Glass plate and method for manufacturing glass plate

By designing multiple spoon-cut concave surfaces on the glass plate and optimizing their surface shape through laser microscope and watershed algorithm, the problem of flash point glare in the anti-glare treatment of existing glass plates is solved, achieving better visual effects .

CN118973976APending Publication Date: 2024-11-15AGC INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202380034592.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Although the existing anti-glare treatment of glass plates suppresses the reflection of surrounding objects, it produces glare called flash points, affecting the visual recognition of the image.

Method used

Using glass plates with multiple spoon-cut concave surfaces, the surface shape is measured by laser microscope and the concave surface is decomposed using a watershed algorithm to ensure that the standard deviation of the concave surface area and depth is within a specific range to reduce the generation of glare.

Benefits of technology

It effectively inhibits the reflection of surrounding objects and significantly reduces the generation of glare, improving the visual recognition of the image.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973976A_ABST
    Figure CN118973976A_ABST
Patent Text Reader

Abstract

The glass plate has a first main surface and a second main surface facing opposite to the first main surface, and the first main surface includes an anti-glare surface. The anti-glare surface has a plurality of concave curved surfaces in the shape of a spoon cut. When the surface shape of the anti-dazzle surface is measured by a laser microscope and the anti-dazzle surface is decomposed into the plurality of concave curved surfaces by a watershed algorithm based on the measurement result, the anti-dazzle surface satisfies the following (A)-(D). (A) The standard deviation S [sigma] of the area S of the concave curved surface in plan view is 32.5 [mu] m2 or less. (B) The number N of the concave curved surfaces per predetermined area in plan view is 250 or more / 100 [mu] m. (C) The average value HAVE of the depth H of the concave curved surface is 0.10 [mu] m or more. (D) The standard deviation (H [sigma]) of the depth (H) is 0.220 [mu] m or less, and the product (HAVE * H [sigma]) of the average value (HAVE) of the depth (H) and the standard deviation (H [sigma]) is 0.085 [mu] m2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to glass sheets and methods of making glass sheets. Background Art

[0002] A protective glass is provided on the surface of an image display device that displays an image. When surrounding objects (including lighting) are reflected in the protective glass, the visibility of the image is reduced. Therefore, research is underway to perform anti-glare treatment on the glass plate constituting the protective glass.

[0003] The anti-glare treatment is a treatment that provides fine concavities and convexities on the main surface of the glass plate. The concavities and convexities can diffuse reflected light and suppress reflection. The anti-glare treatment includes, for example, at least one selected from frosting, etching, and sandblasting.

[0004] The anti-glare treatment of Patent Document 1 includes the steps of sandblasting the main surface of a glass plate using a mixture of sand particles having a chord length of 0.5 μm to 2 μm and water, and then etching the main surface of the glass plate.

[0005] The anti-glare treatment of Patent Document 2 includes a step of frosting the main surface of the glass plate and a step of etching the main surface of the glass plate. In the frosting treatment, for example, a mixed aqueous solution of ammonium fluoride or potassium fluoride and hydrogen fluoride is used.

[0006] The anti-glare treatment of Patent Document 3 includes a step of sandblasting the main surface of the glass plate and then etching the main surface of the glass plate. As particles for sandblasting, particles with a particle size of #2000 or more are used.

[0007] The anti-glare treatment of Patent Document 4 includes a step of sandblasting the main surface of the glass plate and then etching the main surface of the glass plate. As particles for sandblasting, particles with a particle size of #3000 or more are used.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2021-532056

[0011] Patent Document 2: International Publication No. 2018 / 235808

[0012] Patent Document 3: International Publication No. 2018 / 230079

[0013] Patent Document 4: International Publication No. 2018 / 074494 Summary of the invention

[0014] Problems to be solved by the invention

[0015] Anti-glare treatment reduces the reflection of surrounding objects, but produces glare called sparkle. Glare is caused by the unevenness acting as tiny lenses.

[0016] One aspect of the present disclosure provides a technology for suppressing reflection of surrounding objects and suppressing generation of glare.

[0017] Means used to solve problems

[0018] A glass plate in one embodiment of the present disclosure has a first main surface and a second main surface facing opposite to the first main surface, wherein the first main surface includes an anti-glare surface. The anti-glare surface has a plurality of concave surfaces in a spoon-cut shape. When the surface shape of the anti-glare surface is measured using a laser microscope, and the anti-glare surface is decomposed into a plurality of the concave surfaces using a watershed algorithm based on the measurement result, the anti-glare surface satisfies the following (A) to (D). (A) The standard deviation S of the area S of the concave surface when viewed from above σ 32.5μm 2 (B) The number N of the concave curved surfaces per predetermined area in a plan view is 250 or more / 100 μm square. (C) The average value H of the depth H of the concave curved surface is AVE 0.10 μm or more. (D) The standard deviation H of the depth H σ is less than 0.220 μm, and the average value H of the depth H AVE The standard deviation H σ The product of H AVE ×H σ 0.085μm 2 the following.

[0019] Effects of the Invention

[0020] According to one aspect of the present disclosure, it is possible to suppress reflection of surrounding objects and to suppress the generation of glare. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 (A) is a cross-sectional view showing a part of a glass plate according to one embodiment, Figure 1 (B) is to Figure 1 (A) A partially enlarged cross-sectional view.

[0022] Figure 2 It is a diagram showing an example of a measuring device for measuring the anti-glare index value D.

[0023] Figure 3 This is a flowchart showing a method for producing a glass plate according to one embodiment.

[0024] Figure 4This is a cross-sectional view showing an example of a concave curved surface formed starting from a microcrack.

[0025] Figure 5 This is a graph showing the particle size distribution of particles used in Examples 1 to 10 and 12 to 13 in Table 1.

[0026] Figure 6 The anti-glare surface obtained in Examples 1 to 4 in Table 1 is decomposed into a plurality of concave curved surface images using a watershed algorithm.

[0027] Figure 7 The anti-glare surface obtained in Examples 5 to 8 in Table 1 is decomposed into multiple concave surfaces using a watershed algorithm.

[0028] Figure 8 The anti-glare surface obtained in Examples 9 to 11 in Table 1 is decomposed into multiple concave surfaces using a watershed algorithm.

[0029] Fig. 9 The anti-glare surface obtained in Examples 12 and 13 of Table 1 is decomposed into multiple concave surfaces using a watershed algorithm. DETAILED DESCRIPTION

[0030] Hereinafter, the method for implementing the present disclosure will be described with reference to the accompanying drawings. In each of the accompanying drawings, the same or corresponding structures are marked with the same symbols, and the description is sometimes omitted. In the specification, "to" indicating a numerical range means that the numerical values ​​recorded before and after it are included as the lower limit and upper limit.

