Preparation method of lithium ion battery

Designing controllable sublayer electrodes through DCR decomposition theory solves the problems of high R&D costs and long cycles in the lithium-ion battery design process, and quickly formulates strategies and battery performance control, shortens R&D cycles and reduces costs, while improving The battery's cycle performance and energy density are achieved.

CN118970195AActive Publication Date: 2024-11-15HIGHPOWER TECH HUIZHOU +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410914471.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-15
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

There are problems such as high R&D costs and long R&D cycle during the design and development of existing lithium-ion batteries. This is mainly because the battery may degrade performance during long-term storage, which requires a lot of experimental optimization and test verification, resulting in the need of concept to Product conversion takes months or even years.

Method used

Design the sub-layer electrode with controllable DCR components through DCR decomposition theory, screen and composite electrodes according to the pole sheet parameters of the target lithium-ion battery, quickly formulate strategies, and recombinate multiple sub-layer electrodes into composite electrodes and assemble them into batteries to achieve quantitative control Battery electrochemical performance, simplifying battery modeling and simulation and digital management.

Benefits of technology

The R&D cycle is shortened, the R&D cost is reduced, and the battery performance attenuation and capacity dipping caused by local failure is reduced, achieving the high energy density and long life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970195A_ABST
    Figure CN118970195A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a lithium ion battery. The preparation method comprises the following steps: preparing a plurality of positive sub-layer electrodes and negative sub-layer electrodes; acquiring an actual DCR parameter of each positive electrode sub-layer electrode; according to a target DCR parameter of a pole piece of a target lithium ion battery, screening out at least two positive sub-layer electrodes and compounding the positive sub-layer electrodes into a positive composite electrode; according to the voltage drop of the positive electrode composite electrode, screening out at least two negative electrode sub-layer electrodes and compounding the negative electrode sub-layer electrodes into a negative electrode composite electrode; and assembling the positive composite electrode, a negative composite electrode and a diaphragm into the battery. According to the method, the sub-layer electrodes with controllable DCR components are designed based on the DCR decomposition theory, after order requirements and design targets are determined, a strategy is rapidly formulated, the multiple sub-layer electrodes are compounded into the composite electrode, the composite electrode is assembled into the battery, the electrochemical performance of the battery can be quantitatively controlled, modeling simulation of the battery is easy, and the method is suitable for large-scale popularization and application. And digital management of a power supply system of a subsequent application end is realized, so that the research and development period is shortened and the research and development cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion batteries, and in particular to a method for preparing a lithium ion battery. Background Art

[0002] Lithium-ion batteries have become the preferred energy storage solution for electronic devices, electric vehicles, and large-scale energy storage systems due to their high energy density, long cycle life, and relatively stable electrochemical properties. As these applications continue to require higher battery performance, such as higher energy density, longer cycle life, and faster charging capabilities, the requirements for battery design and manufacturing have become more stringent and diverse.

[0003] However, the current design and development process of lithium-ion batteries faces a series of challenges. The main reason is that pre-production battery products often face storage problems, because the battery may degrade during long-term storage, which increases the related maintenance and safety costs. Therefore, in the existing technology, products are usually designed according to demand after obtaining orders. This process involves a lot of experimental optimization and test verification, and it usually takes months or even years to complete the transformation from concept to product, resulting in high R&D costs and long R&D cycles. Summary of the invention

[0004] The embodiment of the present invention provides a method for preparing a lithium ion battery, so as to solve the problems of high R&D cost and long R&D cycle in the design process of the existing lithium ion battery.

[0005] Specifically, the present invention provides a method for preparing a lithium ion battery, comprising the following steps:

[0006] Prepare a plurality of sub-layer electrodes, wherein the plurality of sub-layer electrodes are classified into positive sub-layer electrodes and negative sub-layer electrodes;

[0007] Obtaining the actual DCR parameter of each of the positive sub-layer electrodes; screening out at least two of the positive sub-layer electrodes according to the target DCR parameter of the electrode sheet of the target lithium-ion battery; combining the screened positive sub-layer electrodes into a positive composite electrode; wherein the actual DCR parameter of the positive composite electrode is the same as the target DCR parameter of the positive electrode sheet of the target lithium-ion battery; screening out at least two of the negative sub-layer electrodes according to the voltage drop of the positive composite electrode; combining the screened negative sub-layer electrodes into a negative composite electrode; or,

[0008] Obtaining the actual DCR parameter of each of the negative sub-layer electrodes; screening out at least two of the negative sub-layer electrodes according to the target DCR parameter of the electrode sheet of the target lithium-ion battery; combining the screened negative sub-layer electrodes into a negative composite electrode; wherein the actual DCR parameter of the negative composite electrode is the same as the target DCR parameter of the negative electrode sheet of the target lithium-ion battery; screening out at least two of the positive sub-layer electrodes according to the voltage drop of the negative composite electrode; combining the screened positive sub-layer electrodes into a negative composite electrode;

[0009] The voltage drop ΔU of the positive composite electrode pos The voltage drop ΔU of the negative electrode composite electrode neg same;

[0010] The positive composite electrode, the negative composite electrode and a separator are assembled into a lithium ion battery.

