Organic electron barrier layer compound and organic electroluminescent device thereof

By using electron barrier layer compounds containing nitrogen-containing ring and adamantane structures in organic electroluminescent devices, the problem of insufficient heat resistance and stability of electron barrier materials is solved, the life and efficiency of the device are improved, and the lower life is achieved drive voltage and higher stability.

CN118978475APending Publication Date: 2024-11-19JILIN YUANHE ELECTRONICS MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036013.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The heat resistance and film phase stability of electronic barrier materials in existing organic electroluminescent devices are poor, resulting in a shortened device life and a high driving voltage, affecting device efficiency.

Method used

Using an organic electron barrier layer compound, its structure includes rigid adamantane, a ring-shaped structure and a ring-containing ring-containing ring-shaped to improve charge resistance through nitrogen atomic connection, and fine-tune the energy band gap by introducing substituents to enhance the film phase stability. and glass transition temperature.

Benefits of technology

Improves device life and efficiency, reduces driving voltage, and enhances material stability and application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978475A_ABST
    Figure CN118978475A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of organic electroluminescent materials, and particularly relates to an organic electron barrier layer compound and an organic electroluminescent device thereof, and the organic electron barrier layer compound is used as an auxiliary luminescent compound and comprises a rigid adamantane structure, a fused ring structure screwed with adamantane and a nitrogen-containing fused ring structure connected with the fused ring structure through a nitrogen atom single bond. Adamantane in the structure is of a three-dimensional spatial structure, spatial distortion exists in the molecular structure, intermolecular aggregation can be effectively prevented, the membrane phase stability is high, and the compound is not prone to crystallization. In addition, due to the planarity advantage of the ring-fused structure and the nitrogen-containing ring-fused structure on one side, the overall structure is very stable, the glass transition temperature of the compound is high, and the service life of a prepared device can be greatly prolonged. Compared with a contrast compound, the compound provided by the invention has a relatively deep HOMO energy level, so that an injection barrier between a hole transport layer material and a main body material is smaller, and the driving voltage of a device is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic electroluminescent materials, and in particular relates to an organic electron blocking layer compound and an organic electroluminescent device thereof. Background Art

[0002] The classic double-injection organic electroluminescent device consists of three layers: a hole transport layer, a light-emitting layer, and an electron transport layer. Holes are transported to the light-emitting layer through the hole transport layer and combine with electrons in the electron transport layer to form excitons, which then emit light. Organic electroluminescent devices can be adjusted to obtain various required lights by changing the composition of the light-emitting layer as needed.

[0003] Most of the materials used in organic electroluminescent devices are pure organic matter or organometallic complexes, which can be divided into hole injection materials, hole transport materials, carrier blocking materials, luminescent materials, electron transport materials, electron injection materials, etc. according to their uses. Among them, carrier blocking materials are divided into electron blocking materials and hole blocking materials. In organic electroluminescent devices, hole blocking materials are often directly replaced by electron transport materials or directly removed. For top-emitting devices, electron blocking materials adjust the microcavity length and affect the exciton formation area, which is an indispensable component of the device. The heat resistance and amorphousness of electron blocking materials will have a crucial impact on the life of the device. Materials with poor heat resistance are prone to decomposition during the evaporation process, polluting the evaporation cavity and damaging the life of the device; materials with poor film phase stability will crystallize during the use of the device, reducing the service life of the device. Therefore, the electron blocking material is required to have a high film phase stability and decomposition temperature during use. Summary of the invention

[0004] In order to solve the problems existing in the background technology, the first object of the present invention is to provide an organic electron blocking layer compound, and the technical scheme is as follows:

[0005] An organic electron blocking layer compound has a structure shown in the following general formula I:

[0006]

[0007] Wherein X is selected from a single bond, CR 1 R 2 , O, S or S(=O)2; Y is selected from CR 3 R 4 , O, S; Z is selected from a single bond, CR 5 R 6 , O, S or S(=O)2; R 1 -R 6 are the same or different from each other and are independently selected from hydrogen, C1 to C 10 Alkyl, C6~C 30 The aryl group; R7 -R 10 are the same or different from each other and are independently selected from deuterium, amine, cyano, halogen, C1-C 10 Alkyl, C6~C 30 The aryl group, n is independently selected from 0 to the maximum number of sites that can be substituted in the ring.

[0008] As a preferred embodiment of the present invention, X is selected from a single bond, CR 1 R 2 , O, S; Z is selected from a single bond, CR 5 R 6 , O, S.

[0009] As a preferred embodiment of the present invention, the general formula I is represented by the following formula (1-1) to formula (1-4):

[0010]

[0011] As a preferred embodiment of the present invention, the R 1 , R 2 are the same as each other, selected from methyl or phenyl, R 3 , R 4 The same as each other is methyl; R 5 , R 6 are the same as each other and are selected from methyl or phenyl.