[0031] Reference Figure 1 A glass plate 1 according to an embodiment is described. The glass plate 1 has a first main surface 11 and a second main surface 12 facing opposite to the first main surface 11. The first main surface 11 includes an anti-glare surface. The anti-glare surface is a surface that suppresses reflection of surrounding objects (including lighting). The entire first main surface 11 may be an anti-glare surface, or a portion of the first main surface 11 may be an anti-glare surface.

[0032] The glass plate 1 is used as a protective glass of an image display device. The image display device is assembled in a portable or fixed electronic device. Portable electronic devices include, for example, mobile phones, smart phones, e-book readers, and notebook personal computers. Fixed electronic devices include, for example, desktop personal computers, digital signage, car displays, televisions, and electronic blackboards (IFPs).

[0033] The anti-glare surface has a plurality of concave curved surfaces 111 in a spoon-cut shape. The surface shape of the anti-glare surface is measured, for example, using a laser microscope VK-X260 manufactured by Keyence Corporation and using a 150-fold objective lens in a high-definition mode. The measured surface shape data is analyzed, for example, using image analysis software SPIP (registered trademark) version 5.1.11 manufactured by Image Metrology. In the following description of the surface shape data analysis, the terms enclosed in brackets are terms used in SPIP.

[0034] First, in order to remove the overall tilt, in the "Plane Correction Dialog Box", select "Average Profile Fit" in "Global Correction" and select "Bearing Height To Zero" in "Z Offset Method" to perform tilt correction.

[0035] Next, in Particle & Pore Analysis, set the parameters of the Detection tab as follows. Using Watershed-Dispersed Features, set Detect Pores to On, Plateau Range to 0, Number of Detail Levels to 2, Merge Adjoining Shapes to Off, and Smoothing Filter Size and Finest Filter Size to the arithmetic mean height Sa measured separately as follows. When the arithmetic mean height Sa is above 0.17 μm, set Smoothing Filter Size to 23 pixels (2.13 μm) and Finest Filter Size to 11 pixels (1.02 μm). When the arithmetic mean height Sa is less than 0.17 μm, set the "Filter size smoothing" to 17 pixels (1.58 μm) and the "Minimum filter size" to 7 pixels (0.65 μm). Set the "Slope Noise Reduction" to 10% and the "Slope Image Threshold Percentile" to 0%.

[0036] Next, in Particle / Pore Analysis, set the Post Processing tab as follows: Set Include Shapes on Border to On, set the Z Range to 0.03 μm, and the Diameter to 0.80 μm.

[0037] By performing data analysis of the surface shape with the above settings, the "Area Value" and "Z Range Output" are obtained. The "Area Value" is used as the area S of the concave surface 111 when viewed from above. Viewing from above means observing from a direction orthogonal to the first main surface 11 and the second main surface 12. The "Z Range Output" is used as the depth H of the concave surface 111. The area S and the depth H are calculated for each concave surface 111.

[0038] When the surface shape of the anti-glare surface is measured using a laser microscope as described above and the anti-glare surface is decomposed into a plurality of concave surfaces 111 using a watershed algorithm based on the measurement result, the anti-glare surface preferably satisfies the following (A) to (D).

[0039] (A) Standard deviation S of the area S of the concave surface 111 in plan view σ 32.5μm 2 In this specification, “μm 2 " refers to square micrometers. The smaller the variation in the size of the concave surface 111, the more uniform the appearance of the anti-glare surface becomes. If S σ 32.5μm 2 If the anti-glare surface has a uniform appearance, the glare can be suppressed. σ More preferably 23.5 μm 2 Below. σ More preferably, it is 14.5 μm 2 Below. σ 0.0μm 2 Above. σ More preferably, 3.0 μm 2 Above. σ More preferably, it is 5.0 μm 2 above.

[0040] (B) The number N of concave surfaces 111 per specified area when viewed from above is 250 or more / 100 μm square. N is detected in a square area with a side length of 100 μm when viewed from above. The larger N is, the smaller the distance between the centers of the concave surfaces 111 is, the smaller the size of the concave surfaces 111 is, and the more uniform the appearance of the anti-glare surface becomes. If N is 250 or more / 100 μm square, the appearance of the anti-glare surface can be made sufficiently uniform, and glare can be suppressed. N is more preferably 350 or more / 100 μm square. N is further preferably 450 or more / 100 μm square. In addition, N is preferably less than 1000 / 100 μm square. N is more preferably less than 950 / 100 μm square. N is further preferably less than 900 / 100 μm square.

[0041] (C) Average value H of the depth H of the concave surface 111 AVE The depth H of the concave surface 111 is the depth measured from the edge (boundary) of the concave surface 111. The edge (boundary) of the concave surface 111 is obtained using a watershed algorithm. AVE The larger it is, the easier it is to diffuse the reflected light. AVE If the thickness is 0.10 μm or more, the reflection of surrounding objects can be suppressed. AVE More preferably, it is 0.17 μm or more. AVE More preferably, the thickness is 0.24 μm or more. AVE It is preferably 0.50 μm or less, more preferably 0.47 μm or less, and further preferably 0.44 μm or less.

[0042] (D) Standard deviation H of depth H σ The average value of the depth H is 0.220 μm or less. AVE With standard deviation H σ The product of H AVE ×H σ 0.085μm 2 The smaller the variation of depth H is, the more uniform the appearance of the anti-glare surface becomes. σ 0.220 μm or less and H AVE ×H σ 0.085μm 2 If the anti-glare surface has a uniform appearance, the glare can be suppressed. σ More preferably, it is 0.200 μm or less. σ More preferably, it is 0.180 μm or less. σ 0.000 μm or more. σ More preferably, it is 0.025 μm or more. σ More preferably, it is 0.050 μm or more. AVE×H σ More preferably, 0.080 μm 2 Below. AVE ×H σ More preferably, it is 0.070 μm 2 Below. AVE ×H σ 0.000 μm 2 Above. AVE ×H σ More preferably, 0.003 μm 2 Above. AVE ×H σ More preferably, it is 0.005 μm 2 above.

[0043] The anti-glare surface preferably further satisfies the following (E). (E) The average value S of the area S of the concave curved surface 111 in a plan view: AVE 6μm 2 Above and 33μm 2 Below. If S AVE 33μm 2 Below, the appearance of the anti-glare surface can be made more uniform, and the glare can be further suppressed. AVE 6μm 2 With the above, the reflected light can be further diffused, and the reflection of surrounding objects can be further suppressed. AVE More preferably 6.5 μm 2 Above and 23μm 2 Below. AVE More preferably, it is 7 μm 2 Above and 17μm 2 the following.

