Preparation method of lithium ion battery
By screening and matching the DCR parameters of the positive and negative electrodes, the problems of high R&D costs and long cycles in the design process of lithium-ion batteries have been solved, enabling quantitative control and rapid preparation of battery performance, and improving the cycle life and energy density of the battery.
Patent Information
- Application Number
- CN202410914467.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-15
AI Technical Summary
The design process of existing lithium-ion batteries is characterized by high R&D costs, long development cycles, and easy performance degradation during long-term storage.
By obtaining the actual DCR parameters of the electrodes, positive and negative electrodes are screened and matched, and lithium-ion batteries are assembled according to the relationship 0.56≤x≤0.83, where x is the ratio of the DCR parameters of the positive and negative electrodes. Based on the DCR decomposition theory, multiple electrodes with different actual DCR parameters are designed to achieve quantitative control of the battery's electrochemical performance.
It shortened the R&D cycle, reduced R&D costs, and reduced battery performance degradation by properly matching the positive and negative electrode dynamics, thereby improving the battery's cycle life and energy density.
Smart Images

Figure CN118970194A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion batteries, and in particular to a method for preparing a lithium ion battery. Background Art
[0002] Lithium-ion batteries have become the preferred energy storage solution for electronic devices, electric vehicles, and large-scale energy storage systems due to their high energy density, long cycle life, and relatively stable electrochemical properties. As these applications continue to require higher battery performance, such as higher energy density, longer cycle life, and faster charging capabilities, the requirements for battery design and manufacturing have become more stringent and diverse.
[0003] However, the current design and development process of lithium-ion batteries faces a series of challenges. The main reason is that pre-production battery products often face storage problems, because the battery may degrade during long-term storage, which increases the related maintenance and safety costs. Therefore, in the existing technology, products are usually designed according to demand after obtaining orders. This process involves a lot of experimental optimization and test verification, and it usually takes months or even years to complete the transformation from concept to product, resulting in high R&D costs and long R&D cycles. Summary of the invention
[0004] The embodiment of the present invention provides a method for preparing a lithium ion battery, so as to solve the problems of high R&D cost and long R&D cycle in the design process of the existing lithium ion battery.
[0005] Specifically, the present invention provides a method for preparing a lithium ion battery, comprising the following steps:
[0006] Prepare a plurality of pole pieces, wherein the plurality of pole pieces are classified into positive pole pieces and negative pole pieces;
[0007] Obtaining the actual DCR parameter of each of the pole pieces;
[0008] Screening the positive electrode sheet according to the target DCR parameter of the electrode sheet of the target lithium-ion battery; wherein the actual DCR parameter of the positive electrode sheet is the same as the target DCR parameter of the positive electrode sheet of the target lithium-ion battery;
[0009] The negative electrode sheet is selected to match the screened positive electrode sheet according to the relationship of 0.56≤x≤0.83; wherein x is the ratio of the actual DCR parameter of the positive electrode sheet to the actual DCR parameter of the negative electrode sheet.
[0010] The matched positive electrode sheet, negative electrode sheet and separator are assembled into a lithium ion battery.
[0011] Optional, 0.77≤x≤0.83.
[0012] Optionally, the DCR parameters include one or more of porosity, tortuosity, effective electrochemical area, electrochemical reaction constant, and lithium ion solid phase diffusion coefficient.
[0013] Optionally, the porosity of the actual DCR parameter is calculated by the following formula:
[0014]
[0015] Where ε is the porosity, ρ compressed is the compaction density of the electrode, m electrode is the mass of the electrode, ρ average is the average density of the pole piece, S electrode is the electrode area, L electrode is the thickness of the electrode;
[0016] ratio is the mass ratio of the components in the pole piece, ratio1 is the mass ratio of the first component in the pole piece, and ratio2 is the mass ratio of the second component in the pole piece...ratio n is the mass proportion of the nth component in the electrode;
[0017] ρ is the true density of the components in the pole piece, ρ1 is the true density of the first component in the pole piece, ρ2 is the true density of the second component in the pole piece...ρ n is the true density of the nth component in the electrode.