[0011] Optionally, ΔU neg =I neg1 *R neg1 +I neg2 *R neg2 +...+I negm *R negm ;

[0012] ΔU pos =I pos1 *R pos1 +I pos2 *R pos2 +...+I posn *R posn ;

[0013] Among them, I neg is the current passing through the negative sublayer electrode, I neg1 is the current passing through the first negative electrode sublayer electrode in the negative electrode composite electrode, I neg2 I is the current passing through the second negative electrode sub-layer electrode in the negative electrode composite electrode; negm is the current passing through the mth negative electrode sublayer electrode in the negative composite electrode; R neg is the resistance of the negative sublayer electrode, R neg1 is the resistance of the first negative electrode sub-layer electrode in the negative electrode composite electrode, R neg2 is the resistance of the second negative electrode sub-layer electrode in the negative electrode composite electrode, R negm is the resistance of the mth negative electrode sublayer electrode in the negative composite electrode;

[0014] I pos is the current passing through the positive sublayer electrode, I pos1 I is the current passing through the first positive electrode sub-layer electrode in the positive electrode composite electrode; pos2is the current passing through the second positive electrode layer electrode in the positive electrode composite electrode, I posn is the current passing through the nth positive sub-layer electrode in the positive composite electrode; R pos is the resistance of the positive sublayer electrode, R pos1 is the resistance of the first positive electrode layer in the positive composite electrode, R pos2 is the resistance of the second positive electrode layer electrode in the positive composite electrode, R posn is the resistance of the nth positive sub-layer electrode in the positive composite electrode.

[0015] Optionally, the DCR parameters include one or more of porosity, tortuosity, effective electrochemical area, electrochemical reaction constant, and lithium ion solid phase diffusion coefficient.

[0016] Optionally, the tortuosity of the actual DCR parameter is calculated by the following formula:

[0017]

[0018]

[0019] Where ε is the porosity, ρ compressed is the compaction density of the electrode, m electrode is the mass of the electrode, ρ average is the average density of the pole piece, S electrode For the polar surface, L electrode is the thickness of the electrode;

[0020] ratio is the mass ratio of the components in the electrode. 1 is the mass ratio of the first component in the electrode, ratio 2 is the mass ratio of the second component in the electrode... n is the mass proportion of the nth component in the pole piece; ρ is the true density of the components in the pole piece, ρ1 is the true density of the first component in the pole piece, ρ2 is the true density of the second component in the pole piece...ρn is the true density of the nth component in the pole piece.

[0021] Optionally, the tortuosity of the actual DCR parameter is calculated by any one of the following formulas:

[0022]

[0023] τ=γ·ε -α

[0024] Among them, τ is the tortuosity, ε is the porosity, and R ion is the ionic internal resistance, Acc is the current collector area, L is the electrode thickness, K 0 is the intrinsic conductivity of the electrolyte;

[0025] γ is the correction factor, the value range of γ is 1.5~2.0, ε is the porosity, and α is the Bruggeman index.

[0026] Optionally, the electrochemical reaction constant of the actual DCR parameter is calculated by the following formula:

[0027]

[0028] Where: k is the electrochemical reaction constant, C s,max is the maximum concentration of lithium ions in the solid phase, C s is the lithium ion solid phase concentration of the positive electrode material at 50% SOC, C e is the lithium ion concentration of the electrolyte, i 0 is the exchange current density of the positive electrode material, R is the ideal gas constant, T is the temperature, n is the reaction order, and F is the Faraday constant.

[0029] Optionally, the lithium ion solid phase diffusion coefficient of the actual DCR parameter is calculated by the following formula:

[0030]

[0031] Among them, I p is the peak current; n is the number of electron transfers in the redox process; A is the electrode area immersed in the solution; D is the solid phase diffusion coefficient of lithium ions; ν is the scan rate; C 0 is the concentration of lithium ions participating in the redox reaction.

[0032] Optionally, the positive electrode sheet includes a positive electrode current collector and the positive electrode composite electrode arranged on the surface of the positive electrode current collector, and the material of the positive electrode composite electrode includes one or more of lithium cobalt oxide, lithium iron phosphate, spinel lithium manganese oxide, ternary positive electrode material, and lithium manganese-rich positive electrode material.

[0033] Optionally, the positive sub-layer electrode is prepared by the following steps:

[0034] The SWCNT dispersion and lithium cobalt oxide are uniformly mixed in a mass ratio of 1:0.3-0.5, and dispersed into a slurry; the slurry is filtered onto a filter membrane, and the positive electrode sub-layer electrode is obtained by freeze drying and rolling;

[0035] Based on 100% of the mass of the SWCNT dispersion, the content of the single-walled carbon nanotube is 0.2-0.6wt%, the content of the carboxymethyl cellulose is 0.4-0.8wt%, and the balance is deionized water.

