Compositions and methods for inhibiting tungsten etch
By using specific compositions under acidic conditions, including surface-modified colloidal silica particles and other corrosion inhibitors, the selective removal of tungsten and cobalt is solved, achieving the stability of tungsten and cobalt during efficient chemical mechanical polishing Removal and high surface quality.
Patent Information
- Application Number
- CN202380031816.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to selectively remove tungsten and cobalt under acidic conditions while maintaining high surface quality, especially in chemical mechanical polishing processes, with undesirable etching problems.
Compositions containing surface-modified colloidal silica particles, guanidine derivative corrosion inhibitors, polyacrylamide corrosion inhibitors, iron (III) oxidants and silica phosphate removal rate enhancers are ensured by combining aqueous media. Stability and high selective removal efficiency in a specific pH range.
High selective removal of tungsten and cobalt is achieved, prevents undesired etching, maintains high surface quality and colloidal stability, and is suitable for chemical mechanical polishing processes in semiconductor manufacturing.
Smart Images

Figure BDA0005066809210000081 
Figure BDA0005066809210000151 
Figure BDA0005066809210000361
Abstract
Description
Technical Field
[0001] The invention claimed herein relates to compositions and methods for polishing dielectrics. The invention claimed herein particularly relates to compositions and methods that provide high selectivity for the removal of dielectrics relative to tungsten. Background Art
[0002] The manufacture of integrated circuits (ICs) is a multi-step process. The first step (also known as the front-end or FEOL step) involves patterning a single device such as a transistor (e.g., C-MOSFET) on a semiconductor by a suitable technique such as photolithography or ion implantation. Metal wires / plugs and insulating layers (such as dielectrics) are then inserted to interconnect the individual devices (also known as the back-end or BEOL step). With the continuous reduction of feature sizes in ultra-large-scale integrated circuit (ULSI) technology, it is necessary to form multi-level interconnections.
[0003] Metals such as tungsten, cobalt, ruthenium, and copper are commonly used as connectors, and the choice of a particular metal is made based on its location in the construction. For example, a common first metal interconnect (metal layer 0) is a tungsten plug inserted into a dielectric layer (such as silicon dioxide). On the other hand, during the BEOL steps, copper is the most commonly deposited metal, but for lower interconnect levels (e.g., metal layers 1-4), tungsten and cobalt are commonly used.
[0004] It has been found that CMP (chemical mechanical planarization) is the key technology that enables multi-level interconnect formation, because it can initiate local and global planarization and at the same time provide good surface quality, i.e. an excellent mirror-like defect-free surface finish. Pure mechanical polishing or (fine) grinding will provide excellent planarization, but the surface will become dull. On the other hand, pure chemical polishing (anisotropic etching) will only provide poor planarization results, but provide an excellent mirror-like surface finish.
[0005] In this context, CMP utilizes the interaction of chemical and mechanical action to achieve the desired flatness and finish of the surface to be polished. The mechanical action is usually carried out by the interaction of a CMP composition containing finely dispersed abrasives and a polishing pad, which is typically pressed onto the surface to be polished and mounted on a moving platen. In a typical CMP process step, a rotating wafer holder brings the wafer to be polished into contact with the polishing pad. The CMP composition is usually applied between the wafer to be polished and the polishing pad.
[0006] Typical CMP compositions or slurries contain one or more abrasive (insoluble / dispersed) components and soluble components. The chemical action is provided by the soluble components of the CMP composition. Typically, in order to achieve metal CMP, the chemical composition is usually customized by balancing the corrosion components (e.g., acids, bases, or oxidants) with suitable inhibitors. However, it is important that the soluble and insoluble components are compatible to ensure colloidal stability. Colloidal unstable solutions or aggregates may damage the surface and fine structure of the wafer to be polished by scratching. Therefore, in order to obtain suitable planarization and surface quality, accurate selection of components and their concentrations is necessary to obtain a suitable CMP composition.
[0007] Furthermore, when designing the slurry, the characteristics (e.g., etching) of several or all of the above metals may have to be considered, depending on the integration scheme. For example, when manufacturing an IC involving tungsten (metal 0), CMP is employed to remove the metal and liner / barrier capping layers until a flat metal 0 (or higher) layer is exposed.
[0008] For example, US Pat. No. 6,083,419A describes a CMP composition comprising a compound capable of etching tungsten, at least one tungsten etching inhibitor, wherein the tungsten etching inhibitor is a compound comprising at least one functional group selected from the following: a nitrogen-containing heterocycle without nitrogen-hydrogen bonds, a sulfide, an oxazolidine, or a mixture of these functional groups.
[0009] In the case of, for example, US6,083,419A, since the intended endpoint for such applications is a dielectric (e.g., a silicon oxide layer obtained by CVD deposition with tetraethyl orthosilicate or TEOS), the prior art slurries are tailored to achieve a high removal rate of tungsten relative to silicon oxide. For example, US2019 / 0211227 and US2019 / 0211228 aim to achieve high selectivity for tungsten removal by employing surface-modified colloidal silica particles with a negative charge.
[0010] On the other hand, in order to realize new integration schemes, it is very necessary to selectively remove dielectrics. US 8,492,277 provides a polishing method, which involves using a composition comprising an acyclic organic sulfonic acid to provide selective high removal rates for silicon oxide and silicon nitride. US 8,513,126 achieves similar results using a composition comprising a quaternary ammonium salt. However, in the presence of metals (such as tungsten and cobalt) that are easily removed under acidic conditions, there is an unmet need for obtaining compositions and methods that allow for the removal of dielectrics with high selectivity relative to tungsten and / or cobalt while maintaining high surface quality. Summary of the invention
[0011] Surprisingly, it has been discovered that the compositions of the presently claimed invention, as described below, provide unexpectedly high selectivity for the removal of dielectrics relative to tungsten.
[0012] Thus, in one aspect of the invention claimed herein, a dielectric polishing composition comprising:
[0013] (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge,
[0014] a particle size of 60 nm to 200 nm, and a zeta potential of < -35 mV at a pH ranging from ≥2.0 to ≤4.5;
[0015] (B) a first corrosion inhibitor selected from at least one guanidine derivative;
[0016] (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers;
[0017] (D) at least one iron(III) oxidizing agent;
[0018] (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts;
[0019] (F) at least one stabilizer; and
[0020] (G) an aqueous medium,
[0021] The pH of the composition is in the range of ≥2.0 to ≤4.5.
[0022] In another aspect, the invention claimed herein relates to a method for manufacturing a semiconductor device, the method comprising chemically mechanically polishing a substrate (S) used in the semiconductor industry in the presence of a composition as described herein, the substrate (S) comprising
[0023] (i) Tungsten and / or
[0024] (ii) tungsten alloys; and
[0025] (iii) at least one dielectric layer selected from silicon, silicon oxide, silicon nitride, or a low-k material.
[0026] In another aspect, the invention claimed herein relates to the use of the composition described herein for polishing a substrate (S) comprising: (i) tungsten and / or (ii) a tungsten alloy; and (iii) at least one dielectric layer.
[0027] The invention claimed herein is associated with at least one of the following objects:
[0028] (1) The compositions and methods of the invention claimed herein are intended to provide selective removal of dielectric layers relative to other metals (eg, tungsten and / or cobalt).
[0029] (2) The compositions and methods of the invention claimed herein are intended to provide high silicon oxide (SiO2) and silicon nitride (SiN) removal rates while ensuring low W removal rates.
[0030] (3) The compositions and methods of the invention claimed herein are directed to preventing unwanted tungsten etching during chemical mechanical polishing of tungsten-containing substrates.
[0031] (4) The compositions and methods of the invention claimed herein are directed to preventing unwanted cobalt etching during chemical mechanical polishing of cobalt-containing substrates.
[0032] (5) The compositions of the invention claimed herein are intended to provide stable formulations or dispersions in which no phase separation or agglomeration occurs.
[0033] (6) The compositions of the invention claimed herein are intended to provide suitable dielectric removal rates while preventing undesirable surface defects and ensuring high surface quality.
[0034] Other objects, advantages and applications of the invention claimed herein will become apparent to those skilled in the art from the following detailed description. DETAILED DESCRIPTION
[0035] The following detailed description is merely exemplary in nature and is not intended to limit the invention claimed herein or the application and use of the invention claimed herein. In addition, it is not intended to be bound by any theory presented in the foregoing technical field, background technology, summary of the invention or the following detailed description.
[0036] As used herein, the terms "comprising" or "comprises" and "comprised of" are synonymous with "including" or "includes" or "containing" and are inclusive or open-ended and do not exclude additional unrecited members, elements, or method steps. It should be understood that, as used herein, the terms "comprising" or "comprises" and "comprised of" encompass the terms "consisting of" or "consists of" and "consists".
[0037] In addition, the terms "(a)", "(b)", "(c)", "(d)", etc. in the specification and claims are used to distinguish similar elements and are not necessarily used to describe a sequential order or a chronological order. It should be understood that the terms so used are interchangeable where appropriate, and that the embodiments of the inventions described herein and claimed herein are capable of operating in other sequences than those described or shown herein. If the terms "(A)", "(B)" and "(C)" or "(a)", "(b)", "(c)", "(d)", "(i)", "(ii)", etc. refer to steps of a method or use or an assay, there is no temporal or temporal continuity between the steps, that is, the steps may be performed simultaneously or there may be a time interval of seconds, minutes, hours, days, weeks, months or even years between the steps, unless otherwise indicated in the application as described above or below.
[0038] In the following paragraphs, different aspects of the invention claimed herein are defined in more detail. Unless explicitly indicated to the contrary, each aspect so defined may be combined with any one or more other aspects. In particular, any feature indicated as preferred or advantageous may be combined with any one or more other features indicated as preferred or advantageous.
[0039] References throughout this specification to "one embodiment" or "an embodiment" or "a preferred embodiment" mean that a particular feature, structure, or property described in conjunction with that embodiment is included in at least one embodiment of the invention claimed herein. Thus, the phrases "in one embodiment" or "in an embodiment" or "in a preferred embodiment" that appear in different places throughout this specification do not necessarily all refer to the same embodiment, but may refer to the same embodiment. Furthermore, in one or more embodiments, as will be apparent to those skilled in the art from this disclosure, the features, structures, or properties may be combined in any suitable manner. Furthermore, although some embodiments described herein include some but not other features included in other embodiments, combinations of features of different embodiments are intended to be within the scope of this subject matter and to form different embodiments, as will be understood by those skilled in the art. For example, in the appended claims, any of the claimed embodiments may be used in any combination.