[0044] The haze value of the anti-glare surface is preferably 50% or less. The haze value is measured using a commercially available measuring device. The measuring device and measuring conditions are as follows. Measuring device: Suga Test Instruments Haze Meter HZ-V3; Measuring conditions: measured using C light source according to Japanese Industrial Standards (JIS K 7136: 2000).

[0045] The haze value is preferably 0% or more and 50% or less. If the haze value is 50% or less, the clarity of the transmission image is good. The haze value is more preferably 40% or less, further preferably 35% or less, particularly preferably 30% or less, and further particularly preferably 25% or less.

[0046] The glare index value Sp of the anti-glare surface is preferably 4.6% or less. The specific method for measuring the glare index value Sp is as follows. The pixel pattern (Pixel Pattern) attached to SMS-1000 manufactured by D&MS as a photomask is set on the light-emitting surface of the backlight source with its pattern surface facing upward. Then, the glass plate 1 is set on the pattern surface of the photomask with its first main surface 11 facing upward. In a state where a green monochrome image display composed of RGB (0, 255, 0) is simulated by setting the above-mentioned photomask on the light-emitting surface of the backlight source whose luminous color is green, the camera of the measuring device SMS-1000 manufactured by DM&S is used to shoot a 190dpi area of ​​the pattern surface of the photomask through the glass plate 1. The sparkle value obtained by image analysis of the measuring device is the glare index value Sp. Here, the measurement is performed in DIM (Difference Image Method) mode. The pixel ratio (Pixel Ratio) is adjusted to a height of 9.25, and the measurement is performed with the focus on the pixel surface as much as possible. At this time, the distance between the light shielding plate attached to the camera and the glass plate 1 is about 262 mm. The camera lens uses a 23FM50SP lens with an aperture of 5.6 and a focal length of 50 mm.

[0047] The glare index value Sp is preferably 0.0% or more and 4.6% or less. If the glare index value Sp is 4.6% or less, the generation of glare can be suppressed. The glare index value Sp is more preferably 4.3% or less. The glare index value Sp is further preferably 4.0% or less.

[0048] The anti-glare index value D of the anti-glare surface is preferably 0.10 or more. Figure 2 The method for measuring the anti-glare index value D is described below. Figure 2As shown, the measuring device 70 has a linear light source device 71 and a surface brightness measuring instrument 75. The linear light source device 71 includes a light source 711 and a black plate 712. The black plate 712 is arranged horizontally and has a rectangular (101 mm×1 mm) slit when viewed in the vertical direction. The light source 711 is provided at the slit. The light source 711 is a white light source of a cold cathode tube (CCFL). The glass plate 1 is arranged horizontally below the linear light source device 71 and the surface brightness measuring instrument 75 so that its first main surface 11 faces upward. The surface brightness measuring instrument 75 is arranged on a plane perpendicular to the linear light source device 71 at the center of the length direction of the linear light source device 71. The focus of the surface brightness measuring instrument 75 is aligned with the image of the linear light source device 71 reflected by the glass plate 1. That is, the surface where the focus of the image is converged is consistent with the black plate 712. Among the light rays incident from the linear light source device 71, reflected by the glass plate 1 and incident on the surface brightness measuring instrument 75, when focusing on the light rays 731 and 732 having the same incident angle θi and reflection angle θr, θi=θr=5.7°.

[0049] In addition, the black plate is brought into contact with the second main surface 12 of the glass plate 1. Therefore, the light detected by the surface brightness measuring instrument 75 is the reflected light reflected by the glass plate 1.

[0050] The scattering generated by the glass plate 1 is represented by the difference Δθ between the reflection angle θr and the incident angle θi (Δθ=θr-θi). For example, when focusing on the light rays 733 and 734 with Δθ=0.5°, the light 734 is scattered on the glass plate 1 in a direction deviating 0.5° from the regular reflection. The light 734 is observed in the surface brightness measuring instrument 75 as an image of the portion where the black plate 712 and the imaginary light 733-2 intersect. The incident angle of the imaginary light 733-2 is equal to the reflection angle of the light 734.

[0051] When the surface brightness is obtained by the surface brightness measuring instrument 75, the brightness of the part irradiated by the light 732 reflected on the glass plate 1 is the highest, and a bright line appears at this part. An image with a lower brightness as it moves away from the left and right sides with the bright line as the center is obtained. The brightness of the position away from the bright line reaches a brightness corresponding to the intensity of the light scattered by the glass plate 1. Therefore, the brightness cross-sectional profile in the direction perpendicular to the bright line is extracted. It should be noted that in order to improve the measurement accuracy, the data can also be accumulated in the direction parallel to the bright line.

[0052] When focusing on the light beams 731 and 732 , the incident angle θi and the reflection angle θr are equal, and Δθ = 0.0°. Since the brightness measurement data includes errors, the average brightness value within the range of Δθ = 0.0°±0.1° is set to D1.

[0053] When focusing on light rays 733 and 734, the reflection angle θr is greater than the incident angle θi, and Δθ = 0.5°. Since the brightness measurement data includes errors, the average brightness value within the range of Δθ = 0.5° ± 0.1° is set as D2.

[0054] Similarly, when focusing on light rays 735 and 736, the reflection angle θr is smaller than the incident angle θi, and Δθ = -0.5°. Since the brightness measurement data includes errors, the average brightness within the range of Δθ = -0.5° ± 0.1° is set as D2.

[0055] The obtained D1, D2, and D3 are substituted into the following formula (1) to calculate the anti-glare index value D.

[0056] D=(D2+D3) / (2×D1)···(1).

[0057] It was confirmed that the anti-glare index value D showed a good correlation with the anti-glare judgment result obtained by the observer's visual observation. For example, the smaller the anti-glare index value D (the closer to zero), the worse the anti-glare property. On the contrary, the larger the anti-glare index value D (the closer to 1), the better the anti-glare property.

[0058] The measurement of D1, D2, and D3 can be performed, for example, by using the device SMS-1000 manufactured by DM&S. When using this device, a C1614A lens with a focal length of 16 mm is used with an aperture of 5.6. In addition, the distance from the first main surface 11 of the glass plate 1 to the camera lens is about 300 mm, and the imaging scale is set in the range of 0.0276 to 0.0278.

[0059] The anti-glare index value D is preferably 0.10 or more and less than 1.00. If the anti-glare index value D is 0.10 or more, the reflection of surrounding objects can be suppressed. The anti-glare index value D is more preferably 0.12 or more. The anti-glare index value D is further preferably 0.15 or more.