[0018] Optionally, the tortuosity of the actual DCR parameter is calculated by the following formula:
[0019]
[0020] Among them, τ is the tortuosity, ε is the porosity, and R ion is the ionic internal resistance, Acc is the current collector area, L is the electrode thickness, and K0 is the intrinsic conductivity of the electrolyte.
[0021] Optionally, the tortuosity of the actual DCR parameter is calculated by the following formula:
[0022] τ=γ·ε -α
[0023] Among them, τ is the tortuosity, γ is the correction factor, ε is the porosity, and α is the Bruggeman index.
[0024] Optionally, the electrochemical reaction constant of the actual DCR parameter is calculated by the following formula:
[0025]
[0026]
[0027] Where: k is the electrochemical reaction constant, C s,max is the maximum solid phase concentration of lithium ions in the positive electrode material, C s is the lithium ion solid phase concentration of the positive electrode material at 50% SOC, C e is the lithium ion concentration of the electrolyte, i 0 is the exchange current density of the positive electrode material;
[0028] R is the ideal gas constant, T is the temperature, n is the reaction order, and F is the Faraday constant.
[0029] Optionally, the lithium ion solid phase diffusion coefficient of the actual DCR parameter is calculated by the following formula:
[0030]
[0031] Among them, I p is the peak current; n is the number of electron transfers in the redox process; A is the electrode area immersed in the solution; D is the solid phase diffusion coefficient of lithium ions; ν is the scan rate; C0 is the lithium ion concentration participating in the redox reaction.
[0032] Optionally, the positive electrode sheet includes a positive electrode current collector and a positive electrode membrane provided on the surface of the positive electrode current collector, and the material of the positive electrode membrane includes one or more of lithium cobalt oxide, lithium iron phosphate, spinel lithium manganese oxide, ternary positive electrode material, and lithium manganese-rich positive electrode material;
[0033] The negative electrode sheet includes a negative electrode current collector and a negative electrode material, and the negative electrode material includes a negative electrode active material, a conductive agent, a binder and a solvent; the negative electrode active material includes one or more of a carbon-based negative electrode material, lithium titanate, a silicon-based negative electrode material, a tin-based negative electrode material, and a transition metal oxide negative electrode.
[0034] Optionally, the positive electrode membrane is prepared by the following steps:
[0035] The SWCNT dispersion and lithium cobalt oxide are uniformly mixed in a mass ratio of 1:0.3-0.5, and dispersed into a slurry; the slurry is filtered onto a filter membrane, and the positive electrode membrane is obtained by freeze drying and rolling;
[0036] Based on 100% of the mass of the SWCNT dispersion, the content of the single-walled carbon nanotubes is 0.2-0.6wt%, the content of the carboxymethyl cellulose is 0.4-0.8wt%, and the balance is water.
[0037] The beneficial effects of the present invention are:
[0038] The present invention designs a plurality of positive and negative electrode sheets with different actual DCR parameters based on the DCR decomposition theory. After determining the order requirements and design goals, a strategy is quickly formulated to quickly match the positive and negative electrode sheets and assemble them into batteries. The present invention can achieve quantitative control of the electrochemical performance of the battery, facilitate battery modeling and simulation, and realize digital management of the power supply system at the subsequent application end, thereby shortening the R&D cycle and reducing the R&D cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.