[0040] Furthermore, ranges defined throughout this specification also include the endpoints, ie, a range of 1 to 10 means that both 1 and 10 are included in the range. For the avoidance of doubt, the applicant shall be entitled to any equivalent means under applicable law.
[0041] For the purposes of the invention claimed herein, '% by weight' or 'wt.%' as used in the invention claimed herein is relative to the total weight of the coating composition. Additionally, as described below, the sum of the wt.% of all compounds in each component adds up to 100 wt.-%.
[0042] For purposes of the invention claimed herein, a substrate is defined as a semiconductor wafer made of silicon or similar semi-metals used to fabricate microelectronic devices.
[0043] For purposes of the invention claimed herein, polishing or cleaning refers to the chemical mechanical removal of a specific layer on a substrate during a CMP process. The mechanical action is usually performed by a polishing pad, which is typically pressed against the surface to be polished and mounted on a moving platen. In a typical CMP process step, a rotating wafer holder brings the wafer to be polished into contact with the polishing pad. The CMP composition is usually applied between the wafer to be polished and the polishing pad.
[0044] For purposes of the invention claimed herein, corrosion inhibitors are defined as compounds that form a protective molecular layer on metal surfaces.
[0045] For the purposes of the invention claimed herein, a stabilizer is defined as a compound that forms soluble complex molecules with iron (III) ions, deactivating these ions so that they cannot normally react with other elements or ions (such as phosphate) to produce precipitation or scale. In the absence of a stabilizer, as claimed herein, an undesirable interaction between the iron (III) oxidizer and the silicon-based composition was found, resulting in colloidal instability of the composition.
[0046] A lower dielectric constant can increase the frequency at which current can operate. Dielectric materials with lower dielectric constants used in metallization in IC production (primarily in BEOL) are called low-k materials (dielectric constant k, e.g., 3.5 or lower) or ultra-low-k materials (dielectric constant k, e.g., 2.5 and lower). Several low-k materials are available from Applied Materials under the trade name Black Diamond (see also generally US 6,974,777 B2 or Hosali et al., Analyzing damage from ultralow-k CMP, Solid State Technology, 48 (11) p. 33, 2005). A detailed description of methods for producing low-k materials and their deposition can be found in McClatchie et al., Low Dielectric Constant Oxide Films Deposited Using CVD Techniques, DUMIC Conference Proceedings, (1998), pp. 311 et seq. For purposes of the invention claimed herein, a low-k material is a material having a k value (dielectric constant) of less than 3.5, preferably less than 3.0, and more preferably less than 2.7. An ultra-low-k material is a material having a k value (dielectric constant) of less than 2.4.
[0047] For the purposes of the invention claimed herein, "colloidal silica" means silica that has been prepared by the polycondensation of Si(OH)4. The precursor Si(OH)4 can be obtained, for example, by hydrolysis of a high purity alkoxysilane or by acidifying an aqueous silicate solution. Such colloidal silica can be prepared according to U.S. Pat. No. 5,230,833 or can be obtained as any of a variety of commercially available products, such as PL-1, PL-2, and PL-3 products, and Nalco 1050, 2327 and 2329 products, and other similar products available from DuPont, Bayer, Applied Research, Nissan Chemical, Nyacol, and Clariant.
[0048] For the purposes of the invention claimed herein, "particle size" and "average particle size" are used interchangeably. The average particle size is defined as the particle size distribution of the colloidal silica particles (A) in the aqueous medium (G). 50 value.
[0049] For purposes of the invention claimed herein, the average particle size is measured, for example, using dynamic light scattering (DLS) or static light scattering (SLS) methods. These methods and others are well known in the art, see, for example, Kuntzsch, Timo; Witnik, Ulrike; Hollatz, Michael Stintz; Ripperger, Siegfried; Characterization of Slurries Used for Chemical-Mechanical Polishing (CMP) in the Semiconductor Industry; Chem. Eng. Technol; 26 (2003), Vol. 12, p. 1235. For such measurements, the literature commonly refers to secondary particle size. Of these methods, DLS is the preferred method.
[0050] For the purposes of the invention claimed herein, for dynamic light scattering (DLS), a Malvern Zetasizer ZSP or a Horiba LB-550V (DLS, dynamic light scattering measurement) or any other such instrument is typically used. This technique measures the hydrodynamic diameter of a particle when it scatters a laser light source (e.g. λ=650 nm), detected at an angle of, for example, 90° or 173° to the incident light. Changes in the intensity of the scattered light are due to the random Brownian motion of the particles as they pass through the incident light beam and are monitored as a function of time. The autocorrelation function performed by the instrument as a function of the delay time is used to extract the decay constant; smaller particles pass through the incident light beam at a higher speed and correspond to faster decays.
[0051] For the purposes of the invention claimed herein, the attenuation constant is related to the diffusion coefficient D of the inorganic abrasive particles. t is proportional to and is used to calculate particle size according to the Stokes-Einstein equation:
[0052]
[0053] It is assumed that the suspended particles: (1) have a spherical morphology and (2) are uniformly dispersed (i.e., not agglomerated) throughout the aqueous medium. This relationship is expected to apply to particle dispersions containing less than 1% solids by weight, since there is no significant deviation from the viscosity of the aqueous dispersant, where η = 0.96 mPa·s (at T = 22°C). The particle size distribution of fumed or colloidal silica particle dispersions is typically measured in plastic cuvettes at solids concentrations of 0.1% to 1.0% and, if necessary, diluted with dispersion medium or ultrapure water.
[0054] For the purposes of the invention claimed herein, the BET surface area of the colloidal silica particles is determined in accordance with DIN ISO 9277:2010-09. For this measurement result, the literature commonly refers to the primary particle size.
[0055] For the purposes of the invention claimed herein, an oxidizing agent is defined as a compound that can oxidize the substrate to be polished or one of its layers.
[0056] For the purposes of the invention claimed herein, a pH adjusting agent is defined as a compound added to a composition to adjust its pH to a desired value.
[0057] For purposes of the invention claimed herein, the disclosed measurement techniques are well known to those skilled in the art.
[0058] In aspects of the invention claimed herein, a dielectric polishing composition comprising:
[0059] (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge,
[0060] a particle size of 60 nm to 200 nm, and a zeta potential of <-35 mV at a pH in the range of ≥2.0 to ≤4.5; (B) a first corrosion inhibitor selected from at least one guanidine derivative;
[0061] (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers;
[0062] (D) at least one iron(III) oxidizing agent;
[0063] (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts;
[0064] (F) at least one stabilizer; and
[0065] (G) an aqueous medium,
[0066] The pH of the composition is in the range of ≥2.0 to ≤4.5.
[0067] The dielectric polishing composition of the present invention comprises components (A), (B), (C), (D), (E), (F) and water and optionally additional components as described below.
[0068] (A) Surface modified colloidal silica particles
[0069] According to the invention claimed herein, the composition comprises negatively charged groups on the surface of the particles, wherein the surface modified colloidal silica particles have a negative charge, a particle size of 60 nm to 200 nm, and a zeta potential of <-35 mV at a pH in the range of ≥2.0 to ≤4.5.
[0070] Well known silica selective compositions are typically known to use ceria, however, it was noted that said abrasive resulted in an unacceptably dull finish. Similar undesirable observations were noted when using fumed silica.
[0071] Preferably, the surface modified silica particles have a zeta potential of <-36 mV, more preferably <-37 mV, and most preferably <-38 mV at a pH in the range of ≥2.0 to ≤4.5.
[0072] Preferably, the surface modified silica particles have a zeta potential of >-50 mV, more preferably >-45 mV, and most preferably >-40 mV at a pH in the range of ≥2.0 to ≤4.5.
[0073] Preferably, the surface modified silica particles have a zeta potential of -50 mV to -35 mV, more preferably -45 mV to -35 mV, even more preferably -40 mV to -35 mV, and most preferably -39 mV to -35 mV at a pH in the range of ≥2.0 to ≤4.5.
[0074] The surface-modified silica particles are preferably amorphous and non-agglomerated, and thus typically exist in the form of discrete spheres that are not cross-linked to each other and contain hydroxyl groups on the surface. The surface-modified colloidal silica particles can be obtained by methods known in the art, such as ion exchange of silicates or by sol-gel techniques (e.g., hydrolysis or condensation of metal alkoxides, or peptization of precipitated hydrated silicon oxide, etc.).
[0075] It is known that silica particles can be stabilized by a permanent charge on their surface to prevent agglomeration and ensure colloidal stability. The charge can be positive or negative. Due to the defects observed on the surface when using positively charged (or cationic) silica particles (ref. Figure 2 b), so negative charge is considered essential. This is depicted in Figure 2In a defect-free surface, the substrate is planarized with a composition comprising negatively charged (or anionic) silica particles. The charge on the surface is represented by the zeta potential. The zeta potential of the silica particles (without surface functionalization) depends on the pH value of the aqueous medium (refer to Figure 1 ). At pH above 8, the zeta potential is equal to or lower than -35 mV, i.e., sufficiently low to ensure colloidal stability. Without being bound by theory, it is believed that at acidic pH (e.g., pH 2-4), the charge on the surface is reduced (zeta potential is typically, for example, between +10 and -10 mV) due to the interaction of silica with the protons of the medium. A typical correlation of zeta potential and pH can be found in the literature (Esumi et al., Bull. Chem. Soc. Jpn. [Bulletin of the Chemical Society of Japan], Vol. 61, 1988). Low surface charge may lead to the formation of agglomerates once shear forces are generated (e.g., by filtration or polishing), such as Figure 1 The zeta potential change of the unmodified silica particles in the reference is shown in FIG.
[0076] Preferably, the surface-modified colloidal silica particles (A) having a negative zeta potential of <-35 mV at a pH in the range of ≥2.0 to ≤4.5 are silica particles anion-modified with metallizing ions or modified with sulfonic acid.
[0077] As explained in WO 2006 / 028759 A2, the term "anionically modified with a metallizing ion" as used herein refers in particular to silica particles in which the metallizing ion (ie M(OH)4 - ) are incorporated into the surface of silica particles, replacing Si(OH)4 sites and generating a permanent negative charge.
[0078] Preferably, the surface modified colloidal silica particles (A) having a negative zeta potential of <-35 mV at a pH in the range of ≥2.0 to ≤4.5 are silica particles anionically modified with metallizing ions. More preferably, the metallizing ions are selected from aluminate, stannate, zincate, or plumbate.