[0036] The beneficial effects of the present invention are:

[0037] The present invention designs a sub-layer electrode with controllable DCR components based on the DCR decomposition theory. After determining the order requirements and design goals, a strategy is quickly formulated to combine multiple sub-layer electrodes into a composite electrode and assemble them into a battery. This can achieve quantitative control of the electrochemical performance of the battery, facilitate battery modeling and simulation, and realize digital management of the power system at the subsequent application end, thereby shortening the R&D cycle and reducing R&D costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0039] Figure 1 is a schematic flow chart of a method for preparing a lithium-ion battery in an embodiment of the present invention;

[0040] Figure 2 is a schematic flow chart of a method for preparing a lithium-ion battery in an embodiment of the present invention;

[0041] Figure 3 It is a schematic diagram of a method for preparing a lithium-ion battery in Embodiment 1 of the present invention.

[0042] In the figure: 100, positive composite electrode, 110, positive sub-layer electrode, 200, negative composite electrode, 300, separator. DETAILED DESCRIPTION

[0043] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0044] In the description of the present invention, it should be understood that the terms "longitudinal", "radial", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0045] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0046] Figure 1 is a schematic flow chart of a method for preparing a lithium-ion battery in an embodiment of the present invention, such as Figure 1 As shown, and refer to Figure 2 , Figure 3 The present invention provides a method for preparing a lithium-ion battery, comprising the following steps:

[0047] Obtaining DCR design parameters of a plurality of electrode materials, and preparing the plurality of electrode materials into a plurality of sub-layer electrodes with different thicknesses by roller pressing;

[0048] Prepare a plurality of sub-layer electrodes, wherein the plurality of sub-layer electrodes are classified into positive sub-layer electrodes 110 and negative sub-layer electrodes;

[0049] Obtaining the actual DCR parameter of each of the positive sub-layer electrodes; selecting at least two of the positive sub-layer electrodes 110 according to the target DCR parameter of the electrode sheet of the target lithium-ion battery; combining the selected positive sub-layer electrodes 110 into a positive composite electrode 100; selecting at least two of the negative sub-layer electrodes according to the voltage drop of the positive composite electrode 100; combining the selected negative sub-layer electrodes into a negative composite electrode 200; wherein the actual DCR parameter of the positive composite electrode 100 is the same as the target DCR parameter of the positive electrode sheet of the target lithium-ion battery; the voltage drop ΔU of the positive composite electrode 100 pos The voltage drop ΔU of the negative composite electrode 200 neg same.

[0050] The positive composite electrode 100 is assembled with the negative electrode and the separator 300 to form a battery.

[0051] It should be noted that the release of lithium ions from the positive electrode and the embedding of lithium ions from the negative electrode of lithium-ion batteries will encounter obstacles. The obstacle under DC conditions is the direct current internal resistance (DCR).

[0052] The embodiment of the present invention designs a sub-layer electrode with controllable DCR components based on the DCR decomposition theory. After determining the order requirements and design goals, a strategy is quickly formulated to combine multiple sub-layer electrodes into a composite electrode and assemble them into a battery. This can achieve quantitative control of the electrochemical performance of the battery, facilitate battery modeling and simulation, and realize digital management of the power system of the subsequent application end, thereby shortening the R&D cycle and reducing R&D costs.

[0053] Since the DC internal resistance can be decomposed into ohmic internal resistance, electrochemical reaction internal resistance, and diffusion internal resistance according to the components. If the three internal resistances encountered in the process of lithium ion extraction from the positive electrode and lithium ion embedding from the negative electrode are not reasonably matched, the migration speed of lithium ions in the positive and negative electrode regions will be different, that is, the lithium ions extracted from the positive electrode migrate to the negative electrode region. In theory, the negative electrode has sufficient capacity to accept the lithium ions that migrate from the negative electrode, but because the kinetics of the positive and negative electrodes are not properly matched, the migration speed of lithium ions is different, which will cause the lithium ions in the negative electrode region to be locally "blocked". The lithium ions that are not embedded in the crystals of the negative electrode material in time will still undergo a reduction reaction, resulting in local lithium precipitation. Therefore, due to the kinetic mismatch between the positive and negative electrodes, local overcharge and over-discharge of the battery may occur, thereby affecting the cycle life of the battery. An overly loose kinetic matching relationship will sacrifice the volume energy density and mass energy density of the battery. In addition, the thickness of the sub-layer electrode is controlled by rolling. The smaller the thickness, the smaller the porosity, the greater the tortuosity, the greater the ohmic internal resistance, the unchanged electrochemical reaction internal resistance, and the greater the diffusion internal resistance. That is, the ohmic internal resistance is negatively correlated with the thickness, and thus the actual DCR parameter of the composite electrode can be made the same as the target DCR parameter of the target lithium-ion battery electrode by making the thickness of the composite electrode the same as the electrode thickness of the target lithium-ion battery.