[0060] The glass plate 1 may be a flat plate or a curved plate. The thickness of the glass plate 1 is preferably 5 mm or less, more preferably 3 mm or less. In addition, the thickness of the glass plate 1 is preferably 0.2 mm or more, more preferably 0.3 mm or more.

[0061] The glass of the glass plate 1 is, for example, aluminosilicate glass, alkali aluminosilicate glass, soda-lime glass, borosilicate glass, phosphosilicate glass, alkali aluminoborosilicate glass, lead glass, alkali barium glass, or aluminoborosilicate glass. Specific examples include the following glasses (i) to (v).

[0062] (i) A glass comprising, in terms of mol % based on oxides, 50% to 80% of SiO2, 0% to 26% of Al2O3, 0% to 25% of Na2O, 0% to 10% of B2O3, 0% to 20% of K2O, 0% to 20% of MgO and 0% to 15% of CaO.

[0063] (ii) A glass comprising, in mole % based on oxides, 50% to 80% SiO2, 2% to 25% Al2O3, 0% to 10% Li2O, 0% to 18% Na2O, 0% to 10% K2O, 0% to 15% MgO, 0% to 5% CaO and 0% to 5% ZrO2.

[0064] (iii) A glass comprising, in mol % based on oxides, 50% to 74% of SiO2, 1% to 10% of Al2O3, 6% to 14% of Na2O, 3% to 11% of K2O, 2% to 15% of MgO, 0% to 6% of CaO and 0% to 5% of ZrO2, wherein the total content of SiO2 and Al2O3 is 75% or less, the total content of Na2O and K2O is 12% to 25% and the total content of MgO and CaO is 7% to 15%.

[0065] (iv) A glass comprising, in mole % based on oxides, 68% to 80% SiO2, 4% to 10% Al2O3, 5% to 15% Na2O, 0% to 1% K2O, 4% to 15% MgO and 0% to 1% ZrO2.

[0066] (v) A glass comprising, in mole % based on oxides, 67% to 75% of SiO2, 0% to 4% of Al2O3, 7% to 15% of Na2O, 1% to 9% of K2O, 6% to 14% of MgO, and 0% to 1.5% of ZrO2, wherein the total content of SiO2 and Al2O3 is 71% to 75%, the total content of Na2O and K2O is 12% to 20%, and when CaO is contained, the content of CaO is less than 1%.

[0067] Reference Figure 3 A method for manufacturing a glass plate 1 according to one embodiment is described. The method for manufacturing the glass plate 1 includes obtaining an anti-glare surface by sequentially performing wet blasting (step S101 ) and wet etching (step S102 ) on at least a portion of the first main surface 11 of the glass plate 1 .

[0068] It should be noted that the method for manufacturing the glass plate 1 may also include treatments other than steps S101 to S102. For example, the method may also include chemically strengthening the glass plate 1 after step S102. The chemical strengthening treatment is a treatment for forming a compressive stress layer on the surface of the glass by ion exchange at a temperature below the glass transition temperature. The compressive stress layer is formed by exchanging alkali metal ions with a small ion radius contained in the glass with alkali metal ions with a larger ion radius.

[0069] Step S101 includes wet blasting at least a portion of the first main surface 11 of the glass plate 1. Wet blasting is a process in which a slurry containing particles is sprayed from a nozzle using gas pressure and collides with an object, thereby forming minute cracks (microcracks) in the object.

[0070] The slurry contains particles and a dispersion medium described below. Examples of the dispersion medium include water, a water-soluble organic solvent, or a mixture of water and a water-soluble organic solvent. Examples of the water-soluble organic solvent include lower alcohols or ketones. Specific examples of lower alcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, or tert-butanol. Specific examples of ketones include acetone.

[0071] In addition, the slurry may contain a dispersing aid. Examples of the dispersing aid include carboxymethyl cellulose, polyacrylic acid derivatives or salts thereof, polycarboxylic acid derivatives or salts thereof, or polyureaurethane. Specific examples of polyacrylic acid derivatives or salts thereof include polyacrylic acid, ammonium polyacrylate, sodium polyacrylate, polyacrylamide, acrylate·acrylate copolymer, acrylamide·acrylate copolymer, or acrylate·acrylamide·acrylate copolymer. Specific examples of polycarboxylic acid derivatives or salts thereof include ammonium polycarboxylate or sodium polycarboxylate. The ratio of the dispersing aid in the slurry is preferably 0.03% by mass or more and 2.0% by mass or less.

[0072] From the viewpoint of processability, the particles contained in the slurry are preferably particles having a Mohs hardness higher than that of glass, and are preferably inorganic particles other than spherical particles. The material of the inorganic particles can be a metal (including alloys) or an inorganic compound. The inorganic compound can be a metal compound or a non-metallic compound. As metals, stainless steel, zinc or copper can be mentioned. As inorganic compounds, silicon dioxide, glass, garnet, zirconium oxide, aluminum oxide, silicon carbide, boron carbide or CO2 (dry ice) can be mentioned. Among them, aluminum oxide is preferred. The particles contained in the slurry can use commercial products. As commercial products, for example, white aluminum oxide manufactured by FUJIMI INCORPORATED can be mentioned.

[0073] From the viewpoint of productivity, the concentration of particles in the slurry is preferably 0.05 mass % or more, more preferably 0.1 mass % or more. On the other hand, from the viewpoint of the fluidity of the slurry, the concentration of particles in the slurry is preferably 30 mass % or less, more preferably 10 mass % or less.

[0074] Compared with dry sandblasting, wet sandblasting can use particles with a smaller particle size d and can form a large number of tiny cracks (microcracks). Then, in step S102 described later, as shown in FIG. Figure 4 As shown in FIG. 1 , by isotropically etching the glass with the microcrack 112 as the starting point, the concave surface 111 can be formed. Figure 4 In FIG. 1 , a plurality of dotted lines represent the time-dependent change in the surface shape of the glass. When the glass is isotropically etched, the depth H of the concave surface 111 and the depth of the microcrack 112 are approximately the same.

[0075] The depth of the microcrack 112 varies depending on the particle size d of the particle, etc. The smaller the particle size d, the smaller the impact of the particle, and the smaller the depth of the microcrack 112. The smaller the depth of the microcrack 112, the smaller the area S of the concave surface 111 when viewed from above. In addition, the smaller the depth of the microcrack 112, the smaller the depth H of the concave surface 111.