[0040] Figure 1 It is a schematic flow chart of a method for preparing a lithium-ion battery in Embodiment 1 of the present invention. DETAILED DESCRIPTION
[0041] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0042] In the description of the present invention, it should be understood that the terms "longitudinal", "radial", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0043] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0044] Figure 1is a schematic flow chart of a method for preparing a lithium-ion battery in an embodiment of the present invention, such as Figure 1 As shown, an embodiment of the present invention provides a method for preparing a lithium ion battery, comprising the following steps:
[0045] Prepare a plurality of pole pieces, wherein the plurality of pole pieces are classified into positive pole pieces and negative pole pieces;
[0046] Obtaining the actual DCR parameter of each of the pole pieces;
[0047] Screening the positive electrode sheet according to the target DCR parameter of the electrode sheet of the target lithium-ion battery; wherein the actual DCR parameter of the positive electrode sheet is the same as the target DCR parameter of the positive electrode sheet of the target lithium-ion battery;
[0048] Selecting a negative electrode sheet to match the selected positive electrode sheet according to the relationship of 0.56≤x≤0.83; wherein x is the ratio of the actual DCR parameter of the positive electrode sheet to the actual DCR parameter of the negative electrode sheet;
[0049] The matched positive electrode sheet, negative electrode sheet and separator are assembled into a lithium ion battery.
[0050] The actual DCR parameters in the present invention include one or more of porosity, tortuosity, effective electrochemical area, electrochemical reaction constant, and lithium ion solid phase diffusion coefficient. The present invention designs a plurality of positive and negative electrodes with different actual DCR parameters based on the DCR decomposition theory. After determining the order requirements and design goals, a strategy is quickly formulated to quickly match the positive and negative electrodes and assemble them into batteries, which can achieve quantitative control of the electrochemical performance of the battery, facilitate battery modeling and simulation, and realize digital management of the power system at the subsequent application end, thereby shortening the R&D cycle and reducing R&D costs.
[0051] The removal of lithium ions from the positive electrode and the insertion of lithium ions from the negative electrode of lithium-ion batteries will encounter obstacles. The obstacle under DC working conditions is the direct current internal resistance (DCR), which can be decomposed into ohmic internal resistance, electrochemical reaction internal resistance, and diffusion internal resistance according to its components. If the three internal resistances encountered in the removal of lithium ions from the positive electrode and the insertion of lithium ions from the negative electrode are not reasonably matched, the migration speed of lithium ions in the positive and negative electrode regions will be different, that is, the lithium ions removed from the positive electrode migrate to the negative electrode region. In theory, the negative electrode has sufficient capacity to accept the lithium ions that migrate from the positive electrode, but because the kinetics of the positive and negative electrodes are not properly matched, the migration speed of lithium ions is different, which will cause local "blockage" of lithium ions in the negative electrode region. Lithium ions that are not embedded in the crystals of the negative electrode material will still undergo a reduction reaction, resulting in local lithium precipitation. Therefore, due to the mismatch of the kinetics of the positive and negative electrodes, local overcharge and over-discharge of the battery may occur, thereby affecting the cycle life of the battery. However, an overly loose kinetic matching relationship will sacrifice the volume energy density and mass energy density of the battery;
[0052] Based on the above reasons, the present invention does not match the positive and negative electrode capacities according to the CB value, but matches the actual DCR parameters of the positive and negative electrodes according to the relationship of 0.56≤x≤0.83, so as to quantitatively control the kinetics of the battery electrochemical sub-processes, thereby facilitating the kinetic matching of different electrochemical processes of the positive and negative electrodes. While ensuring the energy density, the possibility of battery performance degradation due to local failure and the occurrence of capacity diving are reduced, thereby taking into account both the high energy density and battery life of the battery.
[0053] In one embodiment of the present invention, the negative electrode sheet includes a negative electrode current collector and a negative electrode material, and the negative electrode material includes a negative electrode active substance, a conductive agent, a binder, and a solvent. The active substance includes one or more of a carbon-based negative electrode material, a lithium titanate, a silicon-based negative electrode material, a tin-based negative electrode material, and a transition metal oxide negative electrode. The conductive agent includes one or more of conductive carbon black, Ketjen black, carbon nanotubes, and graphene. The binder includes one or more of polytetrafluoroethylene, carboxymethyl cellulose, and styrene-butadiene rubber. The solvent includes one or more of ethylene glycol, glycerol, polyethylene glycol, dimethyl sulfoxide, N-methylpyrrolidone, deionized water, alcohol, and N-methylpyrrolidone (NMP).