[0012] As a preferred embodiment of the present invention, the n is 0.

[0013] As a preferred embodiment of the present invention, the structure of the general formula I is as follows:

[0014]

[0015]

[0016]

[0017]

[0018] Another object of the present invention is to provide an organic electroluminescent device comprising a first electrode, a second electrode and an organic material layer disposed therebetween, wherein the organic material layer comprises a carrier blocking layer comprising at least one of the above-mentioned organic electron blocking layer compounds.

[0019] As a preferred embodiment of the present invention, the organic electroluminescent device is applied to a flat panel display device or a flexible display device.

[0020] The beneficial effects of the present invention are as follows:

[0021] The organic electron blocking layer material provided by the present invention comprises a rigid adamantane structure, a cyclic structure connected to the adamantane by a screw, and a nitrogen-containing cyclic structure connected to the cyclic structure by a single bond of a nitrogen atom. The organic carrier blocking layer compound is connected by a nitrogen atom, which improves the charge resistance of the compound; the adamantane in the structure is a three-dimensional spatial structure, and there is a spatial distortion in the molecular structure, which can effectively prevent the aggregation between molecules, and the film phase stability is strong, so that the compound is not easy to crystallize. In addition, the cyclic structure and the nitrogen-containing cyclic structure on one side have the advantage of planarity, so that the overall structure is very stable, the glass transition temperature of the compound is relatively high, and the life of the prepared device can be greatly improved. Moreover, the compound provided by the present invention has a relatively deep HOMO energy level compared to the comparative compound, so that the injection barrier between the hole transport material and the main material is smaller, which is conducive to reducing the driving voltage of the device, and effectively improving the device efficiency, thereby improving the life of the device.

[0022] In addition, by introducing various substituents into the core structure, the energy band gap can be fine-tuned, improving the interfacial properties between organic materials and diversifying the uses of the materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0024] Figure 1 DSC spectrum of the prepared compound 1 (heating rate 10°C / min);

[0025] Figure 2 The chem3D geometry optimization diagram of the prepared compound 1;

[0026] Figure 3 Graphs showing the lifetime of device example 1 and device comparison example 1. DETAILED DESCRIPTION

[0027] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] If the specific conditions are not specified in the embodiments, they are carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially. Some reaction compounds are purchased from commodity suppliers (Zhengzhou Alpha Chemical Co., Ltd.), and some compounds that cannot be directly purchased are prepared by simple reactions of commercially available raw materials. The percentages all refer to mass percentages, and the temperatures are degrees Celsius (℃). Such method principles, operating procedures, conventional post-treatments, silica gel columns, recrystallization purification and other means are well known to synthesizers in the art, and the synthesis process can be fully realized to obtain the target product. The reactions in each preparation embodiment are generally carried out under positive pressure of nitrogen or argon.

[0029] Preparation Example

[0030] Preparation Example 1: Preparation of Compound 1

[0031]

[0032] Compound 1-1 (8.34 g, 22.54 mmol), compound 1-2 (6.70 g, 23.67 mmol), tris(dibenzylideneacetone)dipalladium (Pd2(dba)3) (0.42 g, 0.45 mmol), 2-dicyclohexylphosphine-2',6'-dimethoxybiphenyl (S-Phos) (0.37 g, 0.90 mmol), sodium tert-butoxide (t-BuONa) (4.55 g, 4 7.34mmol) and toluene (120mL), reflux with stirring at 110°C for 6 hours under nitrogen protection; when the system cools to room temperature, the reaction solution is poured into 250mL of deionized water, extracted with dichloromethane (150mL×3), the organic phases are combined and dried over anhydrous magnesium sulfate, and the solvent is removed under reduced pressure to obtain a crude product; the crude product is purified by silica gel column chromatography using n-heptane / dichloromethane system to obtain compound 1 (11.13g, yield 80%), MS: 617.42.

[0033] Preparation Example 2: Preparation of Compound 5

[0034]

[0035] Compound 5-1 (9.29 g, 22.54 mmol), compound 5-2 (7.08 g, 23.67 mmol), Pd2(dba)3 (0.42 g, 0.45 mmol), S-Phos (0.37 g, 0.90 mmol), t-BuONa (4.55 g, 47.34 mmol) and toluene (120 mL) were added to a 250 mL three-necked flask in sequence, and the mixture was stirred under reflux at 110 ° C for 6 hours under nitrogen protection; when the system cooled to room temperature, the reaction solution was poured into 250 mL of deionized water, extracted with dichloromethane (150 mL × 3), the organic phases were combined and dried over anhydrous magnesium sulfate, and the solvent was removed under reduced pressure to obtain a crude product; the crude product was purified by silica gel column chromatography using an n-heptane / dichloromethane system to obtain compound 5 (12.02 g, yield 79%), MS: 675.47.