[0076] The average particle size d of the particles contained in the slurry is preferably AVE (hereinafter also referred to as average particle size d AVE ) is 2.00 μm or more. If the average particle size d AVE If the depth H of the concave surface 111 is 2.00 μm or more, the average value H of the depth H of the concave surface 111 (C) can be obtained. AVE The anti-glare surface is 0.10 μm or more. AVE When the average particle size d is 2.00 μm or more, the processing time of the microcracks 112 can be shortened and the processability of the microcracks 112 can be improved. AVE More preferably, it is 2.05 μm or more. AVE More preferably, it is 2.10 μm or more.

[0077] The particles contained in the slurry preferably have an average particle size d AVE If the average particle size d AVE If the average depth of the microcracks 112 is less than 4.50 μm, the average value S of the area S (E) can be obtained. AVE 6μm 2 Above and 33μm 2 The following anti-glare surface. Average particle size d AVE More preferably, it is 4.00 μm or less. AVEMore preferably, it is 3.50 μm or less. AVE More preferably, it is 3.00 μm or less.

[0078] The coefficient of variation d of the particle size d of the particles contained in the slurry is preferably CV (Coefficient of variation d CV = standard deviation d σ / average value AVE ) is less than 0.400. If the coefficient of variation d CV When the depth H is 0.400 or less, the depth of the microcracks 112 can be made uniform. Therefore, the standard deviation H of the depth H (D) can be obtained. σ is 0.220 μm or less, and the average value H of the depth H AVE With standard deviation H σ The product of H AVE ×H σ 0.085μm 2 Furthermore, by making the depth of the microcracks 112 uniform, the area S of the concave curved surface 111 when viewed from above is also uniform, and (A) the standard deviation S of the area S of the concave curved surface 111 when viewed from above can be obtained. σ 32.5μm 2 In addition, the ratio of microcracks 112 with a depth less than the specified value is reduced, and the ratio of microcracks 112 with a depth greater than the specified value is increased, so that (C) the average value H of the depth H of the concave surface 111 can be obtained. AVE The anti-glare surface is 0.10 μm or more. Coefficient of variation d CV It is more preferably 0.360 or less, further preferably 0.320 or less, and particularly preferably 0.250 or less. From the viewpoint of workability of the classification operation, the coefficient of variation d CV It is preferably 0.030 or more, and more preferably 0.060 or more.

[0079] If the coefficient of variation d CV If the depth of the microcracks 112 is equal to or less than 0.250, the depth of the microcracks 112 can be made uniform. Therefore, the standard deviation H of the depth H (Da) can be obtained. σ is 0.180 μm or less, and the average value H of the depth H AVE With standard deviation H σ The product of H AVE ×H σ 0.070μm 2 Furthermore, by making the depth of the microcracks 112 uniform, the area S of the concave curved surface 111 when viewed from above is also uniform, and the standard deviation S of the area S of the concave curved surface 111 when viewed from above (Aa) can be obtained. σ 14.5μm 2In addition, the ratio of microcracks 112 with a depth less than the specified value is reduced, and the ratio of microcracks 112 with a depth greater than the specified value is increased, so that (C) the average value H of the depth H of the concave surface 111 can be obtained. AVE The anti-glare surface has a thickness of 0.10 μm or more.

[0080] The particles are pre-classified so that the coefficient of variation d CV The method of classification is not particularly limited, and examples thereof include classification using a sieve, gravity classification (horizontal flow, vertical upwelling), inertial force field classification (linear, curved, inclined), centrifugal force field classification (free vortex eddy current, forced vortex eddy current), etc.

[0081] The particle size distribution of the particles contained in the slurry is measured, for example, using a resistive particle size distribution measuring device Multisizer 4e manufactured by Beckman Coulter. The particle size distribution obtained using the above-mentioned particle size distribution measuring device is a particle size distribution obtained as follows: based on the so-called "Coulter principle", the impedance change caused by each particle in the electrolyte solution passing through the measuring part is directly detected, the particle size of each particle is measured one by one as a sphere-converted particle size, and then the number distribution is arranged as a cumulative histogram (or cumulative frequency curve) with the particle size as the horizontal axis and the number (frequency) as the vertical axis. Average particle size d AVE The so-called arithmetic mean diameter is calculated from the number distribution.

[0082] The number of microcracks 112 per unit area can be adjusted by the scanning speed or scanning number of the nozzle. The scanning number is the number of times the beam from the nozzle passes through the same position on the glass surface. The number of microcracks 112 per unit area is adjusted so that the number N of concave curved surfaces 111 per predetermined area when viewed from above is 250 or more / 100 μm square of the anti-glare surface.

[0083] The depth of the microcracks 112 can be adjusted by the material of the particles and the particle size d, as well as by the injection pressure or the projection distance. The injection pressure (gas pressure) is preferably 0.10 MPa to 2.00 MPa, more preferably 0.15 MPa to 0.50 MPa. The projection distance (the distance between the nozzle and the glass plate) is preferably 10 mm to 50 mm, more preferably 20 mm to 40 mm.

[0084] Step S102 includes performing a wet etching process on at least a portion of the first main surface 11 of the glass plate 1. The wet etching process is a process of supplying an etching solution containing an acid or an alkali to the first main surface 11 of the glass plate 1 to form a concave curved surface 111 with the microcrack 112 as a starting point. The etching solution can be supplied by an immersion method in which the glass plate is immersed in the etching solution, or by a spray method in which the etching solution is applied to the glass plate. Compared with the dry etching process, the wet etching process can etch the glass isotropically.

[0085] The etching liquid is, for example, a solution containing an acid. The acid concentration in the etching liquid is preferably 1% to 15% by mass, and particularly preferably 3% to 10% by mass. As the acid, for example, hydrogen fluoride is used. A combination of hydrogen fluoride and hydrogen chloride may also be used.

[0086] When the etching liquid is a solution containing an acid, etching is preferably performed at a temperature of 10° C. to 40° C., preferably 15° C. to 35° C., for 2 to 20 minutes.

[0087] When the etching solution is a solution containing an acid, the etching rate is preferably 0.5 μm / min or more, more preferably 1.0 μm / min or more, and further preferably 2.0 μm / min or more from the viewpoint of fully ensuring the anti-glare effect. The etching rate is preferably 20 μm / min or less.

[0088] The etching solution may also be a solution containing an alkali. The alkali concentration in the etching solution is preferably 1% to 50% by mass, preferably 3% to 50% by mass. As the alkali, for example, at least one alkali selected from sodium hydroxide, potassium hydroxide, potassium carbonate and sodium carbonate is used. These alkalis may be used alone or in combination.

[0089] The etching solution preferably contains a chelating agent in addition to an alkali. The chelating agent inhibits the recrystallization of the glass by forming a chelate with metal ions of the glass dissolved in the etching solution. The content of the chelating agent in the etching solution is preferably 0.1 mol / L or more and 0.5 mol / L or less. As the chelating agent, for example, ethylenediaminetetraacetic acid (EDTA), citric acid, gluconic acid, succinic acid, oxalic acid, tartaric acid or hydroxyethylidene diphosphonic acid (HEDP) can be used.