[0054] The positive electrode sheet includes a positive electrode collector and a positive electrode membrane arranged on the surface of the positive electrode collector. The material of the positive electrode membrane includes a positive electrode active material, a conductive agent and a binder; the positive electrode active material includes one or more of lithium cobalt oxide, lithium iron phosphate, spinel lithium manganese oxide, ternary positive electrode material (Li(NiCoMn)O2), and lithium manganese-rich positive electrode material (xLi2MnO3·(1–x)LiTMO2, TM=Ni, Mn, Co, etc.).
[0055] The thickness of the electrode sheet ranges from 1 μm to 50 μm. The negative electrode material is prepared into a plurality of negative electrode sheets by a dry electrode preparation method or a wet electrode preparation method.
[0056] In one embodiment of the present invention, the actual DCR parameter includes one or more of porosity, tortuosity, effective electrochemical area, electrochemical reaction constant, and lithium ion solid phase diffusion coefficient. The porosity of the actual DCR parameter is calculated by the following formula:
[0057]
[0058] Where ε is the porosity, ρ compressed is the compaction density of the electrode, m electrode is the mass of the electrode, ρ average is the average density of the pole piece, S electrode is the electrode area, L electrode is the thickness of the electrode;
[0059] ratio is the mass ratio of the components in the pole piece, ratio1 is the mass ratio of the first component in the pole piece, and ratio2 is the mass ratio of the second component in the pole piece...ratio n is the mass proportion of the nth component in the electrode;
[0060] ρ is the true density of the components in the pole piece, ρ1 is the true density of the first component in the pole piece, ρ2 is the true density of the second component in the pole piece...ρ n is the true density of the nth component in the electrode.
[0061] The tortuosity of the actual DCR parameter is calculated by either of the following two formulas:
[0062]
[0063] τ=γ·ε -α
[0064] Among them, τ is the tortuosity, ε is the porosity, and R ionis the ionic internal resistance, Acc is the current collector area, L is the electrode thickness, and K0 is the intrinsic conductivity of the electrolyte. Among them, τ is the tortuosity, γ is the correction factor, the value range of γ is 1.5~2.0, ε is the porosity, and α is the Bruggeman index.
[0065] When the tortuosity is calculated by combining X-ray tomography / cross-section scanning electron microscopy and simulation, the fitting formula is τ = γ·ε -α When testing the tortuosity experimentally, the formula Moreover, the two formulas can verify each other, and only when the tortuosity measured by the two methods is the same, the tortuosity is used to ensure the accuracy of the calculation.
[0066] The electrochemical reaction constant of the actual DCR parameter is calculated by the following formula:
[0067]
[0068]
[0069] Where: k is the electrochemical reaction constant, C s,max is the maximum solid phase concentration of lithium ions in the positive electrode material, C s is the lithium ion solid phase concentration of the positive electrode material at 50% SOC, C e is the lithium ion concentration of the electrolyte, i 0 is the exchange current density of the positive electrode material; R is the ideal gas constant, T is the temperature, n is the reaction order, and F is the Faraday constant.
[0070] The lithium ion solid phase diffusion coefficient of the actual DCR parameter is calculated by the following formula:
[0071]
[0072] Among them, I p is the peak current; n is the number of electron transfers in the redox process; A is the electrode area immersed in the solution; D is the solid phase diffusion coefficient of lithium ions; ν is the scan rate; C0 is the lithium ion concentration participating in the redox reaction.
[0073] Specifically, the positive electrode film is prepared by the following steps:
[0074] The SWCNT (single-walled carbon nanotube) dispersion and lithium cobalt oxide are mixed uniformly in a mass ratio of 1:0.3-0.5 and dispersed into a slurry. The slurry is filtered onto a filter membrane, and a positive electrode membrane is obtained by freeze drying and rolling. Furthermore, based on the mass of the SWCNT dispersion as 100%, the content of the single-walled carbon nanotube is 0.2-0.6wt%, the content of the carboxymethyl cellulose is 0.4-0.8wt%, and the balance is water.