[0079] Even more preferably, the surface modified colloidal silica particles (A) having a negative zeta potential of <-35 mV at a pH in the range of ≥2.0 to ≤4.5 are silica particles modified with aluminate anions. Such surface modified colloidal silica particles are disclosed, for example, in WO 2006 / 7028759A2.
[0080] More preferably, the surface-modified colloidal silica particles of component (A) having a negative zeta potential of <-35 mV at a pH in the range of ≥2.0 to ≤4.5 are silica particles modified with sulfonic acid anions. For example, sulfonic acid-modified aqueous anionic silica sols that are highly stable under acidic conditions are disclosed in WO 2010734542 A1. In this context, the sulfonic acid-modified aqueous anionic silica sol is obtained by a process in which a silane coupling agent having a functional group that can be chemically converted to a sulfonic acid group is chemically adsorbed onto the colloidal silica, and the functional group is then converted to a sulfonic acid group. A preferred type of silica dispersion for this type of chemical reaction is a silica dispersion having a sulfonic acid group similar to Figure 1 Silica dispersions (unmodified silica particles) as a function of the zeta potential, where the charge on the particle surface is low under acidic conditions. This is also considered a sign that the silica surface is clean and that the silane can easily react with groups on the silica surface. If the charge on the silica particles is already high (e.g. -36 or -50 mV) before reacting with the silane coupling agent under acidic conditions (e.g. pH 2-3), it is interpreted as a sign that the silica surface is not clean and has been modified. The silane coupling agent may not be able to adequately cover the surface and the charge on the surface may then remain low after the reaction and conversion. Surface-modified particle dispersions with a zeta potential of, for example, -23 mV may have low colloidal stability. This means that the dispersion may be easily destabilized by processes such as filtration or CMP, where shear forces occur. In this case, a filtered silica dispersion measured by a DLS method, such as with a Malvern Zetasizer ZSP, will provide a signal with a high variance (ref. Figure 3 ), which cannot be easily interpreted as an average particle size. Other methods (such as sedimentation) must be used to evaluate colloidal stability. On the other hand, it is noted that silica particles modified with sulfonic acid anions produce a stable DLS signal that is easy to measure (ref. Figure 4 ).
[0081] Preferably, the concentration of the surface-modified colloidal silica particles (A) is in the range of ≧0.01 wt. % to ≦13.0 wt. %, based on the total weight of the composition.
[0082] Based on the total weight of the composition, the concentration of the surface-modified colloidal silica particles (A) is preferably not more than 13.0 wt.%, more preferably not more than 10.0 wt.%, in particular not more than 8.0 wt.%, for example not more than 7.0 wt.%. It has been observed that a particle concentration of more than 10 wt.% can lead to colloidal instability of the composition. Based on the total weight of the composition, the concentration of the surface-modified colloidal silica particles (A) is preferably at least 0.01 wt.%, more preferably at least 0.1 wt.%, even more preferably at least 0.2 wt.%, in particular at least 0.3 wt.%, even more preferably at least 0.5 wt.%, still more preferably at least 0.8 wt.%, more preferably at least 1.0 wt.%, even more preferably at least 1.2 wt.%, still more preferably at least 1.5 wt.%, most preferably at least 1.8 wt.%. Based on the total weight of the composition, the concentration of the surface-modified colloidal silica particles (A) is more preferably in the range of ≥ 0.3 wt.% to ≤ 7.0 wt.%.
[0083] The surface-modified colloidal silica particles (A) may preferably be included in the composition in various particle size distributions. The particle size distribution of the surface-modified colloidal silica particles (A) may be unimodal or multimodal. In the case of a multimodal particle size distribution, a bimodal particle size distribution is generally preferred. For the purposes of the invention claimed herein, a unimodal particle size distribution is preferred for the surface-modified colloidal silica particles (A).
[0084] According to the invention claimed herein, the surface modified colloidal silica particles (A) have an average particle size in the range of 60 nm to 200 nm as determined according to dynamic light scattering techniques.
[0085] The mean or average particle size of the surface-modified colloidal silica particles (A) can vary within a wide range. The mean particle size of the surface-modified colloidal silica particles (A) is preferably in the range of ≥60 nm to ≤190 nm, preferably in the range of ≥60 nm to ≤180 nm, more preferably in the range of ≥62 nm to ≤150 nm, more preferably in the range of ≥65 nm to ≤130 nm, particularly preferably in the range of ≥70 nm to ≤120 nm, most preferably in the range of ≥80 nm to ≤100 nm, in each case measured with the dynamic light scattering technique using an instrument such as a Zetasizer ZSP from Malvern Instruments, Ltd. or a High Performance Particle Sizer (HPPS) or a Horiba LB550.
[0086] At least one inorganic abrasive particle (A) preferably can have various shapes.Therefore, particle (A) can preferably have one or substantially only one type of shape.However, particle (A) also may have different shapes.For example, there may be two types of particles (A) of different shapes.For example, (A) may have the shape of agglomerates, cubes, cubes with beveled edges, octahedrons, icosahedrons, cocoons, nodules or spheres, with or without projections or depressions.
[0087] Preferably, the surface-modified colloidal silica particles (A) are spherical, cocoon-shaped or a mixture of spherical and cocoon-shaped particles. Spherical particles may or may not have protrusions or depressions. Cocoon-shaped particles may or may not have protrusions or depressions. Cocoon-shaped particles are preferably particles with a minor axis of ≥10nm to ≤200nm and preferably a major axis / minor axis ratio of ≥1.4 to ≤2.2, more preferably ≥1.6 to ≤2.0. Preferably, they have an average shape factor of ≥0.7 to ≤0.97, more preferably ≥0.77 to ≤0.92, an average sphericity of preferably ≥0.4 to ≤0.9, more preferably ≥0.5 to ≤0.7, and an average equivalent circular diameter of preferably ≥41nm to ≤66nm, more preferably ≥48nm to ≤60nm, determined in each case by transmission electron microscopy and scanning electron microscopy.
[0088] Most preferably, the surface modified colloidal silica particles (A) are spherical or substantially spherical. The ratio of the major axis / minor axis of the spherical or substantially spherical particles is ≥ 0.9.
[0089] For the purposes of the invention claimed herein, the determination of the shape factor, sphericity and equivalent circular diameter of cocoon-shaped particles is explained below. The shape factor gives the shape and concavity information of a single particle and can be calculated according to the following formula:
[0090] Shape factor = 4π(area / perimeter2)
[0091] A spherical particle with no indentations has a shape factor of 1. As the number of indentations increases, the value of the shape factor decreases. Sphericity gives information about the elongation of individual particles using moments about the mean and can be calculated according to the following formula, where M is the center of gravity of the respective particle:
[0092] Sphericity=(Mxx-Myy)-[4Mxy2+(Myy-Mxx)2]0.5 / (Mxx-Myy)+[4Mxy2+(Myy-Mxx)2]0.5
[0093] Elongation = (1 / sphericity) 0.5
[0094] in
[0095] Mxx=Σ(xx average)2 / N
[0096] Myy=Σ(yy average) 2 / N
[0097] Mxy=Σ[(xx average)*(yy average)] / N
[0098] N is the number of pixels that form the corresponding particle image.
[0099] x,y pixel coordinates
[0100] x average forms the average value of the x coordinates of N pixels of the particle image
[0101] y average is the average of the y coordinates of the N pixels forming the particle image
[0102] The sphericity of a spherical particle is 1. When the particle is elongated, the value of the sphericity decreases. The equivalent circular diameter (hereinafter also abbreviated as ECD) of an individual non-circular particle gives information on the diameter of a circle having the same area as the corresponding non-circular particle. The average shape factor, average sphericity and average ECD are the arithmetic means of the corresponding properties related to the number of particles analyzed.
[0103] For the purpose of the invention claimed herein, the procedure for particle shape characterization is as follows. An aqueous cocoon-shaped silica particle dispersion with a solid content of 20 wt.% is dispersed on a carbon foil and dried. The dried dispersion is analyzed by using an energy-filtered transmission electron microscope (EF-TEM) (120 kV) and a scanning electron microscope secondary electron image (SEM-SE) (5 kV). An EF-TEM image with a resolution of 2k, 16 bits, and 0.6851 nm / pixel is used for analysis. After noise suppression, the image is binary encoded using a threshold. Afterwards, these particles are manually separated. The particles covered and on the edge are distinguished and not used for analysis. The ECD, shape factor, and sphericity as defined previously are calculated and statistically classified.
[0104] (B) First Corrosion Inhibitor
[0105] According to the invention claimed herein, the composition comprises at least one first corrosion inhibitor selected from at least one guanidine derivative.
[0106] As can be seen from Table 1 below, the first corrosion inhibitor selected from at least one guanidine derivative prevents undesirable corrosion of tungsten while promoting high dielectric removal rates (both silicon oxide and silicon nitride).
[0107] Preferably, the at least one guanidine derivative is selected from buformin, phenformin, guanine, proguanil hydrochloride, 2-guanidinobenzimidazole, polyhexamethylene biguanide hydrochloride, polyaminopropyl biguanide, arginine, chlorhexidine or a chlorhexidine salt.
[0108] More preferably, the guanidine derivative is selected from chlorhexidine or a chlorhexidine salt.
[0109] Chlorhexidine or its salts are known to degrade into chemical subclasses over long periods of time, however, it is noted that this degradation has little or no effect on the CMP activity outlined herein. The concentration of the products will vary with conditions (temperature / pressure, etc.). Some possible degradation products as listed in Table II-1 on page 19 of the paper entitled Studies on the mechanisms of solid state and solution instability of drugs by Zhixin Zong are reproduced below. It is considered routine for a skilled person to manipulate the degradation products and / or their concentrations to enhance activity.
[0110]
[0111] Preferably, the chlorhexidine or chlorhexidine salt comprises the degradation products listed above.
[0112] Preferably, the first corrosion inhibitor (B) is chlorhexidine.
[0113] Preferably, the first corrosion inhibitor (B) is selected from chlorhexidine salts.
[0114] More preferably, the chlorhexidine salt is selected from the group consisting of chlorhexidine gluconate, chlorhexidine digluconate, chlorhexidine hydrochloride, chlorhexidine dihydrochloride, chlorhexidine acetate, chlorhexidine diacetate, chlorhexidine hexametaphosphate, chlorhexidine metaphosphate and chlorhexidine trimetaphosphate.
[0115] Most preferably, the first corrosion inhibitor is selected from the group consisting of chlorhexidine, chlorhexidine gluconate, and chlorhexidine digluconate,
[0116] Preferably, the first corrosion inhibitor (B) is present in an amount ranging from ≧0.005 wt. % to ≦0.05 wt. %, based on the total weight of the composition.
