Negative electrode material for secondary battery, and secondary battery
By using a cover layer to protect the composite particles in the secondary battery, the side reaction erosion caused by nonaqueous electrolytes is solved, and the circulation characteristics and stability of the battery are significantly improved.
Patent Information
- Application Number
- CN202380030641.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-19
AI Technical Summary
The silicate phase of the composite particles in the existing secondary batteries is easily eroded by side reactions caused by non-aqueous electrolytes, resulting in deterioration and reduced circulation characteristics. The prior art cannot fully suppress such side reactions.
The ion-conducting phase that contains silicon particles and covers the surface, and a cover layer is formed using lithium sulfonate compounds and linear saturated fatty acid compounds with more than 10 carbon atoms to protect the composite particles from the influence of nonaqueous electrolytes and inhibit ion conduction. phase erosion.
The circulation characteristics of the secondary battery are significantly improved, the composite particles are deteriorated, and the service life of the battery is extended.
Smart Images

Figure CN118985052A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a negative electrode material for a secondary battery and a secondary battery. Background Art
[0002] Non-aqueous electrolyte secondary batteries represented by lithium ion secondary batteries are used as power sources for electronic devices such as portable terminals, power sources for vehicles such as electric cars, etc. Graphite is generally used as a negative electrode active material for non-aqueous electrolyte secondary batteries.
[0003] In recent years, for non-aqueous electrolyte secondary batteries, research has been conducted on using negative electrode active materials having a capacity density (capacity per unit mass) greater than that of graphite. For example, composite particles having a silicate phase and a silicon phase dispersed in the silicate phase have been studied as negative electrode active materials.
[0004] Patent document 1 proposes a negative electrode active material for a secondary battery, which comprises: a silicate phase containing Li, Si and M (M is an alkali metal, an alkaline earth metal, and an element other than Si); silicon particles dispersed in the above-mentioned silicate phase; and metal particles with one or more metals or alloys selected from Fe, Cr, Ni, Mn, Cu, Mo, Zn, and Al as the main component dispersed in the above-mentioned silicate phase, wherein the total content of each element in the above-mentioned silicate phase relative to the element other than oxygen is 3 to 45 mol% for Li, 40 to 78 mol% for Si, and 1 to 40 mol% for M.
[0005] In Patent Document 2, a negative electrode active material for a secondary battery is proposed, which comprises: a silicate phase containing Li, Si and M (M is an alkali metal, an alkaline earth metal, and an element other than Si); silicon particles dispersed in the above-mentioned silicate phase; and oxide particles containing at least any one of oxide particles containing Zr, oxide particles containing Ce, oxide particles containing Ca, oxide particles containing Al, oxide particles containing Fe, oxide particles containing Mg, oxide particles containing Ti and oxide particles containing W dispersed in the above-mentioned silicate phase, wherein the total content of each element in the above-mentioned silicate phase relative to the element other than oxygen is 3 to 45 mol % for Li, 40 to 78 mol % for Si, and 1 to 40 mol % for M.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2019 / 151016 Pamphlet
[0009] Patent Document 2: International Publication No. 2019 / 151026 Pamphlet Summary of the invention
[0010] Problem that the invention aims to solve
[0011] The silicate phase of the composite particles tends to be gradually corroded by side reactions in the battery containing the non-aqueous electrolyte. Due to this corrosion, the composite particles deteriorate and the cycle characteristics of the battery decrease.
[0012] The negative electrode active materials described in Patent Documents 1 and 2 can suppress the destruction of particles caused by the expansion and contraction of silicon during charge and discharge to a certain extent, but the suppression of side reactions is still insufficient.
[0013] Solutions for solving problems
[0014] In view of the above, one aspect of the present disclosure relates to a negative electrode material for a secondary battery, which comprises silicon-containing particles and a covering layer covering at least a portion of the surface of the silicon-containing particles, the silicon-containing particles comprising an ion-conducting phase and a silicon phase dispersed in the ion-conducting phase, and the covering layer comprising a lithium sulfonate compound and a straight-chain saturated fatty acid compound having more than 10 carbon atoms.
[0015] Another aspect of the present disclosure relates to a secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the negative electrode includes the negative electrode material for a secondary battery.