[0075] The present invention is further described below by way of examples. However, the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0076] Taking the active material of the positive electrode as high voltage 4.48V lithium cobalt oxide (LCO-4.48V) as an example, the specific information of lithium cobalt oxide is shown in Table 1.
[0077] Table 1 Specific information of lithium cobalt oxide
[0078] nature Lithium Cobalt Oxide - 4.48V <![CDATA[Particle size, D 50 (μm)]]> 16 <![CDATA[Specific surface area (cm 2 / g)]]> 0.2432 Specific capacity (mAh / g) 188 Electrochemical window (vs.Li / Li+, V) 3.0-4.48
[0079] (1) Preparation of positive electrode
[0080] 0.4wt% SWCNT was dispersed in water to obtain a SWCNT dispersion, wherein the stabilizer in the SWCNT dispersion was 0.6wt% carboxymethyl cellulose. LCO-4.48V and SWCNT dispersion were mixed in a mass ratio of 0.39:1, dispersed into a slurry using a high-speed shear emulsifier, and deionized water was added to adjust the viscosity to obtain a slurry. The slurry was vacuum filtered onto a water-based filter membrane (mixed cellulose ester membrane, 0.45μm thick) to form an emulsion. The emulsion was then freeze-dried for 24h, and a positive electrode film was formed by rolling, and the positive electrode film was composited on the positive current collector to obtain a positive electrode sheet. The above operation was repeated to prepare positive electrode sheets of different thicknesses. Positive electrode sheets of different thicknesses have different DCR electrochemical parameters. Several positive electrode sheets with a thickness of 82μm were selected for the experiment.
[0081] (2) Preparation of negative electrode sheet
[0082] The negative electrode active material graphite, conductive agent conductive carbon black, binder sodium carboxymethyl cellulose, binder styrene butadiene rubber are fully stirred and mixed in an appropriate amount of deionized water solvent according to a mass ratio of 97.8%: 0.4%: 0.8%: 1.0% to form a uniform negative electrode slurry. Then the negative electrode slurry is coated on the negative electrode current collector copper foil, dried, cold pressed, and rolled to a compaction density of 1.75g / cm 3 , and then the negative electrode sheet is obtained after stripping. Several negative electrode sheets with different thicknesses are selected for experiment.
[0083] (3) Taking the positive electrode sheet as an example, obtain the actual DCR parameters of the positive electrode sheet.
[0084] By assembling a symmetrical battery, the electrochemical impedance spectroscopy (EIS) of the symmetrical battery can be tested, and the ionic internal resistance (R ion ). Then the tortuosity of the electrode is calculated by the following formula (1) or (2). The porosity is calculated by formulas (3), (4), and (5).
[0085] τ=γ·ε -α (1)
[0086]
[0087] Among them, τ is the tortuosity, ε is the porosity, and ρ compressed is the compaction density of the electrode, m electrode is the mass of the electrode, ρ average is the average density of the pole piece, S electrode is the electrode area, L electrode is the thickness of the electrode. ratio is the mass ratio of the components in the electrode; ρ is the true density of the components in the electrode. Among them, active-material is the active material (LCO-4.48V), SWCNT is single-walled carbon nanotube, and CMC is carboxymethyl cellulose.
[0088] When the tortuosity is calculated by combining X-ray tomography / cross-section scanning electron microscopy and simulation, the fitting formula is τ=γ·ε -α When the tortuosity is tested by experimental methods, the formula is used. Moreover, the two formulas can verify each other, and only when the tortuosity measured by the two methods is the same, the tortuosity is used to ensure the accuracy of the calculation.
[0089] Among them, the ionic internal resistance R ion The test method is as follows: ① Test the thickness of the electrode: cut the electrode size to 60×75mm and the solid electrode size to 60×45mm, dry, stack, assemble and inject according to the normal process; ② Let it stand for 12 hours to fully wet the electrode; ③ Put on the glass clamp at 0.07MPa; ④ EIS test: clamp the working electrode and the counter electrode between the two pole ears, the test frequency is 0.1-106Hz, 5mV disturbance. Fixed frequency point: at the characteristic frequency (the inflection point of the 45-degree oblique line is the characteristic frequency), Z1=A, the intersection of the real axis: Z2=0, Z1=B; the ionic impedance is calculated according to the following formula: R ion =3×(AB).