[0054] Based on the above reasons, the present invention follows the principle that the overpotential caused by the positive electrode DCR is equal to the overpotential caused by the negative electrode DCR, so that the voltage drop ΔU of the negative electrode composite electrode 200 formed by the negative electrode sub-layer electrode is neg and the voltage drop ΔU of the positive composite electrode 100 pos The same can achieve quantitative control of the kinetics of the battery's electrochemical sub-processes, making it easy to achieve kinetic matching of different electrochemical processes at the positive and negative electrodes. While ensuring energy density, it reduces the possibility of battery performance degradation due to local failure and the occurrence of capacity diving, thereby taking into account both the high energy density and battery life of the battery.

[0055] like Figure 2 As shown, in an alternative embodiment of the present invention, the preparation method comprises the following steps:

[0056] Obtaining DCR design parameters of a plurality of electrode materials, and preparing the plurality of electrode materials into a plurality of sub-layer electrodes with different thicknesses by roller pressing;

[0057] Prepare a plurality of sub-layer electrodes, wherein the plurality of sub-layer electrodes are classified into positive sub-layer electrodes 110 and negative sub-layer electrodes;

[0058] Obtaining the actual DCR parameter of each of the negative sub-layer electrodes; screening out at least two of the negative sub-layer electrodes according to the target DCR parameter of the electrode sheet of the target lithium-ion battery, and combining the screened negative sub-layer electrodes into a negative composite electrode 200; screening out at least two of the positive sub-layer electrodes 110 according to the voltage drop of the negative composite electrode; combining the screened positive sub-layer electrodes 110 into a positive composite electrode 100; wherein the actual DCR parameter of the positive composite electrode 100 is the same as the target DCR parameter of the positive electrode sheet of the target lithium-ion battery; the voltage drop ΔU of the positive composite electrode 100 pos The voltage drop ΔU of the negative composite electrode 200 neg same.

[0059] The positive composite electrode 100 is assembled with the negative electrode and the separator 300 to form a battery.

[0060] Specifically, ΔU neg =I neg *R neg *m;ΔU pos =I pos *R pos *n;

[0061] Where m is the number of negative electrode layers, I neg is the current passing through the negative sublayer electrode, R neg is the resistance of the negative sub-layer electrode; n is the number of positive sub-layer electrodes, I pos is the current passing through the positive sublayer electrode, R pos is the resistance of the positive sublayer electrode.

[0062] In one embodiment of the present invention, the negative electrode sheet includes a negative electrode current collector and the negative electrode composite electrode disposed on the surface of the negative electrode current collector, and the material of the negative electrode composite electrode includes a negative electrode active material, a conductive agent, a binder, and a solvent. The active material includes one or more of a carbon-based negative electrode material, lithium titanate, a silicon-based negative electrode material, a tin-based negative electrode material, and a transition metal oxide negative electrode. The conductive agent includes one or more of conductive carbon black, Ketjen black, carbon nanotubes, and graphene. The binder includes one or more of polytetrafluoroethylene, carboxymethyl cellulose, and styrene-butadiene rubber. The solvent includes one or more of ethylene glycol, glycerol, polyethylene glycol, dimethyl sulfoxide, N-methylpyrrolidone, deionized water, alcohol, and N-methylpyrrolidone (NMP).

[0063] The positive electrode sheet comprises a positive electrode current collector and a positive electrode composite electrode arranged on the surface of the positive electrode current collector. The material of the positive electrode composite electrode comprises a positive electrode active material, a conductive agent and a binder. The positive electrode active material comprises lithium cobalt oxide, lithium iron phosphate, spinel lithium manganese oxide, a ternary positive electrode material (Li(NiCoMn)O 2 ), lithium-rich manganese cathode materials (xLi 2 MnO 3 (1–x)LiTMO 2 ,TM=Ni,Mn,Co,etc.) One or more. The thickness of the pole piece ranges from 1μm to 50μm.

[0064] In one embodiment of the present invention, the actual DCR parameter includes one or more of porosity, tortuosity, effective electrochemical area, electrochemical reaction constant, and lithium ion solid phase diffusion coefficient. The porosity of the actual DCR parameter is calculated by the following formula:

[0065]

[0066] Where ε is the porosity, ρ compressed is the compaction density of the electrode, m electrode is the mass of the electrode, ρ average is the average density of the pole piece, S electrode is the electrode area, L electrode is the thickness of the electrode;

[0067] ratio is the mass ratio of the components in the electrode. 1 is the mass ratio of the first component in the electrode, ratio 2 is the mass ratio of the second component in the electrode... n is the mass proportion of the nth component in the electrode;

[0068] ρ is the true density of the components in the pole piece, ρ1 is the true density of the first component in the pole piece, ρ2 is the true density of the second component in the pole piece...ρ n is the true density of the nth component in the electrode.