[0036] Preparation Example 3: Preparation of Compound 9

[0037]

[0038] Compound 9-1 (8.70 g, 22.54 mmol), compound 9-2 (6.84 g, 23.67 mmol), Pd2(dba)3 (0.42 g, 0.45 mmol), S-Phos (0.37 g, 0.90 mmol), t-BuONa (4.55 g, 47.34 mmol) and toluene (120 mL) were added to a 250 mL three-necked flask in sequence, and the mixture was stirred under reflux at 110 ° C for 6 hours under nitrogen protection; when the system cooled to room temperature, the reaction solution was poured into 250 mL of deionized water, extracted with dichloromethane (150 mL × 3), the organic phases were combined and dried over anhydrous magnesium sulfate, and the solvent was removed under reduced pressure to obtain a crude product; the crude product was purified by silica gel column chromatography using an n-heptane / dichloromethane system to obtain compound 9 (11.67 g, yield 81%), MS: 639.35.

[0039] Preparation Example 4: Preparation of Compound 11

[0040]

[0041] Compound 11-1 (9.06 g, 22.54 mmol), compound 11-2 (6.84 g, 23.67 mmol), Pd2(dba)3 (0.42 g, 0.45 mmol), S-Phos (0.37 g, 0.90 mmol), t-BuONa (4.55 g, 47.34 mmol) and toluene (120 mL) were added to a 250 mL three-necked flask in sequence, and the mixture was refluxed and stirred at 110 ° C for 6 hours under nitrogen protection; when the system cooled to room temperature, the reaction solution was poured into 250 mL of deionized water, extracted with dichloromethane (150 mL×3), the organic phases were combined and dried over anhydrous magnesium sulfate, and the solvent was removed under reduced pressure to obtain a crude product; the crude product was purified by silica gel column chromatography using n-heptane / dichloromethane system to obtain compound 11 (11.77 g, yield 80%), MS: 655.38.

[0042] Preparation Example 5: Preparation of Compound 13

[0043]

[0044] Compound 13-1 (9.78 g, 22.54 mmol), compound 13-2 (8.22 g, 23.67 mmol), Pd2(dba)3 (0.42 g, 0.45 mmol), S-Phos (0.37 g, 0.90 mmol), t-BuONa (4.55 g, 47.34 mmol) and toluene (120 mL) were added to a 250 mL three-necked flask in sequence, and the mixture was stirred under reflux at 110 ° C for 6 hours under nitrogen protection; when the system cooled to room temperature, the reaction solution was poured into 250 mL of deionized water, extracted with dichloromethane (150 mL×3), the organic phases were combined and dried over anhydrous magnesium sulfate, and the solvent was removed under reduced pressure to obtain a crude product; the crude product was purified by silica gel column chromatography using an n-heptane / dichloromethane system to obtain compound 13 (13.78, yield 82%), MS: 745.36.

[0045] Preparation Example 6: Preparation of Compound 16

[0046]

[0047] Compound 16-1 (12.09 g, 22.54 mmol), compound 16-2 (10.63 g, 23.67 mmol), Pd2(dba)3 (0.42 g, 0.45 mmol), S-Phos (0.37 g, 0.90 mmol), t-BuONa (4.55 g, 47.34 mmol) and toluene (120 mL) were added to a 250 mL three-necked flask in sequence, and the mixture was refluxed and stirred at 110 ° C for 6 hours under nitrogen protection; when the system cooled to room temperature, the reaction solution was poured into 250 mL of deionized water, extracted with dichloromethane (150 mL×3), the organic phases were combined and dried over anhydrous magnesium sulfate, and the solvent was removed under reduced pressure to obtain a crude product; the crude product was purified by silica gel column chromatography using an n-heptane / dichloromethane system to obtain compound 16 (16.69, yield 78%), MS: 949.57.

[0048] In addition, it should be noted that other compounds of the present application can be obtained by referring to the preparation methods of the above-mentioned embodiments, so they will not be listed one by one here.

[0049] Device Embodiment

[0050] Preparation of Device Example 1:

[0051] A glass substrate coated with ITO (indium tin oxide) as a thin film with a thickness of 1000 angstroms was placed in distilled water in which a detergent was dissolved and ultrasonically cleaned. After the ITO was cleaned for 30 minutes, ultrasonic cleaning was repeated twice with distilled water for 10 minutes, and then the substrate was ultrasonically cleaned with isopropyl alcohol, acetone and methanol solvents, dried, transferred to a plasma cleaner for cleaning for 5 minutes, and then transferred to a vacuum depositor;