[0090] The relevant data before battery aging is shown in Table 2.
[0091] Table 2 Related parameters of the positive electrode.
[0092] parameter Lithium cobalt oxide <![CDATA[Ionic internal resistance, R ion > 1.315Ω Current collector area, Acc <![CDATA[1.13×10 -4 m 2 ]]> <![CDATA[Intrinsic conductivity of the electrolyte, K0]]> 10.3S / m Pole piece thickness, L <![CDATA[164×10 -6 m]]> Porosity, ε 0.15 Tortuosity, τ 1.40
[0093] Obtaining the key parameters of electrochemical reaction internal resistance:
[0094] By testing the EIS of the positive electrode at different temperatures, the electrochemical reaction impedance R at different temperatures is obtained. ct The exchange current density is obtained according to formula (6), and the electrochemical reaction rate constant is calculated by formula (7). The electrochemical reaction activation energy is calculated by the relationship between the electrochemical reaction rate constant and the temperature in formula (8).
[0095]
[0096] Where: C s,max is the maximum solid phase concentration of lithium ions in lithium cobalt oxide, C s is the lithium ion solid phase concentration of lithium cobalt oxide at 50% SOC, C e is the lithium ion concentration of the electrolyte, i 0 is the exchange current density of lithium cobalt oxide electrode particles, k is the electrochemical reaction constant, E a is the activation energy of the electrochemical reaction, R is the ideal gas constant, T is the temperature, n is the reaction order, F is the Faraday constant, T1 and T2 are arbitrary temperature values, T1≠T2, k1 is the electrochemical reaction constant at T1, and k2 is the electrochemical reaction constant at T2. The specific parameters are shown in Table 3.
[0097] Table 3 Electrochemical reaction related parameters of lithium cobalt oxide (50% SOC)
[0098]
[0099] Obtaining the solid phase diffusion coefficient of lithium ions:
[0100] Based on the Randles-Sevchik equation:
[0101] I p =0.4463zFA(zF / RT) 1 / 2 ΔC0D 1 / 2 v 1 / 2
[0102] At room temperature, there is the following formula:
[0103] I p =2.69×10 5 An 3 / 2 C0D 1 / 2 v 1 / 2
[0104] Among them, I pis the peak current; n is the number of electron transfers in the redox process; A is the electrode area immersed in the solution; D is the diffusion coefficient in the electrode; ν is the scan rate; C0 is the lithium ion concentration participating in the redox reaction.
[0105] The area of the electrode immersed in the solution can generally be considered as its geometric area. The radius of the electrode is 6 mm, and the area of the electrode is 0.000113 m 2 . Since the diffusion of lithium in the electrode material is a very slow process, the scanning rate should be selected below 1mV / s. This experiment selected (0.1mV / s, 0.2mV / s, 0.3mV / s, 0.5mV / s, 0.8mV / s). C0 is the concentration of lithium ions participating in the redox reaction. The corresponding oxidized or reduced charge can be obtained by integrating the corresponding electrode peak. Since it is a single-electron reaction, the charge is the amount of substance of the corresponding lithium ion. Then divide it by the volume of the electrolyte to calculate the concentration of lithium ions participating in the reaction. Plot the peak current at different scanning rates against the square root of the scanning rate. According to Ip-v 1 / 2 The parameters related to the formula are as follows:
[0106] As shown in Table 4.
[0107]
[0108] Table 4 Relevant parameters in the lithium ion diffusion process.