[0117] More preferably, the first corrosion inhibitor (B) is present in an amount of no more than 0.04 wt.%, most preferably no more than 0.03 wt.%, based on the total weight of the composition. The amount of (B) is preferably at least 0.008 wt.%, more preferably at least 0.01 wt.%, based on the total weight of the composition. The concentration of the corrosion inhibitor (B) is more preferably in the range of ≥ 0.01 wt.% to ≤ 0.03 wt.%, based on the total weight of the composition.
[0118] (C) Second Corrosion Inhibitor
[0119] According to the invention claimed herein, the composition comprises at least one second corrosion inhibitor (C) selected from polyacrylamide and polyacrylamide copolymers.
[0120] As can be seen from Table 1 below, the second corrosion inhibitor (C) selected from polyacrylamide and polyacrylamide copolymers prevents undesirable corrosion of tungsten while ensuring high planarization or polishing efficiency. For example, it is noted that the absence of (C) leads to undesirable topological defects (see Example 18 in Table 1 below).
[0121] Preferably, the polyacrylamide copolymer is an anionic or nonionic polyacrylamide copolymer. For the purposes of the invention claimed herein, the polyacrylamide copolymer is preferably not selected from cationic polyacrylamide copolymers. The use of cationic polyacrylamide copolymers in the composition may lead to flocculation and instability. Preferably, the amount of cationic polyacrylamide copolymer in the composition is <0.01 wt % based on the total weight of the composition.
[0122] Preferably, the polyacrylamide copolymer is a nonionic polyacrylamide copolymer.
[0123] More preferably, the polyacrylamide is a homopolymer.
[0124] Preferably, the second corrosion inhibitor (C) is present in an amount ranging from ≧0.005 wt. % to ≦0.02 wt. %, based on the total weight of the composition.
[0125] More preferably, the second corrosion inhibitor (C) is present in an amount of no more than 0.018 wt.%, even more preferably no more than 0.015 wt.%, most preferably no more than 0.012 wt.%, most preferably no more than 0.01 wt.%, based on the total weight of the composition. The amount of (C) is preferably at least 0.0051 wt.%, more preferably at least 0.0055 wt.%, most preferably at least 0.006 wt.%, based on the total weight of the composition. The concentration of the corrosion inhibitor (C) is more preferably in the range of ≥0.0055 wt.% to ≤0.018 wt.%, most preferably in the range of ≥0.006 wt.% to ≤0.012 wt.%, based on the total weight of the composition.
[0126] Preferably, the weight average molecular weight of the second corrosion inhibitor (C) determined by gel permeation chromatography is in the range of ≥5000 g / mol to ≤50,000 g / mol. More preferably, the weight average molecular weight of the second corrosion inhibitor (C) determined by gel permeation chromatography is in the range of ≥5000 g / mol to ≤40,000 g / mol. Even more preferably, the weight average molecular weight of the second corrosion inhibitor (C) determined by gel permeation chromatography is in the range of ≥7500 g / mol to ≤15,000 g / mol.
[0127] (D) Iron(III) oxidants
[0128] According to the invention claimed herein, the composition comprises at least one iron(III) oxidizing agent (D).
[0129] As can be seen from Table 1 below, the iron(III) oxidizing agent (D) oxidizes the substrate to be polished or one of its layers, thereby ensuring a chemical contribution to the removal rate and a high surface quality.
[0130] Preferably, the iron (III) oxidizing agent (D) is selected from iron (III) salts or compounds with nitric acid, sulfuric acid, hydrofluoric acid, hydrochloric acid, hydrobromic acid, hydroiodic acid, perchloric acid, perbromic acid, periodic acid, acetic acid, acetylacetone, o-phosphoethanolamine, phosphonic acid, alendronic acid, acetic acid, phthalic acid, citric acid, adipic acid, oxalic acid, malonic acid, aspartic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, oxalic acid, maleic acid, gluconic acid, muconic acid, ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, or mixtures thereof.
[0131] More preferably, the iron (III) oxidizing agent (D) is selected from iron (III) nitrate or a hydrate thereof. Even more preferably, the iron (III) oxidizing agent (D) is iron (III) nitrate.
[0132] Preferably, the concentration of the iron(III) oxidizing agent (D) is in the range of ≧0.005 wt. % to ≦0.1 wt. %, based on the total weight of the composition.
[0133] More preferably, the iron (III) oxidizing agent (D) is present in an amount of not more than 0.08 wt.%, even more preferably not more than 0.07 wt.%, most preferably not more than 0.05 wt.%, most preferably not more than 0.03 wt.%, based on the total weight of the composition. The amount of (D) is preferably at least 0.0055 wt.%, more preferably at least 0.006 wt.%, most preferably at least 0.008 wt.%, based on the total weight of the composition. The concentration of the iron (III) oxidizing agent (D) is more preferably in the range of ≥0.0055 wt.% to ≤0.008 wt.%, most preferably in the range of ≥0.008 wt.% to ≤0.03 wt.%, based on the total weight of the composition.
[0134] (E) Silicon oxide removal rate enhancer
[0135] According to the invention claimed herein, the composition comprises at least one silicon oxide removal rate enhancer (E) selected from phosphoric acid or its salts.
[0136] As can be seen from Table 1 below, the silicon oxide removal rate enhancer (E) particularly ensures a high silicon oxide removal rate.
[0137] Preferably, the at least one silicon oxide removal rate enhancer (E) is phosphoric acid or a potassium salt of phosphoric acid. More preferably, the at least one silicon oxide removal rate enhancer (E) is dipotassium hydrogen phosphate.
[0138] Preferably, the concentration of the silicon oxide removal rate enhancer (E) is in the range of ≧0.1 wt. % to ≦1.0 wt. % based on the total weight of the composition.
[0139] More preferably, the silicon oxide removal rate enhancer (E) is present in an amount of no more than 0.9 wt.%, even more preferably no more than 0.8 wt.%, most preferably no more than 0.65 wt.%, based on the total weight of the composition. The amount of (E) is preferably at least 0.15 wt.%, more preferably at least 0.2 wt.%, most preferably at least 0.35 wt.%, based on the total weight of the composition. The concentration of the silicon oxide removal rate enhancer (E) is more preferably in the range of ≥0.15 wt.% to ≤0.9 wt.%, most preferably in the range of ≥0.35 wt.% to ≤0.65 wt.%, based on the total weight of the composition.
[0140] In a preferred embodiment, the silicon oxide removal enhancer (E) is phosphoric acid and is present in an amount of ≥ 0.15 wt. % to ≤ 0.9 wt. % based on the total weight of the composition.
[0141] In another preferred embodiment, the silicon oxide removal enhancer (E) is dipotassium hydrogen phosphate and is present in an amount of ≧0.15 wt. % to ≦0.9 wt. % based on the total weight of the composition.
[0142] (F) Stabilizer
[0143] According to the invention claimed herein, the composition comprises at least one stabilizer (F).
[0144] Without being limited by theory, it is expected that the formation of agglomerates is quite prevalent when incompatible components such as silica particles, iron (III) salts and phosphates are used. However, as can be seen from Table 1 below, the stabilizer (F) ensures colloidal stability.
[0145] Preferably, the at least one stabilizer (F) is selected from acetic acid, acetylacetone, o-phosphoethanolamine, phosphonic acid, alendronic acid, acetic acid, phthalic acid, citric acid, adipic acid, oxalic acid, malonic acid, aspartic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, oxalic acid, maleic acid, gluconic acid, muconic acid, ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof.
[0146] More preferably, the at least one stabilizer (F) is selected from phthalic acid, citric acid, adipic acid, oxalic acid, malonic acid, aspartic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, oxalic acid, maleic acid, gluconic acid, muconic acid, ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof.
[0147] Even more preferably, the at least one stabilizer (F) is chosen from ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof.
[0148] Most preferably, the at least one stabilizer (F) is ethylenediaminetetraacetic acid.
[0149] Preferably, the concentration of the stabilizer (F) is in the range of ≧0.005 wt. % to ≦0.15 wt. %, based on the total weight of the composition.
[0150] More preferably, the stabilizer (F) is present in an amount of no more than 0.1 wt.%, even more preferably no more than 0.08 wt.%, most preferably no more than 0.03 wt.%, based on the total weight of the composition. The amount of (F) is preferably at least 0.0055 wt.%, more preferably at least 0.006 wt.%, most preferably at least 0.008 wt.%, based on the total weight of the composition. The concentration of the stabilizer (F) is more preferably in the range of ≥0.0055 wt.% to ≤0.08 wt.%, most preferably in the range of ≥0.008 wt.% to ≤0.03 wt.%, based on the total weight of the composition.
[0151] (G) Aqueous medium
[0152] According to the invention claimed herein, the composition comprises an aqueous medium (G). The aqueous medium (G) can be one type of aqueous medium or a mixture of different types of aqueous media.
[0153] The aqueous medium (G) may preferably be any medium containing water. Preferably, the aqueous medium (G) is a mixture of water and an organic solvent miscible with water. Representative examples of organic solvents include, but are not limited to, C1 to C3 alcohols, alkylene glycols, and alkylene glycol derivatives. More preferably, the aqueous medium (G) is water. In a preferred embodiment of the invention claimed herein, the aqueous medium (G) is deionized water.
[0154] For purposes of the invention claimed herein, if the amounts of components other than (G) total y wt. % of the composition, then the amount of (G) is (100-y) wt. % of the composition.
[0155] Based on the total weight of the composition, the amount of aqueous medium (G) in the composition is preferably not more than 99.9 wt.%, more preferably not more than 99.6 wt.%, most preferably not more than 99 wt.%, particularly preferably not more than 98 wt.%, particularly not more than 97 wt.%, for example not more than 95 wt.%. Based on the total weight of the composition, the amount of aqueous medium (C) in the composition is preferably at least 60 wt.%, more preferably at least 70 wt.%, most preferably at least 80 wt.%, particularly preferably at least 85 wt.%, particularly at least 90 wt.%, for example at least 93 wt.%.
[0156] The properties of the composition may depend on the pH of the respective composition. According to the invention claimed herein, the pH of the composition is in the range of ≥2.0 to ≤4.5. Preferably, the pH of the composition is ≤4.3, more preferably ≤4.2, most preferably ≤4.0, particularly preferably ≤3.9, particularly most preferably ≤3.5. The pH of the composition is preferably ≥2.1, more preferably ≥2.3, most preferably ≥2.5, particularly preferably ≥2.6, particularly most preferably ≥2.8. The pH of the composition is preferably in the range of ≥2.1 to ≤4.3, preferably ≥2.3 to ≤4.2, more preferably ≥2.5 to ≤4.0, most preferably ≥2.8 to ≤3.5.