[0016] Effects of the Invention
[0017] According to the present disclosure, it is possible to suppress a decrease in the cycle characteristics of a secondary battery including a negative electrode including silicon-containing particles.
[0018] The novel features of the present invention are described in the claims, but the present invention relates to both structure and content, and together with other objects and features of the present invention, will be better understood from the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a cross-sectional view schematically showing a negative electrode material for a secondary battery according to one embodiment of the present disclosure.
[0020] Figure 2 This is a schematic perspective view in which a part of a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure is cut away. DETAILED DESCRIPTION
[0021] Hereinafter, examples are given to illustrate the embodiments of the present disclosure, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials are sometimes exemplified, but other numerical values and materials may also be applied as long as the effects of the present disclosure can be obtained. In this specification, the description of "numerical value A to numerical value B" includes numerical value A and numerical value B, which can be replaced by "numerical value A or more and numerical value B or less". In the following description, when the lower limit and upper limit of numerical values related to specific physical properties, conditions, etc. are exemplified, as long as the lower limit is not above the upper limit, any one of the exemplified lower limits can be arbitrarily combined with any one of the exemplified upper limits. When multiple materials are exemplified, one of them can be selected and used alone, or two or more can be used in combination.
[0022] A negative electrode material for a secondary battery according to one embodiment of the present disclosure comprises silicon-containing particles and a covering layer covering at least a portion of the surface of the silicon-containing particles. The silicon-containing particles include an ion-conducting phase and a silicon phase dispersed in the ion-conducting phase. The covering layer includes a lithium sulfonate compound and a linear saturated fatty acid compound having 10 or more carbon atoms. The covering layer is a mixed layer of the lithium sulfonate compound and the linear saturated fatty acid compound. Hereinafter, the silicon-containing particles are also referred to as "composite particles".
[0023] The ion-conducting phase may include, for example, at least one selected from the group consisting of a silicate phase, a silicon oxide phase, and a carbon phase. Hereinafter, at least one of the silicate phase and the silicon oxide phase is also referred to as a "silicon compound phase". Composite particles in which a silicon phase is dispersed in a silicate phase are also referred to as "composite particles containing a silicate phase". Composite particles in which a silicon phase is dispersed in a silicon oxide phase are also referred to as "composite particles containing a silicon oxide phase". Composite particles in which a silicon phase is dispersed in a carbon phase are also referred to as "composite particles containing a carbon phase".
[0024] By covering the surface of the composite particles (ion-conducting phase) with a lithium sulfonate compound, the composite particles are protected from the influence of the non-aqueous electrolyte, the side reaction with the non-aqueous electrolyte is suppressed, and the corrosion of the ion-conducting phase caused by the non-aqueous electrolyte is suppressed. The degradation of the composite particles caused by the corrosion and the reduction in the cycle characteristics of the secondary battery are suppressed.
[0025] By mixing the lithium sulfonate compound and the straight-chain saturated fatty acid compound in the coating layer, the retention of the lithium sulfonate compound on the surface of the composite particles is improved, and the surface of the composite particles is effectively covered with the lithium sulfonate compound, thereby significantly suppressing the corrosion of the ion-conducting phase by the lithium sulfonate compound.
[0026] In the production method described below, the coating layer can be formed so that the straight-chain saturated fatty acid compound is distributed throughout the coating layer and the lithium sulfonate compound is distributed in large amounts in the inner layer of the coating layer (surface side of the composite particles). The lithium sulfonate compound is firmly protected in such a coating layer.
[0027] The negative electrode is prepared, for example, by preparing a slurry containing a negative electrode material and water, applying the slurry to a negative electrode collector, drying, and rolling as needed to form a negative electrode mixture layer. The contact between the lithium sulfonate compound and water in the covering layer is suppressed by the straight-chain saturated fatty acid compound. The straight-chain saturated fatty acid compound has a straight-chain saturated aliphatic hydrocarbon group (with a carbon number of 9 or more) as a hydrophobic group and is not easily soluble in water. Therefore, the dissolution of the lithium sulfonate compound in water when the negative electrode is made is suppressed.
