the total demand of the positive electrode film layer for the electrolyte kinetic performance, and the transmission path of lithium ions in the positive electrode film layer becomes longer, and the initial DCR of the battery will increase significantly.

[0214] The porosity of the positive electrode film layer decreases, and the energy density of the battery increases. However, in Example 28, due to the decrease in the porosity of the positive electrode film layer, the electrolyte kinetic performance level cannot meet the total demand of the positive electrode film layer for the electrolyte kinetic performance, and the electrolyte is difficult to infiltrate the positive electrode film layer, and the transmission resistance of lithium ions in the positive electrode film layer becomes larger. Therefore, the initial DCR of the battery will increase significantly.

[0215] By comparing Examples 29-30, it can be found that the initial DCR of the battery is high, the high-temperature cycle capacity retention rate is low, and the high-temperature storage volume expansion rate is high. This is mainly because, on the one hand, the thickness of the positive electrode film layer increases, the porosity decreases, the electrolyte is difficult to infiltrate the positive electrode film layer, the lithium ion transmission path becomes longer, the transmission resistance becomes larger, and the electrolyte kinetic performance level cannot meet the total demand of the positive electrode film layer for the electrolyte kinetic performance. Therefore, the initial DCR of the battery is high; on the other hand, the content of the electrolyte additive is low, so that the retention level of the additive is less than the required level of the additive, and the additive cannot fully protect the negative electrode interface. Therefore, the high-temperature cycle capacity of the battery decays faster and the high-temperature storage gas production increases.

[0216] By comparing Examples 14-15, it can also be found that as the mass percentage of lithium salt increases, the initial DCR of the battery first decreases and then increases, which is mainly due to changes in the conductivity of the electrolyte. The conductivity of the electrolyte is affected by the total number of mobile lithium ions and the migration rate of lithium ions. As the mass percentage of lithium salt increases, the total number of mobile lithium ions increases, but at the same time, the viscosity of the electrolyte also increases, and the migration rate of lithium ions slows down. Therefore, the mass percentage of lithium salt will have an optimal value, at which time the initial DCR of the battery is the lowest. The higher the mass percentage of lithium salt, the less free organic solvent content in the electrolyte, and the less content of the first solvent that undergoes side reactions at the negative electrode interface. Therefore, the high-temperature cycle capacity of the battery decays slower and the high-temperature storage gas production decreases.

[0217] From the data in Table 3, it can be seen that the battery of Example 1-22 satisfies the mass of the first solvent / rated capacity of the secondary battery ≥ 0.7g / Ah and the mass of the electrolyte / rated capacity of the secondary battery ≤ 3.5g / Ah while also satisfying Formula I and Formula II, and the battery can simultaneously have a lower initial DCR, a higher high-temperature cycle capacity retention rate, and a lower high-temperature storage volume expansion rate. On the one hand, the electrolyte kinetic performance level can meet the total demand of the positive electrode film layer for the battery kinetic performance, so the battery has a lower initial DCR; on the other hand, the electrolyte additive can effectively protect the negative electrode interface and inhibit the aggravation of the negative electrode interface side reaction caused by the instability of the first solvent. Therefore, the high-temperature cycle capacity of the battery decays slower and the high-temperature storage gas production is reduced.

[0218] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A secondary battery comprising a positive electrode plate and an electrolyte; The positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes one or more of an olivine-structured lithium-containing phosphate and modified compounds thereof; The electrolyte includes an organic solvent, and the organic solvent includes a first solvent shown in Formula 1; In formula 1, R 11 is one of hydrogen, C1-C4 alkyl, and C1-C4 halogenated alkyl, R 12 It is one of C1-C4 alkyl and C1-C4 halogenated alkyl; Based on the mass of the electrolyte, the mass percentage of the first solvent is greater than or equal to 20%; And the secondary battery satisfies: The mass of the electrolyte / rated capacity of the secondary battery is less than or equal to 3.6 g / Ah.

2. The secondary battery according to claim 1, wherein Based on the mass of the electrolyte, the mass percentage of the first solvent is 20%-83.3%.

3. The secondary battery according to claim 1, wherein Based on the mass of the electrolyte, the mass percentage of the first solvent is 21.2%-61.3%.

4. The secondary battery according to claim 1, wherein The mass of the electrolyte / rated capacity of the secondary battery is 2.4 g / Ah-3.6 g / Ah.