[0157] The composition further comprises an additive selected from the group consisting of a pH adjuster, an oxidizing agent, a wetting agent, a dispersant, a biocide, or a mixture thereof.
[0158] The at least one pH adjuster is different from components (A), (B), (C), (D), (E), (F) and (G) and is optionally added in addition to said components.
[0159] Preferably, the at least one pH adjusting agent is selected from the group consisting of: inorganic acids, carboxylic acids, amine bases, alkali metal hydroxides, ammonium hydroxides (including tetraalkylammonium hydroxides). Preferably, the at least one pH adjusting agent is selected from the group consisting of: nitric acid, sulfuric acid, phosphorous acid, ammonia, sodium hydroxide and potassium hydroxide. More preferably, the pH adjusting agent is potassium hydroxide.
[0160] Based on the total weight of the composition, the amount of the at least one pH regulator is preferably not more than 10 wt.%, more preferably not more than 2 wt.%, most preferably not more than 0.5 wt.%, particularly not more than 0.1 wt.%, for example not more than 0.05 wt.%. Based on the total weight of the composition, the amount of the at least one pH regulator (E) is preferably at least 0.0005 wt.%, more preferably at least 0.005 wt.%, most preferably at least 0.025 wt.%, particularly at least 0.1 wt.%, for example at least 0.4 wt.%.
[0161] The composition of the invention claimed herein may further contain at least one oxidizing agent.
[0162] Preferably, the at least one oxidizing agent is selected from the group consisting of organic peroxides, inorganic peroxides, nitrates, persulfates, iodates, periodic acid, periodates, permanganates, perchloric acid, perchlorates, bromic acid and bromates. Said oxidizing agent may optionally be present in addition to the iron (III) oxidizing agent.
[0163] More preferably, the at least one oxidizing agent is hydrogen peroxide.
[0164] Preferably, the at least one oxidizing agent is present in an amount ranging from ≧0.01 wt. % to ≦1.0 wt. %, based on the total weight of the composition.
[0165] Preferably, the concentration of the at least one oxidizing agent is no more than 5.0 wt.%, even more preferably no more than 2.0 wt.%, even more preferably no more than 1.0 wt.%, even more preferably no more than 0.8 wt.%, most preferably no more than 0.5 wt.%, in each case based on the total weight of the composition. The concentration of the at least one oxidizing agent is preferably at least 0.01 wt.%, more preferably at least 0.05 wt.%, most preferably at least 0.1 wt.%, in each case based on the total weight of the composition.
[0166] More preferably, the concentration of hydrogen peroxide as oxidizing agent is ≥0.01 wt.% to ≤1.0 wt.%, even more preferably ≥0.05 wt.% to ≤1.0 wt.%, most preferably ≥0.05 wt.% to ≤0.5 wt.%, particularly preferably ≥0.01 wt.% to ≤0.1 wt.%, in each case based on the total weight of the composition.
[0167] Methods for preparing compositions that inhibit tungsten etching are well known. These methods can be used to prepare the compositions of the invention claimed herein. This can be done by dispersing or dissolving components (A), (B), (D) and (E) described above in an aqueous medium (C), preferably water, and optionally adjusting the pH by adding an acid, base, buffer or pH adjuster (F). For this purpose, conventional and standard mixing methods and mixing equipment can be used, such as a stirred vessel, a high shear impeller, an ultrasonic mixer, a homogenizer nozzle or a countercurrent mixer.
[0168] A preferred embodiment of the invention claimed herein is directed to a composition comprising the following components:
[0169] (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge,
[0170] Particle sizes between 60nm and 200nm, and
[0171] zeta potential < -35 mV at pH ≥2.0 to ≤4.5;
[0172] (B) a first corrosion inhibitor selected from at least one guanidine derivative;
[0173] (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers;
[0174] (D) at least one iron(III) oxidizing agent;
[0175] (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts;
[0176] (F) at least one stabilizer selected from the group consisting of ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof; and
[0177] (G) an aqueous medium,
[0178] The pH of the composition is in the range of ≥2.0 to ≤4.5.
[0179] Another preferred embodiment of the invention claimed herein relates to a composition comprising the following components:
[0180] (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge,
[0181] Particle size from 60nm to 200nm,
[0182] Zeta potential < -35 mV at pH ≥2.0 to ≤4.5, and
[0183] A concentration ranging from ≥ 0.01 wt.% to ≤ 13.0 wt.%, based on the total weight of the composition;
[0184] (B) a first corrosion inhibitor selected from at least one guanidine derivative, and the first corrosion inhibitor has a concentration in the range of ≥ 0.005 wt. % to ≤ 0.05 wt. % based on the total weight of the composition;
[0185] (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers, wherein the weight average molecular weight of (C) of the second corrosion inhibitor as determined by gel permeation chromatography is in the range of ≥5000 g / mol to ≤50,000 g / mol;
[0186] (D) at least one iron (III) oxidizing agent in an amount ranging from ≥ 0.005 wt. % to ≤ 0.1 wt. %, based on the total weight of the composition;
[0187] (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts, and the silicon oxide removal rate enhancer has a concentration in the range of ≥ 0.1 wt. % to ≤ 1.0 wt. % based on the total weight of the composition;
[0188] (F) at least one stabilizer selected from the group consisting of ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof, and having a concentration in the range of ≥0.005 wt.% to ≤0.15 wt.% based on the total weight of the composition; and
[0189] (G) an aqueous medium,
[0190] The pH of the composition is in the range of ≥2.0 to ≤4.5.
[0191] Another preferred embodiment of the invention claimed herein relates to a composition comprising the following components:
[0192] (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge,
[0193] Particle size from 60nm to 200nm,
[0194] Zeta potential < -35 mV at pH ≥2.0 to ≤4.5, and
[0195] A concentration ranging from ≥ 0.01 wt.% to ≤ 13.0 wt.%, based on the total weight of the composition;
[0196] (B) a first corrosion inhibitor selected from at least one guanidine derivative, and the first corrosion inhibitor has a concentration in the range of ≥ 0.005 wt. % to ≤ 0.05 wt. % based on the total weight of the composition;
[0197] (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers, and the second corrosion inhibitor has a concentration in the range of ≥ 0.005 wt. % to ≤ 0.02 wt. % based on the total weight of the composition;
[0198] (D) at least one iron (III) oxidizing agent in an amount ranging from ≥ 0.005 wt. % to ≤ 0.1 wt. % based on the total weight of the composition;
[0199] (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts, and the silicon oxide removal rate enhancer has a concentration in the range of ≥ 0.1 wt. % to ≤ 1.0 wt. % based on the total weight of the composition;
[0200] (F) at least one stabilizer selected from the group consisting of ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof, and having a concentration in the range of ≥0.005 wt.% to ≤0.15 wt.% based on the total weight of the composition; and
[0201] (G) an aqueous medium,
[0202] The pH of the composition is in the range of ≥2.0 to ≤4.5.
[0203] Another preferred embodiment of the invention claimed herein relates to a composition comprising the following components:
[0204] (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge,
[0205] Particle size from 60nm to 200nm,
[0206] Zeta potential < -35 mV at pH ≥2.5 to ≤4.0, and
[0207] A concentration in the range of ≥ 0.3 wt. % to ≤ 7.0 wt. %, based on the total weight of the composition;
[0208] (B) a first corrosion inhibitor selected from at least one guanidine derivative, and the first corrosion inhibitor has a concentration in the range of ≥ 0.01 wt. % to ≤ 0.03 wt. % based on the total weight of the composition;
[0209] (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers, and the second corrosion inhibitor has a concentration in the range of ≥ 0.006 wt. % to ≤ 0.012 wt. % based on the total weight of the composition;
[0210] (D) at least one iron (III) oxidizing agent in an amount ranging from ≥ 0.008 wt. % to ≤ 0.03 wt. %, based on the total weight of the composition;
[0211] (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts, and the silicon oxide removal rate enhancer has a concentration in the range of ≥ 0.35 wt. % to ≤ 0.65 wt. % based on the total weight of the composition;
[0212] (F) at least one stabilizer selected from the group consisting of ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof, and having a concentration in the range of ≥0.008 wt.% to ≤0.03 wt.% based on the total weight of the composition; and
[0213] (G) an aqueous medium,
[0214] The pH of the composition is in the range of ≥2.5 to ≤4.0.
[0215] A preferred embodiment of the invention claimed herein is directed to a composition comprising the following components:
[0216] (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge,
[0217] Particle size from 60nm to 200nm,
[0218] Zeta potential < -35 mV at pH ≥2.5 to ≤4.0, and
[0219] A concentration in the range of ≥ 0.3 wt. % to ≤ 7.0 wt. %, based on the total weight of the composition;
[0220] (B) a first corrosion inhibitor selected from at least one guanidine derivative, and the first corrosion inhibitor has a concentration in the range of ≥ 0.01 wt. % to ≤ 0.03 wt. % based on the total weight of the composition;
[0221] (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers, wherein the weight average molecular weight of (C) of the second corrosion inhibitor as determined by gel permeation chromatography is in the range of ≥7500 g / mol to ≤15,000 g / mol;
[0222] (D) at least one iron (III) oxidizing agent in an amount ranging from ≥ 0.008 wt. % to ≤ 0.03 wt. %, based on the total weight of the composition;
[0223] (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts, and the silicon oxide removal rate enhancer has a concentration in the range of ≥ 0.35 wt. % to ≤ 0.65 wt. % based on the total weight of the composition;
[0224] (F) at least one stabilizer selected from the group consisting of ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof, and having a concentration in the range of ≥0.008 wt.% to ≤0.03 wt.% based on the total weight of the composition; and
[0225] (G) an aqueous medium,
[0226] The pH of the composition is in the range of ≥2.5 to ≤4.0.
[0227] Method for manufacturing a semiconductor device
[0228] In another aspect, the invention claimed herein relates to a method for manufacturing a semiconductor device, the method comprising chemically mechanically polishing a substrate (S) used in the semiconductor industry in the presence of a composition as described herein, the substrate (S) comprising
[0229] (i) Tungsten and / or
[0230] (ii) tungsten alloys; and
[0231] (iii) at least one dielectric layer selected from silicon, silicon oxide, silicon nitride, or a low-k material.
[0232] Preferably, the dielectric layer comprises a combination of silicon oxide and silicon nitride.