[0028] When a lithium sulfonate compound, a linear saturated fatty acid compound, and water are added to composite particles to prepare a slurry, the lithium sulfonate compound dissolves in water, and the lithium sulfonate compound cannot be fully loaded on the surface of the composite particles. In addition, when NMP is used instead of water as the dispersion medium of the slurry, the linear saturated fatty acid compound dissolves in NMP, making it difficult to load the lithium sulfonate compound on the surface of the composite particles.
[0029] (Lithium sulfonate compound)
[0030] The lithium sulfonate compound is a lithium salt of a sulfonic acid compound. The sulfonic acid compound is an organic compound having a sulfonic acid group (SO3H). The sulfonic acid compound may be a monosulfonic acid compound or a disulfonic acid compound. The lithium sulfonate compound may be used alone or in combination of two or more.
[0031] The lithium sulfonate compound is preferably a compound represented by the following general formula (1): In the general formula (1), R is an n-valent aliphatic hydrocarbon group having 1 to 5 carbon atoms, and n is 1 or 2.
[0032]
[0033] The lithium sulfonate compound more preferably contains at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and lithium propanesulfonate, and among them, it is particularly preferred to contain lithium methanesulfonate.
[0034] The amount of the lithium sulfonate compound covering the surface of the composite particles (hereinafter also referred to as the supported amount of the lithium sulfonate compound) can be 1 part by mass or more, 1 part by mass or more and 10 parts by mass or less, or 1 part by mass or more (or 2 parts by mass or more) and 6 parts by mass or less relative to 100 parts by mass of the composite particles.
[0035] When the loading amount of the lithium sulfonate compound is 1 part by mass or more, the surface of the composite particles can be fully covered with the lithium sulfonate compound, and the side reaction inhibition effect brought by the lithium sulfonate compound can be easily obtained. When the loading amount of the lithium sulfonate compound is 6 parts by mass or less, a negative electrode material (covering layer) with low resistance can be easily obtained. When a covering layer containing a lithium sulfonate compound and a straight-chain saturated fatty acid compound is formed, the lithium sulfonate compound can be loaded on the surface of the composite particles in an amount within the above range.
[0036] (Straight chain saturated fatty acid compounds)
[0037] The straight-chain saturated fatty acid compound includes a straight-chain saturated fatty acid and a metal salt thereof. A straight-chain saturated fatty acid is a compound having a carboxyl group (COOH) bonded to the end of a straight-chain saturated hydrocarbon group (straight-chain alkyl group) having 9 or more carbon atoms. Examples of metals forming the salt include lithium, calcium, aluminum, magnesium, sodium, zirconium, potassium, zinc, copper, iron, and the like. Among them, lithium is preferred.
[0038] The linear saturated fatty acid compound is preferably a compound that has excellent stability to the nonaqueous electrolyte and is easily liquefied in the heat treatment step when the cover layer is formed as described later. In this case, the lithium sulfonate compound can be firmly supported on the surface of the composite particles by the linear saturated fatty acid compound, and the side reaction suppression effect brought about by the lithium sulfonate compound can be easily and stably obtained.
[0039] The straight-chain saturated fatty acid compound (higher fatty acid compound) having a carbon number of 10 or more is not easily soluble in water. In the production of the negative electrode using a slurry containing water, it is easy to obtain the protective effect of the straight-chain saturated fatty acid compound on the lithium sulfonate compound. The carbon number of the straight-chain saturated fatty acid compound can be 10 or more and 30 or less, or 10 or more and 25 or less. When the carbon number of the straight-chain saturated fatty acid compound is 25 or less, it is easy to liquefy by heat treatment, and it is easy to load the lithium sulfonate on the surface of the composite particles.
[0040] Examples of the linear saturated fatty acid compound having a carbon number of 10 or more and 30 or less include capric acid (carbon number 10), lauric acid (carbon number 12), myristic acid (carbon number 14), pentadecanoic acid (carbon number 15), palmitic acid (carbon number 16), heptadecanoic acid (carbon number 17), stearic acid (carbon number 18), arachidic acid (carbon number 20), behenic acid (carbon number 22), etc. The linear saturated fatty acid compound may be used alone or in combination of two or more.