5. The secondary battery according to claim 1, wherein The mass of the electrolyte / rated capacity of the secondary battery is 2.4 g / Ah-3.5 g / Ah.

6. The secondary battery according to claim 1, wherein The mass of the electrolyte / rated capacity of the secondary battery is 2.9 g / Ah-3.3 g / Ah.

7. The secondary battery according to any one of claims 1 to 6, wherein The secondary battery also satisfies: the content of the first solvent / (thickness of the positive electrode film layer×3+0.008 / porosity of the positive electrode film layer)≥1, The content of the first solvent refers to the mass percentage of the first solvent based on the total mass of the organic solvent. The thickness of the positive electrode film layer refers to the thickness of the single-sided positive electrode film layer on the positive electrode current collector in mm.

8. The secondary battery according to claim 7, wherein The content of the first solvent / (thickness of the positive electrode film layer×3+0.008 / porosity of the positive electrode film layer)=1-1.

84.

9. The secondary battery according to any one of claims 1 to 6, wherein The electrolyte also includes an additive, the reduction potential of the additive is ≥0.8V (vs Li + / Li).

10. The secondary battery according to claim 9, wherein The content of the additive is ≥3%, and the content of the additive refers to the mass percentage of the additive based on the total mass of the electrolyte.

11. The secondary battery according to claim 10, wherein The content of the additive is 3% to 9%.

12. The secondary battery according to claim 9, wherein The additives include organic additives, and the organic additives include one or more of vinylene carbonate, fluoroethylene carbonate, vinyl carbonate, vinyl sulfate, and 1,3-propane sultone.

13. The secondary battery according to claim 12, wherein: The organic additive includes vinylene carbonate, fluoroethylene carbonate, and at least one selected from vinyl carbonate, vinyl sulfate, and 1,3-propane sultone.

14. The secondary battery according to claim 12 or 13, wherein: The additives also include inorganic additives, and the additive-free additives include one or more of tris(trimethylsilyl)phosphate, lithium bis(oxalatoborate), lithium difluorobis(oxalatophosphate), lithium tetrafluorooxalatophosphate, and lithium difluorooxalatoborate.

15. The secondary battery according to claim 14, wherein Based on the total mass of the additives, the mass percentage of the organic additive is ≥50%.

16. The secondary battery according to claim 14, wherein Based on the total mass of the additives, the mass percentage of the organic additive is ≥70%.

17. The secondary battery according to claim 14, wherein Based on the total mass of the additives, the mass percentage of the organic additive is 83.3%-94.4%.

18. The secondary battery according to claim 14, wherein Based on the total mass of the additives, the mass percentage of the inorganic additive is ≤50%.

19. The secondary battery according to claim 14, wherein The mass percentage of the inorganic additive is ≤30% based on the total mass of the additive.

20. The secondary battery according to claim 14, wherein Based on the total mass of the additives, the mass percentage of the inorganic additives is 5.6%-16.7%.

21. The secondary battery according to claim 1, wherein The secondary battery further comprises a negative electrode plate, the negative electrode plate comprises a negative electrode active material, and the secondary battery further satisfies: (liquid retention coefficient×content of additive) / (negative electrode relative mass×specific surface area of ​​negative electrode active material×0.012+liquid retention coefficient×content of first solvent×0.03)≥1, The electrolyte retention coefficient refers to the ratio of the mass of the electrolyte to the rated capacity of the secondary battery, measured in g / Ah; The content of additives refers to the mass percentage of additives based on the total mass of the electrolyte; The negative electrode relative mass refers to the ratio of the mass of the negative electrode active material in the negative electrode sheet to the rated capacity of the secondary battery, measured in g / Ah; The specific surface area of ​​the negative electrode active material is expressed in m 2 / g.

22. The secondary battery according to claim 21, wherein (liquid retention coefficient×content of additive) / (negative electrode relative mass×specific surface area of ​​negative electrode active material×0.012+liquid retention coefficient×content of first solvent×0.03)=2-3.

27.

23. The secondary battery according to claim 1, wherein The thickness of the positive electrode film layer is ≥ 0.07 mm; and / or The porosity of the positive electrode film layer is ≤50%.

24. The secondary battery according to claim 23, wherein The thickness of the positive electrode film layer is 0.07mm-0.14mm.