[0233] Preferably, the ratio of the material removal rate (MRR) of silicon oxide to the material removal rate (MRR) of tungsten is in the range of 2:1 to 100:1. More preferably, the ratio of the material removal rate (MRR) of silicon oxide to the material removal rate (MRR) of tungsten is in the range of 3:1 to 70:1. Even more preferably, the ratio of the material removal rate (MRR) of silicon oxide to the material removal rate (MRR) of tungsten is in the range of 3:1 to 50:1. More preferably, the ratio of the material removal rate (MRR) of silicon oxide to the material removal rate (MRR) of tungsten is in the range of 3:1 to 40:1. Still more preferably, the ratio of the material removal rate (MRR) of silicon oxide to the material removal rate (MRR) of tungsten is in the range of 3:1 to 20:1. Most preferably, the ratio of the material removal rate (MRR) of silicon oxide to the material removal rate (MRR) of tungsten is in the range of 4:1 to 15:1.
[0234] Preferably, the ratio of the material removal rate (MRR) of silicon nitride to the material removal rate (MRR) of tungsten is in the range of 1.2: 1 to 5: 1. More preferably, the ratio of the material removal rate (MRR) of silicon nitride to the material removal rate (MRR) of tungsten is in the range of 1.3: 1 to 4: 1. Even more preferably, the ratio of the material removal rate (MRR) of silicon nitride to the material removal rate (MRR) of tungsten is in the range of 1.3: 1 to 3.5: 1. Most preferably, the ratio of the material removal rate (MRR) of silicon nitride to the material removal rate (MRR) of tungsten is in the range of 1.5: 1 to 3.0: 1.
[0235] Preferably, the static etch rate (SER) of tungsten is <20 ppb. More preferably, the static etch rate (SER) of tungsten is <18 ppb. Even more preferably, the static etch rate (SER) of tungsten is <15 ppb. Most preferably, the static etch rate (SER) of tungsten is <12 ppb.
[0236] Preferably, the material removal rate (MRR) of silicon oxide is More preferably, the material removal rate (MRR) of silicon oxide is Even more preferably, the material removal rate (MRR) of silicon oxide is Most preferably, the material removal rate (MRR) of silicon oxide is
[0237] Preferably, the material removal rate (MRR) of silicon nitride is More preferably, the material removal rate (MRR) of silicon nitride is Most preferably, the material removal rate (MRR) of silicon nitride is
[0238] There is no particular limitation on the semiconductor devices that can be manufactured by the method according to the invention claimed herein. The semiconductor device can be an electronic component containing semiconductor materials, such as, for example, silicon, germanium, and III-V materials. The semiconductor device can be a device manufactured as a single discrete device or a device manufactured as an integrated circuit (IC), which consists of several devices manufactured and interconnected on a wafer. The semiconductor device can be a two-terminal device, such as a diode; a three-terminal device, such as a bipolar transistor; a four-terminal device, such as a Hall effect sensor or a multi-terminal device. Preferably, the semiconductor device is a multi-terminal device. The multi-terminal device can be a logic device as an integrated circuit and a microprocessor, or a storage device as a random access memory (RAM), a read-only memory (ROM), and a phase change random access memory (PCRAM). Preferably, the semiconductor device is a multi-terminal logic device. In particular, the semiconductor device is an integrated circuit or a microprocessor.
[0239] Typically, tungsten (W) is used for copper interconnects in integrated circuits. Excess tungsten above the dielectric can be removed by a known chemical mechanical polishing process.
[0240] Typically, the tungsten / tungsten alloy can be produced or obtained in different ways, such as ALD, PVD or CVD processes. Typically, the tungsten and / or tungsten alloy can be of any type, form or shape. The tungsten and / or tungsten alloy preferably has a layer and / or overgrowth shape. If the tungsten and / or tungsten alloy has a layer or overgrowth shape, the tungsten and / or tungsten alloy content is preferably greater than 90% by weight of the corresponding layer and / or overgrowth, more preferably greater than 95%, most preferably greater than 98%, particularly greater than 99%, for example greater than 99.9%. The tungsten and / or tungsten alloy is preferably filled or grown in a trench or plug between other substrates, more preferably filled or grown in a trench or plug of a dielectric material such as, for example, SiO2, silicon, low-k (BD1, BD2) or ultra-low-k material or other insulating and semiconductor materials used in the semiconductor industry. For example, in a through silicon via (TSV) intermediate process, insulating materials such as polymers, photoresists and / or polyimides can be used as insulating materials between subsequent process steps of wet etching and CMP after exposing the TSV from the back of the wafer due to their insulating / isolating properties.
[0241] use
[0242] In another aspect, the invention claimed herein relates to the use of the composition described herein for polishing a substrate (S) comprising: (i) tungsten and / or (ii) a tungsten alloy; and (iii) at least one dielectric layer.
[0243] Preferably, the at least one dielectric layer is selected from silicon, silicon oxide, silicon nitride, or a low-k material. More preferably, the dielectric layer comprises a combination of silicon oxide and silicon nitride.
[0244] Preferably, the composition is used in semiconductor manufacturing and processes thereof.
[0245] The invention claimed herein is explained in more detail by means of the accompanying drawings.
[0246] Figure 1 The effect of pH on the zeta potential value of surface modified colloidal silica particles (ie component (A)), ie measured by electrophoresis measurements, is shown. Colloidal silica particles with two different particle sizes, 75 and 109 nm, were investigated.
[0247] Figure 2 Surface images (obtained by SEM) of substrates polished using the composition are depicted. A substrate polished with a composition according to the invention comprising anionic colloidal silica particles is shown in Figure 2 a, while the substrate polished with cationic colloidal silica particles is shown in Figure 2 b.
[0248] Figure 3 Depicted are DLS measurements of filtered silica dispersions measured with a Malvern Zetasizer ZSP when the zeta potential of the surface modified colloidal silica particles is > -35 mV at a pH in the range of ≥2.0 to ≤4.5. The measurements show that the DLS method is unable to record stable measurements when the zeta potential of the surface modified colloidal silica particles is > -35 mV at a pH in the range of ≥2.0 to ≤4.5. At pH 2.8, the zeta potential of the silica particles was set to -23 mV with 0.1 M potassium chloride for the measurements.
[0249] Figure 4 Depicted are DLS measurements of filtered silica dispersions measured with a Malvern Zetasizer ZSP when the zeta potential of the surface modified colloidal silica particles was < -35 mV at a pH ranging from ≥2.0 to ≤4.5.
[0250] The composition according to the invention claimed herein has at least one of the following advantages:
[0251] (1) The compositions and methods of the invention claimed herein show high selectivity for the removal of silicon oxide relative to tungsten.
[0252] (2) The compositions and methods of the invention claimed herein show improved performance in inhibiting etching, especially inhibiting the etching of tungsten and cobalt (as evidenced by low SER values).
[0253] (3) The compositions of the invention claimed herein provide stable formulations or dispersions wherein no phase separation or agglomeration occurs, especially under acidic conditions.
[0254] (4) The compositions of the invention claimed herein allow for easy processability, such as compatibility with industrially relevant steps such as microfiltration.
[0255] (5) The method of the invention claimed herein is easy to apply and requires as few steps as possible.
[0256] (6) The compositions and methods of the invention claimed herein allow for good tunability, thereby achieving high silicon oxide (SiO2) and silicon nitride (SiN) removal rates while ensuring low tungsten (W) removal rates.
[0257] (7) The composition of the invention claimed herein is intended to provide suitable removal rates as mentioned above while preventing undesirable surface defects and ensuring high surface quality.
[0258] Example
[0259] Hereinafter, a list of examples is provided to further illustrate the present disclosure without intending to limit the present disclosure to the specific examples listed below.
[0260] 1. A dielectric polishing composition comprising
[0261] (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge,
[0262] Particle sizes between 60nm and 200nm, and
[0263] zeta potential < -35 mV at pH ranging from ≥2.0 to ≤4.5;
[0264] (B) a first corrosion inhibitor selected from at least one guanidine derivative;
[0265] (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers;
[0266] (D) at least one iron(III) oxidizing agent;
[0267] (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts;
[0268] (F) at least one stabilizer; and
[0269] (G) an aqueous medium,
[0270] The pH of the composition is in the range of ≥2.0 to ≤4.5.
[0271] 2. The composition of embodiment 1, wherein the surface modified colloidal silica particles have a zeta potential of -80 mV to -35 mV at a pH in the range of ≥2.0 to ≤4.5.
[0272] 3. The composition of any one of embodiments 1 to 2, wherein the concentration of the surface modified colloidal silica particles (A) is in the range of ≥ 0.01 wt. % to ≤ 13.0 wt. %, based on the total weight of the composition.
[0273] 4. The composition of any one of embodiments 1 to 3, wherein the guanidine derivative is selected from buformin, phenformin, guanine, proguanil hydrochloride, 2-guanidinobenzimidazole, polyhexamethylene biguanide hydrochloride, polyaminopropyl biguanide, chlorhexidine or a chlorhexidine salt.
[0274] 5. The composition of any one of embodiments 1 to 4, wherein the first corrosion inhibitor (B) is chlorhexidine.
[0275] 6. The composition of any one of embodiments 1 to 5, wherein the concentration of the first corrosion inhibitor (B) is in the range of ≧0.005 wt. % to ≦0.05 wt. %, based on the total weight of the composition.
[0276] 7. The composition of any one of embodiments 1 to 6, wherein the pH of the composition is in the range of ≥2.5 to ≤4.0.
[0277] 8. The composition of any one of embodiments 1 to 7, wherein the weight average molecular weight of the second corrosion inhibitor (C) determined according to gel permeation chromatography is in the range of ≧5000 g / mol to ≦50,000 g / mol.
[0278] 9. The composition of any one of embodiments 1 to 8, wherein the concentration of the second corrosion inhibitor (C) is in the range of ≧0.001 wt. % to ≦0.5 wt. %, based on the total weight of the composition.
[0279] 10. The composition according to any one of embodiments 1 to 9, wherein the iron (III) oxidizing agent (D) is selected from iron (III) nitrate or a hydrate thereof.
[0280] 11. The composition of any one of embodiments 1 to 10, wherein the concentration of the iron (III) oxidizing agent (D) is in the range of ≥ 0.005 wt. % to ≤ 0.1 wt. %, based on the total weight of the composition.
[0281] 12. The composition of any one of embodiments 1 to 11, wherein the concentration of the silicon oxide removal rate enhancer (E) is in the range of ≥ 0.1 wt. % to ≤ 1.0 wt. %, based on the total weight of the composition.