[0069] The tortuosity of the actual DCR parameter is calculated by either of the following two formulas:

[0070]

[0071] τ=γ·ε -α

[0072] Among them, τ is the tortuosity, ε is the porosity, and R ion is the ionic internal resistance, Acc is the current collector area, L is the electrode thickness, K 0is the intrinsic conductivity of the electrolyte. Among them, τ is the tortuosity, γ is the correction factor, the value range of γ is 1.5-2.0, ε is the porosity, and α is the Bruggeman index. In addition, the two formulas can verify each other. Only when the tortuosity measured by the two methods is the same, the tortuosity is used to ensure the accuracy of the calculation.

[0073] The electrochemical reaction constant of the actual DCR parameter is calculated by the following formula:

[0074]

[0075] Where: k is the electrochemical reaction constant, C s,max is the maximum solid phase concentration of lithium ions in the positive electrode material, C s is the lithium ion solid phase concentration of the positive electrode material at 50% SOC, C e is the lithium ion concentration of the electrolyte, i 0 is the exchange current density of the positive electrode material, R is the ideal gas constant, T is the temperature, n is the reaction order, and F is the Faraday constant.

[0076] The lithium ion solid phase diffusion coefficient of the actual DCR parameter is calculated by the following formula:

[0077]

[0078] Among them, I p is the peak current; n is the number of electron transfers in the redox process; A is the electrode area immersed in the solution; D is the solid phase diffusion coefficient of lithium ions; ν is the scan rate; C 0 is the concentration of lithium ions participating in the redox reaction.

[0079] Specifically, the positive sub-layer electrode is prepared by the following steps:

[0080] The SWCNT (single-walled carbon nanotube) dispersion and lithium cobalt oxide are uniformly mixed in a mass ratio of 1:0.3-0.5 and dispersed into a slurry. The slurry is filtered onto a filter membrane, and a sub-layer electrode is obtained by freeze drying and rolling. Furthermore, based on the mass of the SWCNT dispersion as 100%, the content of the single-walled carbon nanotube is 0.2-0.6wt%, the content of the carboxymethyl cellulose is 0.4-0.8wt%, and the balance is deionized water.

[0081] The present invention is further described below by way of examples. However, the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0082] Example 1

[0083] Taking the positive electrode material as high voltage 4.48V lithium cobalt oxide (LCO-4.48V) as an example, the specific information of lithium cobalt oxide is shown in Table 1.

[0084] Table 1 Specific information of lithium cobalt oxide

[0085] nature Lithium Cobalt Oxide - 4.48V <![CDATA[Particle size, D 50 (μm)]]> 16 <![CDATA[Specific surface area (cm 2 / g)]]> 0.2432 Specific capacity (mAh / g) 188 <![CDATA[Electrochemical window (vs. Li / Li + , V)]]> 3.0-4.48

[0086] (1) Preparation of positive sublayer electrode

[0087] 0.4wt% SWCNT was dispersed in water to obtain a SWCNT dispersion, wherein the stabilizer in the SWCNT dispersion was 0.6wt% carboxymethyl cellulose. LCO-4.48V and SWCNT dispersion (0.4wt% SWCNT was dispersed in water, 0.6wt% carboxymethyl cellulose was used as a stabilizer) were mixed in a mass ratio of 0.39:1, dispersed into a slurry using a high-speed shear emulsifier, and deionized water was added to adjust the viscosity to obtain a slurry. The slurry was vacuum filtered onto a water-based filter membrane (mixed cellulose ester membrane, thickness 0.45μm) to form a milky tissue. The milky tissue was then freeze-dried for 24h and rolled to form a positive sub-layer electrode. A variety of positive sub-layer electrodes of different thicknesses were prepared according to the above steps, and the positive sub-layer electrodes of different thicknesses had different DCR electrochemical parameters. Two groups of sub-layer electrodes with thicknesses of 82μm (A) and 100μm (B) were selected for the experiment.

[0088] (2) Preparation of negative electrode layer

[0089] The negative electrode active material graphite, conductive agent conductive carbon black, binder sodium carboxymethyl cellulose, and binder styrene butadiene rubber are fully stirred and mixed in an appropriate amount of deionized water solvent according to a mass ratio of 97.8%: 0.4%: 0.8%: 1.0% to form a uniform negative electrode slurry. Then the negative electrode slurry is vacuum filtered onto a water-based filter membrane (mixed cellulose ester membrane, thickness 0.45μm) to form a milky tissue. The milky tissue is then freeze-dried for 24 hours and rolled to form a negative electrode sub-layer electrode with a rolling compaction density of 1.75g / cm3. After stripping, the negative electrode sheet is obtained. Select multiple negative electrode sub-layer electrodes with different thicknesses for the experiment.