[0041] From the viewpoints of being not easily soluble in water, having a low melting point, having a hydrophilic group and a hydrophobic group, and thus having good dispersibility after coating, the straight-chain saturated fatty acid compound preferably includes a stearic acid compound. The stearic acid compound includes stearic acid and its metal salt. As the metal forming the salt, the metals exemplified above can be exemplified. Among them, lithium stearate (STL) is preferred from the viewpoint of having good affinity with the lithium sulfonate compound and being the same lithium salt.
[0042] The amount of the straight-chain saturated fatty acid compound covering the surface of the composite particles (hereinafter, also referred to as the loading amount of the straight-chain saturated fatty acid compound) can be 1 part by mass or more, or 1 part by mass or more (or 2 parts by mass or more) and 6 parts by mass or less relative to 100 parts by mass of the composite particles. When the loading amount of the straight-chain saturated fatty acid compound is 1 part by mass or more, the effect of improving the retention of the lithium sulfonate compound on the surface of the composite particles brought about by the straight-chain saturated fatty acid compound can be fully obtained. When the loading amount of the straight-chain saturated fatty acid compound is 6 parts by mass or less, it is easy to obtain a negative electrode material (covering layer) with low resistance.
[0043] The supported amounts of the lithium sulfonate compound and the straight-chain saturated fatty acid compound (the amounts relative to 100 parts by mass of the composite particles) were determined by the following method.
[0044] The negative electrode material is washed with N-methyl-2-pyrrolidone (NMP) to dissolve the straight-chain saturated fatty acid compound. The washing is to stir the 20°C NMP into which the negative electrode material is added for 1 hour, filter the stirred NMP, and further wash the residue (solid content) with NMP. The filtrate is recovered and quantitatively analyzed by ICP emission spectrometry to determine the mass of the straight-chain saturated fatty acid compound dissolved in the filtrate (NMP).
[0045] The NMP attached to the residue (solid content) is removed by drying. Then, the solid content is washed with water to dissolve the lithium sulfonate compound. The washing is performed by stirring the 20°C water into which the solid content is added for 1 hour, filtering the stirred water, and further washing the residue (solid content) with water. The filtrate is recovered and quantitatively analyzed by ICP emission spectrometry to determine the mass of the lithium sulfonate compound dissolved in the filtrate (water).
[0046] The water adhering to the residue (solid content) is removed by drying to obtain a solid content insoluble in NMP and water. When the negative electrode material comprises composite particles containing a silicon compound phase, the mass of the solid content insoluble in NMP and water is determined as the mass of the composite particles containing a silicon compound phase.
[0047] In the case where the negative electrode material has composite particles containing a silicon compound phase having a conductive layer, a carbon-sulfur analyzer is used to perform a quantitative analysis of carbon on the solid components insoluble in water and NMP. The amount of carbon obtained is derived from the carbon material of the conductive layer. The value obtained by subtracting the mass of carbon obtained by analysis from the mass of the solid components insoluble in water and NMP is obtained as the mass of the composite particles containing a silicon compound phase.
[0048] The supported amount of the lithium sulfonate compound was determined by (mass of the lithium sulfonate compound / mass of the composite particles)×100 using the mass of the lithium sulfonate compound and the mass of the composite particles determined above.
[0049] Using the mass of the linear saturated fatty acid compound and the mass of the composite particles obtained above, the amount of the linear saturated fatty acid compound supported was obtained by (mass of the linear saturated fatty acid compound / mass of the composite particles)×100.
[0050] The thickness of the covering layer is preferably thin enough not to substantially affect the average particle size of the composite particles. From the viewpoint of protecting the composite particles from the influence of the electrolyte, the thickness of the covering layer is preferably 1 nm or more. From the viewpoint of suppressing the increase in resistance, the thickness of the covering layer is preferably 300 nm or less. The thickness of the covering layer may be less than the thickness of the conductive layer described later. The thickness of the covering layer can be measured by cross-sectional observation of the composite particles using an electron microscope. The electron microscope uses a scanning electron microscope (SEM) or a TEM (transmission electron microscope).