[0282] 13. The composition of any one of embodiments 1 to 12, wherein the stabilizer (F) is selected from acetic acid, acetylacetone, o-phosphoethanolamine, phosphonic acid, alendronic acid, acetic acid, phthalic acid, citric acid, adipic acid, oxalic acid, malonic acid, aspartic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, oxalic acid, maleic acid, gluconic acid, muconic acid, ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof.
[0283] 14. The composition according to claims 1 to 13, wherein the concentration of the stabilizer (F) is in the range of ≥ 0.005 wt.% to ≤ 0.15 wt.%, based on the total weight of the composition.
[0284] 15. The composition of any one of embodiments 1 to 14, wherein the composition further comprises an additive selected from the group consisting of a pH adjuster, an oxidizing agent, a wetting agent, a dispersant, a biocide, or a mixture thereof.
[0285] 16. A composition according to any one of embodiments 1 to 15, wherein the composition is used for polishing a substrate (S), wherein the substrate (S) comprises: (i) tungsten and / or (ii) a tungsten alloy; and (iii) at least one dielectric layer selected from silicon, silicon oxide, silicon nitride, or a low-k material.
[0286] 17. A method for manufacturing a semiconductor device, the method comprising chemically mechanically polishing a substrate (S) used in the semiconductor industry in the presence of a composition as described in any one of embodiments 1 to 16, wherein the substrate (S) comprises
[0287] (i) Tungsten and / or
[0288] (ii) tungsten alloys; and
[0289] (iii) at least one dielectric layer selected from silicon, silicon oxide, silicon nitride, or a low-k material.
[0290] 18. The method of embodiment 17, wherein a ratio of a material removal rate (MRR) of silicon oxide to a material removal rate (MRR) of tungsten is in a range of 2:1 to 100:1.
[0291] 19. The method of any one of embodiments 17 to 18, wherein a ratio of a material removal rate (MRR) of silicon nitride to a material removal rate (MRR) of tungsten is in a range of 1.2:1 to 5:1.
[0292] 20. The method of any one of embodiments 17 to 19, wherein the static etch rate (SER) of tungsten is <20 ppb.
[0293] 21. The method of any one of embodiments 17 to 20, wherein the material removal rate (MRR) of silicon oxide is
[0294] 22. The method of any one of embodiments 17 to 21, wherein the material removal rate (MRR) of silicon nitride is
[0295] 23. Use of the composition according to any one of embodiments 1 to 16 for polishing a substrate (S) comprising: (i) tungsten and / or (ii) a tungsten alloy; and (iii) at least one dielectric layer.
[0296] 24. The use according to embodiment 23, wherein the at least one dielectric is selected from silicon, silicon oxide, silicon nitride, or a low-k material.
[0297] While the invention claimed herein has been described in terms of specific embodiments thereof, certain modifications and equivalents will be apparent to those skilled in the art and are intended to be included within the scope of the invention claimed herein.
[0298] Examples
[0299] The invention claimed herein is illustrated in detail by the following working examples. More particularly, the experimental methods specified hereinafter are part of the general disclosure of the present application and are not limited to the specific working examples.
[0300] The general procedures for slurry preparation and experiments are described below.
[0301] Components:
[0302] ·By product name PLXC (cationic particles) Commercially available silica particles and available from Fuso Chemical Corporation PL5D (anionic particles)
[0303] Chlorhexidine and chlorhexidine digluconate available from Sigma Aldrich
[0304] Deionized water available from BASF SE
[0305] Polyacrylamide available from Sigma-Aldrich
[0306] Hydrogen peroxide available from BASF
[0307] Guanidine carbonate available from Sigma-Aldrich
[0308] Cetyltrimethylammonium bromide (CTAB) available from Sigma-Aldrich
[0309] Slurry composition:
[0310] The slurry composition comprises:
[0311] (A) Silica particles with a particle size of 60 nm to 200 nm and a zeta potential of < -35 mV at a pH of about 3
[0312] (B) First corrosion inhibitor: Chlorhexidine digluconate
[0313] (C) Second corrosion inhibitor: polyacrylamide
[0314] (D) Oxidant: Iron (III) nitrate
[0315] (E) silicon oxide removal rate enhancer: dipotassium hydrogen phosphate; and
[0316] (F) Deionized water (DIW)
[0317] method
[0318] Procedure for preparing slurry composition
[0319] The components in the slurry composition are thoroughly mixed and all mixing procedures are carried out under stirring. Aqueous stock solutions of each compound (A), (B), (C), (D) and (E) are prepared by dissolving the required amount of the corresponding compound in ultrapure water (UPW). For the stock solutions of each component, phosphoric acid (H3PO4) is preferably used to support dissolution. The pH of the stock solution is adjusted to about pH 3.9 with KOH. The stock solution of (B) has a concentration of 20 wt.% chlorhexidine digluconate solution and that of (C) is 0.08 wt.%. For (A), a dispersion as provided by the supplier is used, typically with an abrasive concentration of about 20%-30% by weight.
[0320] The oxidant (D) is used as a buffered iron EDTA salt solution. The solution is prepared by mixing iron (III) nitrate (1.0 wt.%), dipotassium hydrogen phosphate (5 wt.%) and H4-EDTA (in a slight molar excess relative to iron) in UPW. Alternatively, the oxidant (D) is used in the form of a Fe (III) EDTA solution obtainable by common known methods. For example, as reported by Lind et al., Stereochemistry of Ethylenediamintetraacetato Complexes, Inorganic Chemistry Vol. 3, No. 1, 1964 (p. 34 et seq.).
[0321] The final composition was passed through a 5 μm syringe filter prior to DLS measurements as outlined below, or through a 0.1 μm prior to CMP. Filtration is an industrially important process and the colloidal stability of the composition is further highlighted by its ability to remain colloidal stable through microfiltration.
[0322] Inorganic particles used in the examples (A)
[0323] The example according to the invention contains colloidal silica particles (A1) having an average secondary particle size (d2) of 109 nm as determined via a Malvern Zeta Sizer ZSP instrument using the dynamic light scattering (DLS) technique. The silica surface has been partially modified with sulfonic acid.
[0324] Particle Shape Characterization Procedure
[0325] Aqueous cocoon-shaped silica particle dispersion with 20wt.% solid content is dispersed on carbon foil and dried. The dried dispersion is analyzed by using energy filtering-transmission electron microscope (EF-TEM) (120 kV) and scanning electron microscope secondary electron image (SEM-SE) (5 kV). EF-TEM images with a resolution of 2k, 16 bits, and 0.6851nm / pixel are used for analysis. After noise suppression, the image is binary encoded using a threshold. Afterwards, these particles are manually separated. The particles covered and on the edge are distinguished and not used for analysis. ECD, shape factor and sphericity as defined before are calculated and statistical classification is performed.
[0326] Zeta potential measurement
[0327] The zeta potential values were measured with a Malvern Zetasizer ZSP (software version 7.11) equipped with a DTS1070 disposable folded capillary cell. The measurements were recorded at 25°C and 0.1% solid concentration. To ensure the same, the sample solution was filtered through a Millex SV Low Protein Durapore PVDF membrane (5 μm). The zeta potential was calculated by the measured electrokinetic mobility and particle size, as obtained by DLS measurements and fitted in the Smoluchowski model.
[0328] pH Measurement
[0329] The pH value was measured with a pH combination electrode (Schott, blue line 22 pH electrode).
[0330] Particle size measurement - Dynamic light scattering (DLS)
[0331] The measurements were performed with a Malvern Zetasizer ZSP equipped with a semi-micro polystyrene cuvette. The measurements were performed at 25°C by dispersing particles (A) in water (0.1%). Instrument settings: dispersant: water (viscosity: 0.8872 mPa*s; RI 1.330); 5 measurements, 60 s each; automatic attenuator selection was: measurement position fixed at 4.65; analysis model: general.
[0332] Figure 3 and 4Depicted are DLS measurements of filtered silica dispersions measured with a Malvern Zetasizer ZSP when the zeta potential of the surface modified colloidal silica particles is >-35 mV and <-35 mV at a pH ranging from ≥2.0 to ≤4.5 (based on Example 1 of the present invention). Figure 3 showed that the DLS method could not record stable measurements when the zeta potential of the surface-modified colloidal silica particles was > -35 mV (zeta potential adjustment by KCl) at a pH in the range of ≥2.0 to ≤4.5. On the other hand, stable signals could be recorded when the zeta potential of the surface-modified colloidal silica particles was < -35 mV at a pH in the range of ≥2.0 to ≤4.5 (ref. Figure 4 ).
[0333] Static Etch Rate (SER) Experiment of W
[0334] The SER experiment was performed as follows:
[0335] • The tungsten (W) coated wafer was cut into several 2.5 x 2.5 cm coupons and washed with deionized water (DIW).
[0336] • Each coupon was treated with 0.1% citric acid solution for 4 min, and then washed with DIW.
[0337] • Place 300 ml of freshly prepared slurry in a beaker and bring it to 60°C.
[0338] • A tungsten (W) coupon was placed in the slurry and kept in the slurry for 10 min in the SER equipment.
[0339] The tungsten (W) test piece was taken out and rinsed with DIW for 1 min and dried with nitrogen.
[0340] The concentration of tungsten ions in the slurry after etching was measured by ICP-MS.
[0341] Static Etching Rate (SER) Experiment of Co
[0342] The SER experiment was performed as follows:
[0343] • The cobalt (Co) coated wafer was cut into several 2.5×2.5 cm coupons and washed with deionized water (DIW). Each coupon was treated with 0.1% citric acid solution for 4 min and then washed with DIW.
[0344] ·Measure the thickness of tungsten (Co) film (d 之前 ).
[0345] • Place 300 ml of freshly prepared slurry in a beaker and bring it to 60°C.
[0346] • A cobalt (Co) coupon was placed in the slurry and kept in the slurry for 10 min in the SER equipment.
[0347] The cobalt (Co) coupon was taken out and rinsed with DIW for 1 min and dried with nitrogen.
[0348] ·The cobalt (Co) film thickness (d 之后 ).
[0349] The static etch rate (SER) is determined by the following formula:
[0350] SER(A / min)=(d 之前 -d 之后 ) / 10
[0351] Standard CMP process for 300mm barrier polished wafers:
[0352] CMP polisher: 300mm AMAT Reflexion
[0353] Slurry flow rate: 300ml / min
[0354] Down pressure: 2.0psi
[0355] Polishing plate speed: 123rpm
[0356] Polishing head speed: 117rpm
[0357] Polishing pad: Fujibo H600
[0358] Pad conditioning: 3M disc A189L (commercial product); 3lb; 6.5s; (to prevent pad glazing)
[0359] Measuring surface defects using SEM:
[0360] Surface defects were measured via SEM (Hitachi SU8220).The wafers were polished for 1.0 min, polished and dried before inspection.