[0090] (3) Taking the positive electrode sheet as an example, obtain the actual DCR parameters of the positive electrode sheet.

[0091] By assembling a symmetrical battery, the electrochemical impedance spectroscopy (EIS) of the symmetrical battery can be tested and the ionic internal resistance (Rion) of the electrode can be obtained. The tortuosity of the electrode can then be calculated using the following formula (1) or (2), and the porosity can be calculated using the following formulas (3)-(5).

[0092] τ=γ·ε -α (1)

[0093]

[0094] Among them, τ is the tortuosity, ε is the porosity, and R ion is the ionic internal resistance, Acc is the current collector area, L is the electrode thickness, K 0 is the intrinsic conductivity of the electrolyte, γ is the correction factor, the value range of γ is 1.5~2.0, ε is the porosity, α is the Bruggeman index, ρ compressed is the compaction density of the electrode, m electrode is the mass of the electrode, ρ average is the average density of the pole piece, S electrode is the electrode area, L electrode is the thickness of the electrode. ratio is the mass ratio of the components in the electrode; ρ is the true density of the components in the electrode. Among them, active-material is the active material (LCO-4.48V), SWCNT is single-walled carbon nanotube, and CMC is carboxymethyl cellulose. The relevant data before battery aging are shown in Table 2.

[0095] Table 2 Relevant parameters of sub-layer electrodes.

[0096] parameter Lithium cobalt oxide <![CDATA[Internal resistance of the ion, R ion > 1.315Ω Current collector area, Acc <![CDATA[1.13×10-4m 2 ]]> <![CDATA[Electrolyte conductivity, K 0 > 10.3S / m Total electrode thickness, L 164×10-6m Porosity, ε 0.15 Tortuosity, τ 1.40

[0097] Obtaining the key parameters of electrochemical reaction internal resistance:

[0098] By testing the EIS of the positive electrode at different temperatures, the electrochemical reaction impedance R at different temperatures is obtained. ct The exchange current density is obtained according to formula (6), and the electrochemical reaction rate constant is calculated by formula (7). The electrochemical reaction activation energy is calculated by the relationship between the electrochemical reaction rate constant and the temperature in formula (8).

[0099]

[0100] Among them: C s,max is the maximum solid phase concentration of lithium ions in lithium cobalt oxide, C s is the lithium ion solid phase concentration of lithium cobalt oxide at 50% SOC, C e is the lithium ion concentration of the electrolyte, i 0 is the exchange current density of lithium cobalt oxide electrode particles, k is the electrochemical reaction constant, E a is the activation energy of the electrochemical reaction, R is the ideal gas constant, T is the temperature, n is the reaction order, F is the Faraday constant, T 1 、T 2 is any temperature value, T 1 ≠T 2 , k 1 T 1 The electrochemical reaction constant, k2 T 2 The specific parameters are shown in Table 3.

[0101] Table 3 Electrochemical reaction related parameters of lithium cobalt oxide (50% SOC)

[0102]

[0103] Obtaining the solid phase diffusion coefficient of lithium ions:

[0104] Based on the Randles-Sevchik equation:

[0105] I p =0.4463zFA(zF / RT) 1 / 2 ΔC 0 D 1 / 2 v 1 / 2

[0106] At room temperature, there is the following formula:

[0107] I p =2.69×10 5 An 3 / 2 C 0 D 1 / 2 v 1 / 2

[0108] Among them, I p is the peak current; n is the number of electron transfers in the redox process; A is the electrode area immersed in the solution; D is the diffusion coefficient in the electrode; ν is the scan rate; C 0 is the concentration of lithium ions participating in the redox reaction.

[0109] The area of ​​the electrode immersed in the solution can generally be considered as its geometric area. The radius of the electrode is 6 mm, and the area of ​​the electrode is 0.000113 m 2 Since the diffusion of lithium in the electrode material is a very slow process, the scan rate should be selected below 1mV / s. This experiment selected (0.1mV / s, 0.2mV / s, 0.3mV / s, 0.5mV / s, 0.8mV / s). 0 is the concentration of lithium ions participating in the redox reaction. The corresponding oxidized or reduced charge can be obtained by integrating the corresponding electrode peak. Since it is a single-electron reaction, the charge is the amount of substance of the corresponding lithium ion. Then divide it by the volume of the electrolyte to calculate the concentration of lithium ions participating in the reaction. Plot the peak current at different scan rates against the square root of the scan rate. According to I p -v 1 / 2 The parameters related to the formula are shown in Table 4.

[0110]

[0111] Table 4 Relevant parameters in the lithium ion diffusion process.