[0051] (Conductive layer)
[0052] From the viewpoint of improving electrical conductivity, a conductive layer containing a conductive carbon material may be sandwiched between the composite particles and the covering layer. That is, the covering layer may be formed in the form of a conductive layer covering the surface of the composite particles. The thickness of the conductive layer is preferably thin enough not to substantially affect the average particle size of the composite particles. From the viewpoint of ensuring electrical conductivity, the thickness of the conductive layer is preferably 1 nm or more. From the viewpoint of suppressing the increase in resistance, the total thickness of the covering layer and the conductive layer is preferably 300 nm or less. The thickness of the conductive layer can be measured in the same manner as the case of the covering layer.
[0053] The conductive layer is formed by mixing a raw material of a conductive carbon material with composite particles, and firing the mixture to carbonize the raw material of the conductive carbon material. As the raw material of the conductive material, for example, coal tar pitch or coal tar pitch, petroleum asphalt, phenolic resin, etc. can be used. The firing of the mixture of the raw material of the conductive carbon material and the composite particles is carried out, for example, in an inert atmosphere (for example, an atmosphere of argon, nitrogen, etc.). The firing temperature is preferably above 450°C and below 1000°C. In the case of the above temperature range, it is easy to form a conductive layer with high conductivity in a silicate phase with low crystallinity. The firing temperature is preferably above 550°C and below 900°C, and more preferably above 650°C and below 850°C. The firing time is, for example, above 1 hour and below 10 hours.
[0054] (Method for producing covering layer)
[0055] The method for preparing the covering layer includes, for example, a mixing treatment step of dry-mixing the composite particles (or the composite particles having the conductive layer) with the powders of the lithium sulfonate compound and the linear saturated fatty acid compound to obtain a mixture, and a heat treatment step of heat-treating the mixture. When the composite particles have the conductive layer on the surface, the covering layer is formed on the surface of the composite particles through the conductive layer.
[0056] By the mixing treatment step, an intermediate (mixture) in which a mixture of a lithium sulfonate compound and a straight-chain saturated fatty acid compound is attached to the surface of the composite particles is obtained. The dry mixing treatment can use a ball milling method or the like. The amount of the lithium sulfonate compound added can be 1 part by mass or more and 6 parts by mass or less relative to 100 parts by mass of the composite particles. The amount of the straight-chain saturated fatty acid compound added can be 1 part by mass or more and 6 parts by mass or less relative to 100 parts by mass of the composite particles.
[0057] In the heat treatment process, the intermediate is heated to a temperature above the melting point of the straight-chain saturated fatty acid compound, for example. Through the heat treatment process, the straight-chain saturated fatty acid compound in the mixture is liquefied, and the gap between the composite particles and the particles of the lithium sulfonate compound and the gap between the particles of the lithium sulfonate compound are filled and diffused around the composite particles and the particles of the lithium sulfonate compound. Thus, the retention of the lithium sulfonate compound on the surface of the composite particles is improved. In this way, a covering layer as a mixed layer of the lithium sulfonate compound and the straight-chain saturated fatty acid compound is formed. By crushing the mixture after the heat treatment, the composite particles with the covering layer are obtained.
[0058] It is desirable that the heat treatment be carried out at a temperature above the melting point of the straight-chain saturated fatty acid compound and below the decomposition temperature of the straight-chain saturated fatty acid compound. When lithium stearate is used as the straight-chain saturated fatty acid compound, the heat treatment temperature can be above the melting point (220°C) of lithium stearate and below the decomposition temperature (400°C), for example, preferably above 250°C and below 300°C. The heat treatment can be carried out under an inert gas atmosphere. The heat treatment time can be, for example, about 1 hour to 3 hours.
[0059] The particle sizes of the lithium sulfonate compound and the linear saturated fatty acid compound added in the mixing treatment step are preferably smaller than the particle size of the composite particles. In this case, it is easy to evenly cover the surface of the composite particles (covering layer) with the lithium sulfonate compound and the linear saturated fatty acid compound. The average particle sizes of the lithium sulfonate compound and the linear saturated fatty acid compound can be 1 to 100 μm, or 1 to 10 μm, respectively.