[0090] When the etching solution is a solution containing an alkali, etching is preferably performed at a temperature of 65° C. to 150° C., preferably 80° C. to 150° C. for 20 minutes to 40 hours.

[0091] When the etching solution is a solution containing an alkali, the etching rate is preferably 0.05 μm / min or more, more preferably 0.10 μm / min or more, and further preferably 0.15 μm / min or more, from the viewpoint of sufficiently ensuring the anti-glare effect. The etching rate is preferably 1.50 μm / min or less.

[0092] Example

[0093] The following will describe the experimental data. Examples 1 to 10 are examples, and Examples 11 to 13 are comparative examples.

[0094] [Example 1]

[0095] In Example 1, the first main surface of the glass plate was subjected to wet blasting, wet etching, and chemical strengthening in sequence to produce an anti-glare glass. As the glass plate, a Dragontrail (registered trademark) manufactured by AGC Corporation was prepared. The glass plate had a size of 100 mm×100 mm and a thickness of 1.0 mm.

[0096] In the wet blasting treatment, a wet blasting device (manufactured by Moko Co., Ltd., device name: Jr. Type II) was used. The slurry was prepared by mixing ceramic particles, a dispersing aid, and water as a dispersing medium. The content of ceramic particles in the entire slurry (slurry concentration) was 1.1% by weight. The ceramic particles were obtained by classifying white alumina (particle size #4000) manufactured by FUJIMI INCORPORATED. The average particle size d of the ceramic particles was AVE is 2.64 μm, and the coefficient of variation d CV The spray pressure (air pressure) of the slurry was 0.25 MPa, the projection distance (the distance between the nozzle and the glass plate) was 30 mm, the scanning speed of the nozzle was 200 mm / sec, and the number of scanning times of the nozzle was 20 times. The slurry was sprayed together with compressed air. In Example 1, the air pressure refers to the pressure of the compressed air. After the wet blasting and before the wet etching, pure water cleaning and drying were performed.

[0097] In the wet etching process, the glass plate was immersed in an etching solution at 25° C. for 286 seconds, thereby etching the first main surface of the glass plate by 15.9 μm. The second main surface of the glass plate was protected by a pre-bonded acid-resistant protective film. The etching solution was an aqueous solution containing 5% by mass of hydrogen fluoride and 5% by mass of hydrogen chloride. The protective film was peeled off after the wet etching process and before the chemical strengthening process.

[0098] In the chemical strengthening treatment, the glass plate is immersed in a molten salt of potassium nitrate heated to 450°C for 1 hour. Then, the glass plate is lifted out of the molten salt and slowly cooled to room temperature over 1 hour. Thus, a compressive stress layer is formed on both the first main surface and the second main surface of the glass plate.

[0099] [Example 2]

[0100] In Example 2, the average particle size d AVE is 2.22 μm and the coefficient of variation d CV Anti-glare glass was produced under the same conditions as in Example 1, except that the glass plate was immersed in an etching solution at 25°C for 240 seconds in a wet etching process to etch the first main surface of the glass plate by 13.6 μm.

[0101] [Example 3]

[0102] In Example 3, an anti-glare glass was produced under the same conditions as in Example 1, except that the glass plate was immersed in an etching solution at 25° C. for 436 seconds in the wet etching process to etch the first main surface of the glass plate by 23.4 μm.

[0103] [Example 4]

[0104] In Example 4, the average particle size d AVE is 2.22 μm and the coefficient of variation d CV Anti-glare glass was produced under the same conditions as in Example 1, except that the glass plate was immersed in an etching solution at 25°C for 360 seconds in a wet etching process to etch the first main surface of the glass plate by 20.6 μm.

[0105] [Example 5]

[0106] In Example 5, the average particle size d AVE is 3.04 μm and the coefficient of variation d CVAn anti-glare glass was produced under the same conditions as in Example 1, except that the glass plate was immersed in an etching solution at 25°C for 360 seconds in a wet etching process to etch the first main surface of the glass plate by 20.8μm.

[0107] [Example 6]

[0108] In Example 6, an anti-glare glass was produced under the same conditions as in Example 5, except that the glass plate was immersed in an etching solution at 25° C. for 480 seconds in the wet etching process to etch the first main surface of the glass plate by 27.2 μm.

[0109] [Example 7]

[0110] In Example 7, anti-glare glass was produced under the same conditions as in Example 5, except that the slurry concentration was 1.1 wt %, the nozzle was scanned 20 times, and the glass plate was immersed in an etching solution at 25° C. for 360 seconds in a wet etching process to etch the first main surface of the glass plate by 19.7 μm.

[0111] [Example 8]

[0112] In Example 8, an anti-glare glass was produced under the same conditions as in Example 7, except that the glass plate was immersed in an etching solution at 25° C. for 480 seconds in the wet etching process to etch the first main surface of the glass plate by 25.3 μm.

[0113] [Example 9]

[0114] In Example 9, the average particle size d AVE is 3.01 μm and the coefficient of variation d CV An anti-glare glass was produced under the same conditions as in Example 1, except that the glass plate was immersed in an etching solution at 25° C. for 480 seconds in a wet etching process to etch the first main surface of the glass plate by 26.3 μm.

[0115] [Example 10]

[0116] In Example 10, the average particle size d AVE is 2.06 μm and the coefficient of variation d CVAnti-glare glass was produced under the same conditions as in Example 1, except that the glass plate was immersed in an etching solution at 25°C for 480 seconds in a wet etching process to etch the first main surface of the glass plate by 24.9 μm.

[0117] [Example 11]

[0118] In Example 11, the first main surface of the glass plate was subjected to frosting, wet etching, and chemical strengthening in sequence to produce an anti-glare glass. As a glass plate, a Dragontrail (registered trademark) manufactured by AGC Corporation was prepared. The glass plate had a size of 100 mm×100 mm and a thickness of 1.0 mm.

[0119] In the frosting treatment, the glass plate was immersed in a chemical liquid at 25° C. for 3 minutes. The second main surface of the glass plate was protected by a pre-attached acid-resistant protective film. The chemical liquid was an aqueous solution containing 8 wt % hydrogen fluoride and 8 wt % potassium fluoride. After the frosting treatment and before the wet etching treatment, pure water washing and drying were performed.