[0112] parameter Lithium cobalt oxide <![CDATA[I p -v 1 / 2 Slope]]> 0.1463 <![CDATA[Electrode area (m 2 )]]> 1.13×10-4 <![CDATA[Lithium ion concentration (mol / m 3 )]]> 16440.3 <![CDATA[Lithium ion solid-phase diffusion coefficient (m 2 / s)]]> 8.57×10-14

[0113] By obtaining the above key electrochemical parameters, the DCR of the lithium cobalt oxide electrode can be calculated. The relevant parameters of the A and B sub-layer electrodes are shown in Table 5:

[0114] Table 5 DCR related parameters of the two sub-layer electrodes

[0115]

[0116] (4) Compounding positive sub-layer electrodes with different DCR sizes

[0117] Different positive electrode sub-layer electrodes are combined into a double-layer positive electrode composite electrode by hot pressing.

[0118] (5) The negative electrode sheet is tested according to the method in step (3) and combined into a negative electrode composite electrode.

[0119] (6) The positive electrode composite electrode, the negative electrode composite electrode and the separator are assembled into a lithium-ion battery, and the cycle performance test is performed. Among them, the positive electrode sublayer electrode close to the current collector in the positive electrode composite electrode (hereinafter referred to as the near current collector layer) is A, and the positive electrode sublayer electrode close to the separator (hereinafter referred to as the near separator layer) is B.

[0120] The differences between Examples 2-4 and Comparative Examples 1-3 and Example 1 are shown in Table 6.

[0121] Table 6 Composite electrode structure of Examples 1-4

[0122]

[0123]

[0124] The cycle performance of the lithium ion batteries of Examples 1-4 and the lithium ion batteries of Comparative Examples 1-3 was tested, and the cycle performance comparison is shown in Table 7.

[0125]

[0126] From Table 7, we can see that:

[0127] Example 1 is the best example. Compared with Example 1, Example 3 and Example 2, and Example 4 and Example 3, the cycle performance of the composite electrode is not inferior to that of the electrode integrally formed in the prior art, indicating that the composite electrode composed of multiple sub-layer electrodes does not reduce its cycle performance. At the same time, the present invention designs a sub-layer electrode with controllable DCR components based on the DCR decomposition theory, prepares multiple sub-layer electrodes with different parameters in advance, and quickly formulates a strategy after determining the order requirements and design goals, and combines multiple sub-layer electrodes into a composite electrode and assembles them into a battery, which can realize quantitative control of the electrochemical performance of the battery, facilitate battery modeling and simulation, and realize digital management of the power system of the subsequent application end, thereby shortening the R&D cycle and reducing R&D costs.

[0128] Moreover, compared with comparative example 1, when the thickness is the same, the cycle performance of the double-layer composite electrode of example 1 is improved, indicating that the cycle performance of the composite electrode formed by reasonable arrangement of the sub-layer electrodes can be improved, while shortening the R&D cycle and reducing the R&D cost, it can also improve the cycle performance and obtain an electrode structure with excellent cycle performance.

[0129] The embodiments described above are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included in the protection scope of the present invention.

Claims

1. A method for preparing a lithium ion battery, characterized in that: The following steps are involved: Prepare a plurality of sub-layer electrodes, wherein the plurality of sub-layer electrodes are classified into positive sub-layer electrodes and negative sub-layer electrodes; Obtaining the actual DCR parameter of each of the positive sub-layer electrodes; screening out at least two of the positive sub-layer electrodes according to the target DCR parameter of the electrode sheet of the target lithium-ion battery; combining the screened positive sub-layer electrodes into a positive composite electrode; wherein the actual DCR parameter of the positive composite electrode is the same as the target DCR parameter of the positive electrode sheet of the target lithium-ion battery; screening out at least two of the negative sub-layer electrodes according to the voltage drop of the positive composite electrode; combining the screened negative sub-layer electrodes into a negative composite electrode; or, Obtaining the actual DCR parameter of each of the negative sub-layer electrodes; screening out at least two of the negative sub-layer electrodes according to the target DCR parameter of the electrode sheet of the target lithium-ion battery; combining the screened negative sub-layer electrodes into a negative composite electrode; wherein the actual DCR parameter of the negative composite electrode is the same as the target DCR parameter of the negative electrode sheet of the target lithium-ion battery; screening out at least two of the positive sub-layer electrodes according to the voltage drop of the negative composite electrode; combining the screened positive sub-layer electrodes into a negative composite electrode; The voltage drop ΔU of the positive composite electrode pos The voltage drop ΔU of the negative electrode composite electrode neg same; The positive composite electrode, the negative composite electrode and a separator are assembled into a lithium ion battery.