[0052] On the ITO transparent electrode, the compound [HI] was thermally vacuum deposited to a thickness of 100 angstroms to form a hole injection layer; the compound [HT] was vacuum deposited to 800 angstroms on the hole injection layer to form a hole transport layer; the compound 1 was vacuum deposited to a thickness of 50 angstroms on the hole transport layer to form an electron blocking layer; the compound [BH] and the compound [BD] were vacuum deposited to a thickness of 200 angstroms at a ratio of 97:3 on the electron blocking layer to form a light emitting layer; the compound [ET] and the compound [LiQ] (lithium quinoline) were vacuum deposited to form an electron transport layer with a thickness of 300 angstroms at a ratio of 1:1 on the light emitting layer; yttrium (Yb) and magnesium silver (1:9) were sequentially deposited on the electron transport layer to a thickness of 10 angstroms and 1000 angstroms, respectively, to form a cathode. The vacuum degree during deposition was maintained at 1×10 -7 Up to 5×10 -8 Entrust.

[0053] Preparation of device examples 2 to 18:

[0054] When forming the electron blocking layer, the compound shown in Table 1 was used instead of Compound 1 in Device Example 1, and an organic electroluminescent device was prepared by the same method as Device Example 1.

[0055] Preparation of Comparative Examples 1 and 2:

[0056] An organic electroluminescent device was prepared in the same manner as in Device Example 1, except that Comparative Compound 1 and Comparative Compound 2 were used instead of Compound 1 in Device Example 1 when forming the electron blocking layer.

[0057] The structure of the compound used in the above preparation process is as follows:

[0058]

[0059]

[0060] The HOMO value of each compound was calculated by Gaussian calculation software; for the organic electroluminescent devices manufactured using each compound as an electron blocking layer in the device examples and device comparative examples, the ... 2 The driving voltage and current efficiency were measured at a current density of 50 mA / cm 2 The time required for the brightness to decrease to 97% of the initial brightness (LT97) was measured at a current density of 1.5 Å. The results are shown in Table 1 below:

[0061] Table 1

[0062]

[0063] In Table 1 above, compared with the comparative example, under the same current density, it can be seen that the current efficiency of the device embodiment is greatly improved, the driving voltage is reduced, and the service life is improved. For example Figure 3 The lifespan comparison diagram of the devices prepared in Comparative Example 1 and Example 1, J = 50 mA / cm 2 At this current density, the brightness drops to 970cd / m 2 When the device is used in Example 1, the life of the device is longer than that of the device used in Comparative Example 1. Figure 2 The molecular structure diagram of compound 1 of the present invention adjusted by chem3D shows more intuitively that the planar rigidity of the compound structure is good and its glass transition temperature is high (see Figure 1 , Tg value 125.04°C), so the film formation stability is very good during the thermal evaporation process, which is beneficial to improving the life of the device; in addition, compared with the comparative example compounds, the compounds provided in the present application have a deeper HOMO energy level and can better form ohmic contact with the main material, which is beneficial to reducing the driving voltage of the device and effectively improving the device efficiency, thereby improving the life of the device and having broad application prospects.

Claims

1. An organic electron blocking layer compound, It is characterized in that It has the structure shown in the following general formula I: Wherein X is selected from a single bond, CR 1 R 2 , O, S or S(=O) 2 ; Y is selected from CR 3 R 4 , O, S; Z is selected from a single bond, CR 5 R 6 , O, S or S(=O) 2 ; R 1 -R 6 are the same or different from each other and are independently selected from hydrogen, C 1 ~C 10 Alkyl, C 6 ~C 30 The aryl group; R 7 -R 10 are the same or different from each other and are independently selected from deuterium, amine, cyano, halogen, C 1 ~C 10 Alkyl, C 6 ~C 30 The aryl group, n is independently selected from 0 to the maximum number of sites that can be substituted in the ring.

2. The organic electron blocking layer compound according to claim 1, It is characterized in that The X is selected from a single bond, CR 1 R 2 , O, S; Z is selected from a single bond, CR 5 R 6 , O, S.

3. The organic electron blocking layer compound according to claim 2, It is characterized in that General formula I is represented by the following formula (1-1) to formula (1-4):

4. The organic electron blocking layer compound according to claim 2, It is characterized in that The R 1 , R 2 are the same as each other, selected from methyl or phenyl, R 3 , R 4 The same as each other is methyl; R 5 , R 6 are the same as each other and are selected from methyl or phenyl.

5. The organic electron blocking layer compound according to claim 2, It is characterized in that The n is 0.

6. The organic electron blocking layer compound according to claim 1, It is characterized in that The structure of the general formula I is as follows:

7. An organic electroluminescent device, It is characterized in that The method comprises a first electrode, a second electrode and an organic material layer arranged therebetween, wherein the organic material layer comprises a carrier blocking layer, and the preparation material of the carrier blocking layer comprises at least one organic electron blocking layer compound as claimed in any one of claims 1 to 6.

8. The organic electroluminescent device according to claim 7, It is characterized in that The organic electroluminescent device is applied to a flat panel display device or a flexible display device.