[0109] parameter Lithium cobalt oxide <![CDATA[Ip-v 1 / 2 Slope]]> 0.1463 <![CDATA[Electrode area (m 2 )]]> <![CDATA[1.13×10 -4 ]]> <![CDATA[Lithium ion concentration (mol / m 3 )]]> 16440.3 <![CDATA[Lithium ion solid-phase diffusion coefficient (m 2 / s)]]> <![CDATA[8.57×10 -14 ]]>
[0110] By obtaining the above key electrochemical parameters, the DCR of the lithium cobalt oxide electrode can be calculated. The relevant parameters of the two positive electrode sheets A and B are shown in Table 5:
[0111] Table 5 DCR related parameters of two positive electrode sheets
[0112]
[0113] (4) Test the negative electrode sheet according to the method in step (3).
[0114] The key parameters of the positive electrode and negative electrode are shown in Table 6 below.
[0115] Table 6 Actual DCR parameters of positive and negative electrodes
[0116]
[0117] Different negative electrode sheets are matched and combined with positive electrode sheets with the same parameters to obtain lithium ion batteries of Examples 1-3 and Comparative Examples 1-3. The differences in the matching of actual DCR parameters of the lithium ion batteries of Examples 1-3 and Comparative Example 1 are shown in Table 7.
[0118] Table 7 Matching of DCR parameters of Examples 1-4 and Comparative Example 1
[0119]
[0120]
[0121] The cycle performance of the batteries of Examples 1-3 and the batteries of Comparative Examples 1-3 was tested, and the comparison of the cycle performance is shown in Table 8.
[0122]
[0123] It can be seen from Table 8 that compared with Comparative Example 1, the specific capacity of the battery after multiple cycles after positive and negative electrode DCR matching in Examples 1-3 did not decrease significantly. At the same time, the present invention designs multiple positive and negative electrode sheets with different actual DCR parameters based on the DCR decomposition theory. After determining the order requirements and design goals, a strategy is quickly formulated to quickly match the positive and negative electrode sheets and assemble them into batteries, which can achieve quantitative control of battery electrochemical performance, facilitate battery modeling and simulation, and realize digital management of the power system at the subsequent application end, thereby shortening the R&D cycle and reducing R&D costs.
[0124] Moreover, compared with Comparative Example 1, Examples 1 and 2 show that the cycle performance and coulombic efficiency of the battery with reasonable positive and negative electrode DCR matching are improved. In other words, the battery with reasonable positive and negative electrode DCR matching can improve its cycle performance while shortening the R&D cycle and reducing the R&D cost, thereby obtaining a battery with excellent cycle performance.
[0125] Furthermore, compared with Example 1, Example 3 has a positive electrode DCR much greater than that of the negative electrode, a large amount of active material at the negative electrode, a large amount of SEI film is formed at the negative electrode, a large amount of cyclable lithium is consumed, the capacity of the first 20 cycles decreases more, and the subsequent cycles are relatively stable. Compared with Example 1, Comparative Examples 2 and 3 have a negative electrode DCR much greater than that of the positive electrode DCR, a large amount of active material at the positive electrode, a small capacity decrease in the first 20 cycles, and cyclable lithium is easily precipitated at the negative electrode in the subsequent cycles to form lithium dendrites, forming a micro-short circuit, and causing a sudden decrease in capacity. Therefore, it is shown that not all DCR parameter matching in any proportion does not affect the specific capacity of the battery. Only by following the method provided by the present invention to match the DCR parameters can a battery with excellent cycle performance be obtained.
[0126] The embodiments described above are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.
Claims
1. A method for preparing a lithium ion battery, characterized in that: The following steps are involved: Prepare a plurality of pole pieces, wherein the plurality of pole pieces are classified into positive pole pieces and negative pole pieces; Obtaining the actual DCR parameter of each of the pole pieces; Screening the positive electrode sheet according to the target DCR parameter of the electrode sheet of the target lithium-ion battery; wherein the actual DCR parameter of the positive electrode sheet is the same as the target DCR parameter of the positive electrode sheet of the target lithium-ion battery; Selecting a negative electrode sheet to match the selected positive electrode sheet according to the relationship of 0.56≤x≤0.83; wherein x is the ratio of the actual DCR parameter of the positive electrode sheet to the actual DCR parameter of the negative electrode sheet; The matched positive electrode sheet, negative electrode sheet and separator are assembled into a lithium ion battery.