2. The preparation method according to claim 1, characterized in that: ΔU neg =I neg1 *R neg1 +I neg2 *R neg2 +...+I negm *R negm ; ΔU pos =I pos1 *R pos1 +I pos2 *R pos2 +...+I posn *R posn ; Among them, I neg is the current passing through the negative sublayer electrode, I neg1 is the current passing through the first negative electrode sublayer electrode in the negative electrode composite electrode, I neg2 I is the current passing through the second negative electrode sub-layer electrode in the negative electrode composite electrode; negm is the current passing through the mth negative electrode sublayer electrode in the negative composite electrode; R neg is the resistance of the negative sublayer electrode, R neg1 is the resistance of the first negative electrode sub-layer electrode in the negative electrode composite electrode, R neg2 is the resistance of the second negative electrode sub-layer electrode in the negative electrode composite electrode, R negm is the resistance of the mth negative electrode sublayer electrode in the negative composite electrode; I pos is the current passing through the positive sublayer electrode, I pos1 I is the current passing through the first positive electrode sub-layer electrode in the positive electrode composite electrode; pos2 is the current passing through the second positive electrode layer electrode in the positive electrode composite electrode, I posn is the current passing through the nth positive sub-layer electrode in the positive composite electrode; R pos is the resistance of the positive sublayer electrode, R pos1 is the resistance of the first positive electrode layer in the positive composite electrode, R pos2 is the resistance of the second positive electrode layer electrode in the positive composite electrode, R posn is the resistance of the nth positive sub-layer electrode in the positive composite electrode.

3. The preparation method according to claim 1, characterized in that: The DCR parameters include one or more of porosity, tortuosity, effective electrochemical area, electrochemical reaction constant, and lithium ion solid phase diffusion coefficient.

4. The preparation method according to claim 3, characterized in that: The tortuosity of the actual DCR parameter is calculated by the following formula: Where ε is the porosity, ρ compressed is the compaction density of the electrode, m electrode is the mass of the electrode, ρ average is the average density of the pole piece, S electrode For the polar surface, L electrode is the thickness of the electrode; ratio is the mass ratio of the components in the pole piece, ratio1 is the mass ratio of the first component in the pole piece, and ratio2 is the mass ratio of the second component in the pole piece...ratio n is the mass proportion of the nth component in the pole piece; ρ is the true density of the component in the pole piece, ρ1 is the true density of the first component in the pole piece, ρ2 is the true density of the second component in the pole piece...ρ n is the true density of the nth component in the electrode.

5. The preparation method according to claim 3, characterized in that: The tortuosity of the actual DCR parameter is calculated by the following formula: Among them, τ is the tortuosity, ε is the porosity, and R ion is the ionic internal resistance, Acc is the current collector area, L is the electrode thickness, and K0 is the intrinsic conductivity of the electrolyte.

6. The preparation method according to claim 3, characterized in that: The tortuosity of the actual DCR parameter is calculated by the following formula: τ=γ·ε -α Among them, τ is the tortuosity, γ is the correction factor, the value range of γ is 1.5~2.0, ε is the porosity, and α is the Bruggeman index.

7. The preparation method according to claim 3, characterized in that: The electrochemical reaction constant of the actual DCR parameter is calculated by the following formula: Where: k is the electrochemical reaction constant, C s,max is the maximum concentration of lithium ions in the solid phase, C s is the lithium ion solid phase concentration of the positive electrode material at 50% SOC, C e is the lithium ion concentration of the electrolyte, i 0 is the exchange current density of the positive electrode material, R is the ideal gas constant, T is the temperature, n is the reaction order, and F is the Faraday constant.

8. The preparation method according to claim 3, characterized in that: The lithium ion solid phase diffusion coefficient of the actual DCR parameter is calculated by the following formula: Among them, I p is the peak current; n is the number of electron transfers in the redox process; A is the electrode area immersed in the solution; D is the solid phase diffusion coefficient of lithium ions; ν is the scan rate; C0 is the lithium ion concentration participating in the redox reaction.

9. The preparation method according to claim 1, characterized in that: The positive electrode sheet includes a positive electrode collector and the positive electrode composite electrode arranged on the surface of the positive electrode collector. The material of the positive electrode composite electrode includes one or more of lithium cobalt oxide, lithium iron phosphate, spinel lithium manganese oxide, ternary positive electrode material, and lithium manganese-rich positive electrode material.

10. The preparation method according to claim 9, characterized in that: The positive sub-layer electrode is prepared by the following steps: The SWCNT dispersion and lithium cobalt oxide are uniformly mixed in a mass ratio of 1:0.3-0.5, and dispersed into a slurry; the slurry is filtered onto a filter membrane, and the positive electrode sub-layer electrode is obtained by freeze drying and rolling; Based on 100% of the mass of the SWCNT dispersion, the content of the single-walled carbon nanotube is 0.2-0.6wt%, the content of the carboxymethyl cellulose is 0.4-0.8wt%, and the balance is deionized water.

Citation Information

Patent Citations

  • Lithium ion battery preparation method and lithium ion battery

    CN113540571A

  • Method for decomposing direct current internal resistance of lithium ion battery based on numerical model

    CN114280480A

  • Method for improving matching consistency of lithium ion batteries

    CN116742163A

  • Secondary battery and electric device

    CN117253976A

  • Lithium ion battery and electronic device comprising same

    CN117334835A