[0120] In the wet etching treatment, the glass plate was immersed in an etching solution at 25° C. for 3 minutes. The second main surface of the glass plate was continuously protected by the acid-resistant protective film. The etching solution was an aqueous solution containing 10 wt % of hydrogen fluoride. The protective film was peeled off after the wet etching treatment and before the chemical strengthening treatment.

[0121] In the chemical strengthening treatment, the glass plate is immersed in a molten salt of potassium nitrate heated to 450°C for 1 hour. Then, the glass plate is lifted out of the molten salt and slowly cooled to room temperature over 1 hour. Thus, a compressive stress layer is formed on both the first main surface and the second main surface of the glass plate.

[0122] [Example 12]

[0123] In Example 12, the average particle size d AVE is 4.74 μm and the coefficient of variation d CV Anti-glare glass was produced under the same conditions as in Example 1, except that ceramic particles with a thickness of 0.483 (Macoho Beads (Product No.: AX-3-15) manufactured by Macoho Co., Ltd.) were used and the first main surface of the glass plate was etched by 20.3 μm by immersing the glass plate in an etching solution at 25° C. for 360 seconds in a wet etching process.

[0124] [Example 13]

[0125] In Example 13, an anti-glare glass was produced under the same conditions as in Example 12, except that the glass plate was immersed in an etching solution at 25° C. for 480 seconds in the wet etching process to etch the first main surface of the glass plate by 27.2 μm.

[0126] [Summarize]

[0127] The treatment conditions and treatment results of Examples 1 to 13 are shown in Table 1. In addition, the particle size distribution of the aluminum oxide particles used in the wet blasting treatment of Examples 1 to 10 and Examples 12 to 13 is shown in Table 1. Figure 5 In addition, the surface shapes of the anti-glare surfaces of Examples 1 to 13 were measured using a laser microscope VK-X260 manufactured by Keyence Corporation and analyzed using image analysis software SPIP (registered trademark) version 5.1.11 manufactured by Image Metrology Corporation. The results are shown in FIG. Figure 6 to Figure 9 middle. Figure 6 to Figure 9 The image shown in is an image obtained by photographing a rectangular area (long side length: 94.9 μm, short side length: 71.2 μm). Figure 6 to Figure 9 In the figure, the surface shape (height difference) of the anti-glare surface is expressed in grayscale. Figure 6 to Figure 9 The lower the brightness, the lower the height.

[0128] [Table 1]

[0129]

[0130] As shown in Table 1, unlike Examples 12 to 13, in Examples 1 to 10, the average particle size d AVE is 2.00 μm or more and the coefficient of variation d CV Wet sandblasting and wet etching of slurry with particles of 0.400 or less. Figure 5 As shown, the variation in the particle size of the aluminum oxide particles in Examples 1 to 10 is smaller than that in Examples 12 to 13. In Example 11, wet blasting was not performed.

[0131] As a result, unlike the anti-glare surfaces of Examples 11 to 13, the anti-glare surfaces of Examples 1 to 10 had (A)S σ 32.5μm 2 Below, (B) N is 250 or more / 100μm square, (C) H AVE is 0.10 μm or more, and (D) H σ 0.220μm or less, H AVE ×H σ 0.085μm 2Therefore, unlike the anti-glare surfaces of Examples 11 to 13, the anti-glare surfaces of Examples 1 to 10 have a glare index value Sp of 4.6% or less and an anti-glare index value D of 0.10 or more.

[0132] As shown in Table 1, unlike Examples 9 and 10, in Examples 1 to 8, the average particle size d AVE is 2.00 μm or more and the coefficient of variation d CV Wet sandblasting and wet etching of slurry with particles of 0.250 or less. Figure 5 As shown, in Examples 1 to 8, the variation in the particle size of the aluminum oxide particles is smaller than in Examples 9 and 10.

[0133] As a result, unlike the anti-glare surfaces of Examples 9 to 10, the anti-glare surfaces of Examples 1 to 8 had (Aa)S σ 14.5μm 2 Below, (Ba)N is 450 or more / 100μm square, (C)H AVE 0.10 μm or more, and (Da) H σ 0.180μm or less, H AVE ×H σ 0.070μm 2 Therefore, unlike the anti-glare surfaces of Examples 9 to 10, the anti-glare surfaces of Examples 1 to 8 have a glare index value Sp of 4.0% or less and an anti-glare index value D of 0.10 or more.

[0134] The glass plate and the method for manufacturing the glass plate of the present disclosure are described above, but the present disclosure is not limited to the above-mentioned embodiments, etc. Various changes, corrections, substitutions, additions, deletions and combinations can be made within the scope of the claims, which of course also belong to the technical scope of the present disclosure.

[0135] This application claims the priority based on Japanese Patent Application No. 2022-075351 filed with the Japan Patent Office on April 28, 2022, and all the contents of Japanese Patent Application No. 2022-075351 are incorporated herein by reference.

[0136] Description of symbols

[0137] 1 Glass Pane

[0138] 11. First main surface

[0139] 111 Concave surface

[0140] 12 Second main surface

Claims

1. A glass plate, comprising a first main surface and a second main surface facing opposite to the first main surface, wherein the first main surface comprises an anti-glare surface, the anti-glare surface comprises a plurality of concave surfaces in a spoon-cut shape, wherein: When the surface shape of the anti-glare surface is measured by a laser microscope, and the anti-glare surface is decomposed into a plurality of concave surfaces by a watershed algorithm based on the measurement result, the anti-glare surface satisfies: The standard deviation S of the area S of the concave surface when viewed from above σ 32.5μm 2 the following, The number N of the concave curved surfaces per predetermined area in a plan view is 250 or more / 100 μm square, The average value H of the depth H of the concave surface AVE 0.10μm or more, The standard deviation H of the depth H σ 0.220μm or less, The average value H of the depth H AVE The standard deviation H σ The product of H AVE ×H σ 0.085μm 2 the following.

2. The glass sheet according to claim 1, wherein The average value S of the area S of the anti-glare surface AVE 6μm 2 Above and 33μm 2 the following.