2. The preparation method according to claim 1, characterized in that: 0.77≤x≤0.83。 3. The preparation method according to claim 1, characterized in that: The DCR parameters include one or more of porosity, tortuosity, effective electrochemical area, electrochemical reaction constant, and lithium ion solid phase diffusion coefficient.
4. The preparation method according to claim 3, characterized in that: The porosity of the actual DCR parameter is calculated by the following formula: Where ε is the porosity, ρ compressed is the compaction density of the electrode, m electrode is the mass of the electrode, ρ average is the average density of the pole piece, S electrode For the polar surface, L electrode is the thickness of the electrode; ratio is the mass ratio of the components in the pole piece, ratio1 is the mass ratio of the first component in the pole piece, and ratio2 is the mass ratio of the second component in the pole piece...ratio n is the mass proportion of the nth component in the electrode; ρ is the true density of the components in the pole piece, ρ1 is the true density of the first component in the pole piece, ρ2 is the true density of the second component in the pole piece...ρ n is the true density of the nth component in the electrode.
5. The preparation method according to claim 4, characterized in that: The tortuosity of the actual DCR parameter is calculated by the following formula: Among them, τ is the tortuosity, ε is the porosity, and R ion is the ionic internal resistance, Acc is the current collector area, L is the electrode thickness, and K0 is the intrinsic conductivity of the electrolyte.
6. The preparation method according to claim 4, characterized in that: The tortuosity of the actual DCR parameter is calculated by the following formula: τ=γ·ε -α Among them, τ is the tortuosity, γ is the correction factor, the value range of γ is 1.5~2.0, ε is the porosity, and α is the Bruggeman index.
7. The preparation method according to claim 3, characterized in that: The electrochemical reaction constant of the actual DCR parameter is calculated by the following formula: Where: k is the electrochemical reaction constant, C s,max is the maximum solid phase concentration of lithium ions, Cs is the solid phase concentration of lithium ions in the positive electrode material at 50% SOC, and C e is the lithium ion concentration of the electrolyte, i 0 is the exchange current density of the positive electrode material, R ct is the electrochemical reaction impedance; R is the ideal gas constant, T is the temperature, n is the reaction order, and F is the Faraday constant.
8. The preparation method according to claim 3, characterized in that: The lithium ion solid phase diffusion coefficient of the actual DCR parameter is calculated by the following formula: Among them, I p is the peak current; n is the number of electron transfers in the redox process; A is the electrode area immersed in the solution; D is the solid phase diffusion coefficient of lithium ions; ν is the scan rate; C0 is the lithium ion concentration participating in the redox reaction.
9. The preparation method according to claim 1, characterized in that: The positive electrode sheet includes a positive electrode current collector and a positive electrode membrane provided on the surface of the positive electrode current collector, wherein the material of the positive electrode membrane includes one or more of lithium cobalt oxide, lithium iron phosphate, spinel lithium manganese oxide, ternary positive electrode material, and lithium manganese-rich positive electrode material; The negative electrode sheet includes a negative electrode current collector and a negative electrode material, and the negative electrode material includes a negative electrode active material, a conductive agent, a binder and a solvent; the negative electrode active material includes one or more of a carbon-based negative electrode material, lithium titanate, a silicon-based negative electrode material, a tin-based negative electrode material, and a transition metal oxide negative electrode.
10. The preparation method according to claim 1, characterized in that: The positive electrode film is prepared by the following steps: The SWCNT dispersion and lithium cobalt oxide are uniformly mixed in a mass ratio of 1:0.3-0.5, and dispersed into a slurry; the slurry is filtered onto a filter membrane, and the positive electrode membrane is obtained by freeze drying and rolling; Based on 100% of the mass of the SWCNT dispersion, the content of the single-walled carbon nanotubes is 0.2-0.6wt%, the content of the carboxymethyl cellulose is 0.4-0.8wt%, and the balance is water.
Citation Information
Cited By
Preparation method of lithium / sodium ion battery failure analysis symmetric battery
CN119780743A