[0361] Table 1: Composition Examples
[0362]
[0363]
[0364] *The exact amount of phosphoric acid depends on the pH of the surface modified silica raw dispersion and the reaction concentration.
[0365]
[0366] Preparation of Fe(III) Oxidant Solutions Using Phosphoric Acid as Stabilizer (Comparative Examples C11-C13)
[0367] C11 - Place 20.0 g of ultrapure water (UPW) in a beaker. Add 0.2 g of 10% phosphoric acid, followed by 15 g UPW. Add KOH (1.0 mol / l) until pH is about 4, followed by 10 g UPW. Then add 6 g of 1.0% Fe(NO3)3 x 9H2O in UPW and make up the final volume to 100 g.
[0368] C12 - The procedure was followed as outlined for C11 except 2.0 g of 10% phosphoric acid was added.
[0369] C13 - The procedure as outlined for C12 was followed except that 30 g of 1.0% Fe(NO3)3 x 9H2O in UPW was added before making the volume to 100 g.
[0370] Preparation of Fe(III) oxidant solution using H4-EDTA as stabilizer (according to Examples 1-3)
[0371] Place 20.0 g UPW in a beaker. Add 5.0 g K2HPO4 and stir until a clear solution is obtained. Add 0.12 g H4-EDTA (ethylenediaminetetraacetic acid). Stir the mixture until a clear solution is obtained. Add 25 g UPW. Add phosphoric acid (10%) until a pH of about 4 is reached. Add 10 g ferric nitrate solution (1.0%) under stirring.
[0372] Experimental Results
[0373] Table 3
[0374]
[0375]
[0376] Table 4
[0377] Guanidine derivatives W SER(ppb) Buformin 18.5 Phenformin 17.1 Guanine 23.8 Proguanil Hydrochloride 18.1 2-Guandinobenzimidazole 28.6 Polyhexamethylene biguanide hydrochloride 33.8 Polyaminopropyl biguanide 29.5
[0378] A composition was prepared according to Example 1 by replacing chlorhexidine digluconate with 0.02% of the mentioned guanidine derivative.
[0379] Results and Discussion
[0380] Table 1 shows the Static Etching Rate (SER) and Material Removal Rate (MRR) for different compositions. Two different concentrations of silica particles (A) (2 wt.% and 6.5 wt.%) were tested to determine the compatibility of the components with low particle concentrations (as seen in ready-to-use formulations) and high particle concentrations (as seen in concentrate formulations). For example, despite the presence of high silica particle content (6.5 wt.%), Example 1 of the present invention was found to exhibit unexpected colloidal stability. It is noted that the combination of the various components (A) to (G) is critical for Examples 1-3 of the present invention to provide acceptable polishing efficiency as well as solution stability. The zeta potential of the unmodified silica particles was found to increase under acidic conditions (pH <7) (reference Figure 1 ). However, unexpectedly, it was found that the surface modified colloidal silica particles maintained a consistently low zeta potential (in the range of -35 to -60 mV), thus providing colloidal stability even under acidic conditions. Figure 2 a) of the substrate polished with the composition according to the present invention showed a smooth surface, while it was found that the cationic colloidal silica particles ( Figure 2 b) leads to clearly visible agglomerates on the substrate surface (corresponding to comparative example C10). Adding chlorhexidine or chlorhexidine digluconate as corrosion inhibitor (B) in the composition in combination with polyacrylamide as corrosion inhibitor (C) provides a tungsten SER lower than 12ppb in the pH range provided. It is also noted that adding chlorhexidine alone (comparative example C9) or the absence of components (B) and (C) (comparative examples C1-C5) in the composition leads to undesirable effects, such as surface topological defects and low silicon oxide removal rate. In addition, using only phosphoric acid as a stabilizer (C11-C13) to prepare Fe (III) oxidant solution leads to undesirable precipitation. On the other hand, the Fe (III) oxidant solution prepared according to examples 1-3 provides a transparent and amber solution.
[0381] Adding other corrosion inhibitors known in the art such as glycine under the same conditions can also lead to undesirable effects such as high tungsten (W) SER or high cobalt (Co) SER. Table 3 also shows the significant effect of pH on the SER of tungsten. The higher pH range results in a lower static etch rate of tungsten (W).
[0382] In addition, many guanidine derivatives were tested, and as can be seen from the results listed in Table 4, the compositions including these guanidine derivatives also had similar results, such as low tungsten (W) SER.
[0383] Compositions according to examples of the invention claimed herein show improved properties of high SiO2 and SiN MRR, low W MRR, low W and Co SER, while having colloidal or high dispersion stability.
Claims
1. A dielectric polishing composition comprising (A) surface-modified colloidal silica particles comprising negatively charged groups on the surface of the particles, wherein the surface-modified colloidal silica particles have a negative charge, Particle sizes between 60nm and 200nm, and zeta potential < -35 mV at pH ranging from ≥2.0 to ≤4.5; (B) a first corrosion inhibitor selected from at least one guanidine derivative; (C) a second corrosion inhibitor selected from polyacrylamide or polyacrylamide copolymers; (D) at least one iron (III) oxidizing agent; (E) at least one silicon oxide removal rate enhancer selected from phosphoric acid and its salts; (F) at least one stabilizer; and (G) an aqueous medium, The pH of the composition is in the range of ≥2.0 to ≤4.
5.
2. The composition according to claim 1, wherein The surface modified colloidal silica particles have a zeta potential of -80 mV to -35 mV at a pH in the range of ≥2.0 to ≤4.
5.
3. The composition according to any one of claims 1 to 2, wherein The concentration of the surface-modified colloidal silica particles (A) is in the range of ≧0.01 wt. % to ≦13.0 wt. %, based on the total weight of the composition.
4. The composition according to any one of claims 1 to 3, wherein The guanidine derivative is selected from buformin, phenformin, guanine, proguanil hydrochloride, 2-guanidinobenzimidazole, polyhexamethylene biguanide hydrochloride, polyaminopropyl biguanide, chlorhexidine or a chlorhexidine salt.
5. The composition according to any one of claims 1 to 4, wherein The concentration of the first corrosion inhibitor (B) is in the range of ≧0.005 wt. % to ≦0.05 wt. %, based on the total weight of the composition.
6. The composition according to any one of claims 1 to 5, wherein The pH of the composition is in the range of ≥2.5 to ≤4.
0.
7. The composition according to any one of claims 1 to 6, wherein The weight average molecular weight of the second corrosion inhibitor (C) determined according to gel permeation chromatography is in the range of ≧5000 g / mol to ≦50,000 g / mol.
8. The composition according to any one of claims 1 to 7, wherein The concentration of the second corrosion inhibitor (C) is in the range of ≧0.005 wt. % to ≦0.02 wt. %, based on the total weight of the composition.
9. The composition according to any one of claims 1 to 8, wherein The iron (III) oxidizing agent (D) is selected from iron (III) nitrate or its hydrate.
10. The composition according to any one of claims 1 to 9, wherein The concentration of the iron (III) oxidizing agent (D) is in the range of ≧0.005 wt. % to ≦0.1 wt. %, based on the total weight of the composition.
11. The composition according to any one of claims 1 to 10, wherein The concentration of the silicon oxide removal rate enhancer (E) is in the range of ≧0.1 wt. % to ≦1.0 wt. % based on the total weight of the composition.
12. The composition according to any one of claims 1 to 11, wherein The stabilizer (F) is selected from acetic acid, acetylacetone, o-phosphoethanolamine, phosphonic acid, alendronic acid, acetic acid, phthalic acid, citric acid, adipic acid, oxalic acid, malonic acid, aspartic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, oxalic acid, maleic acid, gluconic acid, muconic acid, ethylenediaminetetraacetic acid, propylenediaminetetraacetic acid, N,N-bis(carboxymethyl)alanine, nitrilotriacetic acid, diethylenetriaminepentaacetic acid, bis(salicylidene)ethylenediamine, aminotri(methylenephosphonic acid), diethylenetriaminepenta(methylphosphonic acid), ethylenediaminetetra(methylenephosphonic acid), or a mixture thereof.
13. The composition according to any one of claims 1 to 12, wherein The concentration of the stabilizer (F) is in the range of ≧0.005 wt. % to ≦0.15 wt. %, based on the total weight of the composition.
14. The composition according to any one of claims 1 to 13, wherein The composition further comprises an additive selected from the group consisting of a pH adjuster, an oxidizing agent, a wetting agent, a dispersant, a biocide, or a mixture thereof.
15. The composition according to any one of claims 1 to 14, wherein The composition is used for polishing a substrate (S), wherein the substrate (S) comprises: (i) tungsten and / or (ii) a tungsten alloy; and (iii) at least one dielectric layer selected from silicon, silicon oxide, silicon nitride, or a low-k material.
16. A method for manufacturing a semiconductor device, the method comprising chemically mechanically polishing a substrate (S) used in the semiconductor industry in the presence of a composition as claimed in any one of claims 1 to 15, wherein the substrate (S) comprises (i) Tungsten and / or (ii) tungsten alloys; and (iii) at least one dielectric layer selected from silicon, silicon oxide, silicon nitride, or a low-k material.
17. The method according to claim 16, wherein: The ratio of the material removal rate (MRR) of silicon oxide to the material removal rate (MRR) of tungsten is in the range of 2:1 to 100:
1.
18. The method according to any one of claims 16 to 17, wherein: The static etch rate (SER) of tungsten is <20ppb.
19. The method according to any one of claims 16 to 18, wherein: The material removal rate (MRR) of silicon oxide is > 20. The method according to any one of claims 16 to 19, wherein: The material removal rate (MRR) of silicon nitride is > 21. Use of a composition according to any one of claims 1 to 15 for polishing a substrate (S) comprising: (i) tungsten and / or (ii) tungsten alloys; and (iii) at least one dielectric layer.
22. The use according to claim 21, wherein The at least one dielectric is selected from silicon, silicon oxide, silicon nitride, or a low-k material.
Citation Information
Patent Citations
Tungsten buff polishing compositions with improved topography
US20190211227A1
Tungsten bulk polishing method with improved topography
US20190211228A1
Low sodium, low metals silica polishing slurries
US5230833A
Polishing composition including an inhibitor of tungsten etching
US6083419A
CMP compositions for low-k dielectric materials
US6974777B2