3. The glass sheet according to claim 1 or 2, wherein: The anti-glare surface has a glare index value Sp of 4.6% or less, an anti-glare index value D of 0.10 or more, Glare index value Sp: The pixel pattern attached to SMS-1000 manufactured by D&MS as a photomask is set on the light-emitting surface of the backlight source with its pattern surface facing upward, and then the glass plate is set on the pattern surface of the photomask with the first main surface facing upward. In a state where a green monochrome image display composed of RGB (0, 255, 0) is simulated by setting the photomask on the light-emitting surface of the backlight source whose luminous color is green, a 190 dpi area of ​​the pattern surface of the photomask is photographed through the glass plate using a camera of a measuring device SMS-1000 manufactured by DM&S. The flash point value obtained by image analysis of the measuring device is Sp. The distance between the shading plate installed on the camera and the glass plate is 262 mm. The lens of the camera uses a 23FM50SP lens with an aperture of 5.6 and a focal length of 50 mm; Anti-glare index value D: Using the measuring device arranged opposite to the first main surface of the glass plate, a white light source of a cold cathode tube arranged at a rectangular slit of 101 mm in length and 1 mm in width on a black flat plate irradiates the glass plate at an incident angle of 5.7°, and the brightness of the reflected light is measured. The lens of the camera of the measuring device uses a C1614A lens with an aperture of 5.6 and a focal length of 16 mm. The distance from the first main surface of the glass plate to the lens of the camera is 300 mm, and the image is formed. The scaling ratio is set in the range of 0.0276 to 0.0278, and D is calculated by the formula "D = (D2 + D3) / (2 × D1)" when the difference Δθ between the reflection angle θr and the incident angle θi (Δθ = θr - θi) is in the range of 0.0° ± 0.1° and the average value of the brightness of the reflected light is set to D1, the average value of the brightness of the reflected light is set to D2 when Δθ is in the range of 0.5° ± 0.1° and the average value of the brightness of the reflected light is set to D3 when Δθ is in the range of -0.5° ± 0.1°.

4. A method for manufacturing a glass plate, wherein the glass plate has a first main surface and a second main surface facing opposite to the first main surface, the first main surface includes an anti-glare surface, the anti-glare surface has a plurality of concave surfaces in a spoon-cut shape, wherein: The method for manufacturing the glass sheet comprises the following steps: Use the average value d including the particle size d AVE The coefficient of variation of the particle size d is 2.00 μm or more. CV wet blasting at least a portion of the first main surface with a slurry of particles having a (coefficient of variation = standard deviation / average value) of 0.400 or less; and After the wet blasting, at least a portion of the first main surface is wet-etched using an etching solution containing an acid or an alkali.

5. The method for manufacturing a glass plate according to claim 4, wherein: The average particle size d of the particles is AVE It is 2.00 μm or more and 4.50 μm or less.

6. The method for manufacturing a glass plate according to claim 4 or 5, wherein: The particles have a Mohs hardness higher than that of the glass sheet.

7. A glass plate, comprising a first main surface and a second main surface facing opposite to the first main surface, wherein the first main surface comprises an anti-glare surface, the anti-glare surface comprises a plurality of concave surfaces in a spoon-cut shape, wherein: When the surface shape of the anti-glare surface is measured by a laser microscope, and the anti-glare surface is decomposed into a plurality of concave surfaces by a watershed algorithm based on the measurement result, the anti-glare surface satisfies: The standard deviation S of the area S of the concave surface when viewed from above σ 14.5μm 2 the following, The number N of the concave curved surfaces per predetermined area in a plan view is 450 or more / 100 μm square, The average value H of the depth H of the concave surface AVE 0.10μm or more, The standard deviation H of the depth H σ 0.180μm or less, The average value H of the depth H AVE The standard deviation H σ The product of H AVE ×H σ 0.070μm 2 the following.

8. The glass sheet according to claim 7, wherein: The average value S of the area S of the anti-glare surface AVE 6μm 2 Above and 17μm 2 the following.

9. The glass sheet according to claim 7 or 8, wherein: The anti-glare surface has a glare index value Sp of 4.0% or less, an anti-glare index value D of 0.10 or more, Glare index value Sp: The pixel pattern attached to SMS-1000 manufactured by D&MS as a photomask is set on the light-emitting surface of the backlight source with its pattern surface facing upward, and then the glass plate is set on the pattern surface of the photomask with the first main surface facing upward. In a state where a green monochrome image display composed of RGB (0, 255, 0) is simulated by setting the photomask on the light-emitting surface of the backlight source whose luminous color is green, a 190 dpi area of ​​the pattern surface of the photomask is photographed through the glass plate using a camera of a measuring device SMS-1000 manufactured by DM&S. The flash point value obtained by image analysis of the measuring device is Sp. The distance between the shading plate installed on the camera and the glass plate is 262 mm. The lens of the camera uses a 23FM50SP lens with an aperture of 5.6 and a focal length of 50 mm; Anti-glare index value D: Using the measuring device arranged opposite to the first main surface of the glass plate, a white light source of a cold cathode tube arranged at a rectangular slit of 101 mm in length and 1 mm in width on a black flat plate irradiates the glass plate at an incident angle of 5.7°, and the brightness of the reflected light is measured. The lens of the camera of the measuring device uses a C1614A lens with an aperture of 5.6 and a focal length of 16 mm. The distance from the first main surface of the glass plate to the lens of the camera is 300 mm, and the image is formed. The scaling ratio is set in the range of 0.0276 to 0.0278, and D is calculated by the formula "D = (D2 + D3) / (2 × D1)" when the difference Δθ between the reflection angle θr and the incident angle θi (Δθ = θr - θi) is in the range of 0.0° ± 0.1° and the average value of the brightness of the reflected light is set to D1, the average value of the brightness of the reflected light is set to D2 when Δθ is in the range of 0.5° ± 0.1° and the average value of the brightness of the reflected light is set to D3 when Δθ is in the range of -0.5° ± 0.1°.

10. A method for manufacturing a glass plate, the glass plate comprising a first main surface and a second main surface facing opposite to the first main surface, the first main surface comprising an anti-glare surface, the anti-glare surface comprising a plurality of concave surfaces in a spoon-cut shape, wherein: The method for manufacturing the glass sheet comprises the following steps: Use the average value d including the particle size d AVE The coefficient of variation of the particle size d is 2.00 μm or more. CV wet blasting at least a portion of the first main surface with a slurry of particles having a (coefficient of variation = standard deviation / average value) of 0.250 or less; and After the wet blasting, at least a portion of the first main surface is wet-etched using an etching solution containing an acid or an alkali.

11. The method for manufacturing a glass plate according to claim 10, wherein: The average particle size d of the particles is AVE It is 2.00 μm or more and 4.50 μm or less.

12. The method for manufacturing a glass plate according to claim 10 or 11, wherein: The particles have a Mohs hardness higher than that of the glass sheet.

Citation Information

Patent Citations

  • Anti-glare surface treatment method and articles thereof

    CN102869629A

  • Anti-glare surface treatment method and articles thereof

    CN103534219A

  • Method for Processing Surface of Light-Transmitting Glass and Light-Transmitting Glass Processed by said Method

    CN104230172A

  • Glass plate and display device

    CN110054418A

  • Glass plate, glass plate having Anti-reflection layer, and method for producing glass plate