25. The secondary battery according to claim 23, wherein The thickness of the positive electrode film layer is 0.07mm-0.12mm.

26. The secondary battery according to claim 1, wherein The porosity of the positive electrode film layer is 5%-50%.

27. The secondary battery according to claim 21, wherein Negative electrode relative mass ≤ 2.1g / Ah; and / or, The specific surface area of ​​the negative electrode active material is 0.5 m 2 / g-6.0m 2 / g; and / or, Based on the total mass of the electrolyte, the content of the additive is ≥2.5%.

28. The secondary battery according to claim 27, wherein The relative mass of the negative electrode is 1.2g / Ah-1.9g / Ah; and / or, The specific surface area of ​​the negative electrode active material is 1.5 m 2 / g-2.8m 2 / g; and / or, Based on the total mass of the electrolyte, the content of the additive is 2.5%-9%.

29. The secondary battery according to claim 1, wherein In formula 1, R 11 is one of hydrogen, methyl, ethyl, propyl, butyl, fluoromethyl, fluoroethyl, fluoropropyl and fluorobutyl, R 12 It is one of methyl, ethyl, propyl, butyl, fluoromethyl, fluoroethyl, fluoropropyl and fluorobutyl.

30. The secondary battery according to claim 1, wherein The first solvent shown in Formula 1 is selected from one or more of the following compounds:

31. The secondary battery according to claim 1, wherein In formula 1, R 11 is one of hydrogen, methyl, ethyl, propyl and butyl, R 12 It is one of methyl, ethyl, propyl and butyl.

32. The secondary battery according to claim 1, wherein The organic solvent further comprises one or more of the second solvent shown in Formula 2 and the third solvent shown in Formula 3. In Formula 2, R 21 is one of H, methyl and ethyl. In Formula 3, R 31 , R 32 Each is independently one of methyl, ethyl and propyl; 33. The secondary battery according to claim 32, wherein: The second solvent shown in Formula 2 is selected from one or two of the following compounds:

34. The secondary battery according to claim 32, wherein: The third solvent shown in Formula 3 is selected from one or more of the following compounds:

35. The secondary battery according to claim 32, wherein The organic solvent includes compound 2-1, compound 3-1 and one of the following compounds 1-1 to 1-8:

36. The secondary battery according to claim 32, wherein: Based on the total mass of the organic solvent, the mass percentage of the second solvent is ≥ 10%; and / or, Based on the total mass of the organic solvent, the mass percentage of the third solvent is ≥ 0%.

37. The secondary battery according to claim 36, wherein: Based on the total mass of the organic solvent, the mass percentage of the second solvent is 10% to 80%; and / or, Based on the total mass of the organic solvent, the mass percentage of the third solvent is 5% to 80%.

38. The secondary battery according to claim 37, wherein Based on the total mass of the organic solvent, the mass percentage of the second solvent is 20% to 50%; and / or, based on the total mass of the organic solvent, the mass percentage of the third solvent is 5% to 20%.

39. The secondary battery according to claim 1, wherein The lithium-containing phosphate with olivine structure includes one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.

40. The secondary battery according to any one of claims 1 to 6, wherein The single-sided coating weight of the positive electrode film layer is 23 mg / cm 2 ~29mg / cm 2 , and / or, The compaction density of the positive electrode film layer is 2.1 g / cm 3 ~2.8g / cm 3 .

41. The secondary battery according to claim 40, wherein The single-sided coating weight of the positive electrode film layer is 25 mg / cm 2 ~29mg / cm 2 , and / or, The compaction density of the positive electrode film layer is 2.3 g / cm 3 ~2.6g / cm 3 .

42. A battery module comprising the secondary battery according to any one of claims 1 to 41.

43. A battery pack comprising the secondary battery according to any one of claims 1 to 41 and the battery module according to claim 42.

44. An electrical device comprising at least one of the secondary battery according to any one of claims 1 to 41, the battery module according to claim 42, and the battery pack according to claim 43.

Citation Information

Patent Citations

  • Electrolyte and lithium ion battery

    CN111864261A

  • Nonaqueous electrolyte secondary cell and method for charging same

    CN1783548A

  • Additive for non-aqueous liquid electrolyte, non-aqueous liquid electrolyte, and lithium secondary battery comprising the same

    KR1020150050149A

  • Electrolyte solution, secondary battery containing electrolyte solution and preparation method therefor

    WO2017190355A1