[0060] In the case of forming a covering layer by the above-mentioned preparation method, the lithium sulfonate compound in the covering layer may have a tendency to be hardly distributed in the surface layer of the covering layer, but to be distributed in large quantities in the inner layer of the covering layer. It is believed that this is due to the influence of the compatibility and specific gravity relationship between the lithium sulfonate compound and the straight-chain saturated fatty acid compound (the specific gravity of the lithium sulfonate compound is large). It should be noted that when the thickness of the covering layer is set to T, the surface layer refers to an area with a depth of less than 0.01T from the outermost surface of the covering layer. The inner layer refers to an area with a depth of more than 0.2T from the outermost surface of the covering layer. In the case of such a distribution, the lithium sulfonate compound is firmly protected by the covering layer, and the effect of inhibiting the corrosion of the ion conductive phase caused by the lithium sulfonate compound (inhibiting side reactions) is significantly obtained.
[0061] The analysis of the covering layer can be performed, for example, by X-ray photoelectron spectroscopy (XPS), Raman spectroscopy, time-of-flight secondary ion mass spectrometry (TOF-SIMS), etc. When the surface analysis of the negative electrode material is performed based on XPS, a peak derived from the lithium sulfonate compound is easily observed in the inner layer of the covering layer. On the other hand, the peak is hardly observed in the surface layer of the covering layer. Specifically, the peak is a peak with a binding energy of about 165 to 170 eV and an intensity (c / s) of 200 to 1000.
[0062] (Composite particles)
[0063] The composite particles have a structure in which a silicon phase is dispersed in an ion-conducting phase (matrix). The stress associated with the expansion and contraction of the silicon phase during charge and discharge is relieved by the ion-conducting phase, suppressing the cracking and rupture of the composite particles. Therefore, it is possible to take into account both the high capacity brought by silicon inclusion and the improvement of cycle characteristics. The ion-conducting phase may include a silicon compound phase (at least one of a silicate phase and a silicon oxide phase), or may include a carbon phase. The ion-conducting phase may be composed of one phase or a plurality of phases.
[0064] The silicon oxide phase is composed of a compound of Si and O. The main component of the silicon oxide phase (for example, 95 to 100% by mass) can be silicon dioxide. The silicate phase is composed of a compound containing a metal element, silicon (Si) and oxygen (O). The silicate phase preferably contains at least lithium silicate. In this case, lithium ions can easily enter and exit the silicate phase. It should be noted that, among the silicon oxide phase and the silicate phase, the silicate phase is preferably the main component from the perspective of small irreversible capacity. Here, the "main component" refers to a component that accounts for more than 50% by mass of the total mass of the silicon compound phase, and may also account for more than 70% by mass. The ion-conducting phase is composed of a silicon compound phase, contains a lithium silicate phase as the main component, and may also contain a small amount of silicon oxide phase.
[0065] The composite particles may be composite particles including a silicate phase and a silicon phase dispersed in the silicate phase (composite particles containing a silicate phase). The composite particles containing a silicate phase may be obtained, for example, by pulverizing a mixture of silicate and raw silicon with a ball mill or the like while stirring to obtain microparticles, heat-treating the mixture in an inert atmosphere, and pulverizing the sintered product obtained by the heat treatment.
[0066] The silicate phase preferably contains at least one of an alkali metal element (a first group element other than hydrogen in the long period periodic table) and a second group element in the long period periodic table. Alkali metal elements include lithium (Li), potassium (K), sodium (Na), etc. The second group elements include magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), etc. The silicate phase may further contain rare earth elements such as lanthanum (La), aluminum (Al), boron (B), and other elements.
[0067] Lithium silicate is a silicate containing lithium (Li), silicon (Si) and oxygen (O). The atomic ratio of O to Si in lithium silicate: O / Si is, for example, greater than 2 and less than 4. When the O / Si ratio exceeds 2 and is less than 4 (z in the formula described below is 0<z<2), it is advantageous in terms of the stability of the silicate phase and lithium ion conductivity. It is preferred that the O / Si ratio is greater than 2 and less than 3. The atomic ratio of Li to Si in lithium silicate: Li / Si is, for example, greater than 0 and less than 4.
[0068] The composition of lithium silicate can be expressed by the formula: Li 2z SiO 2+zIt is represented by (0 < z < 2). From the viewpoints of stability, ease of production, lithium ion conductivity, etc., z preferably satisfies the relationship of 0 < z < 1, and more preferably z = 1 / 2. The lithium silicate satisfying z = 1 / 2 can be represented by Li2Si2O5.
[0069] The average particle diameter of the fine silicon phase (before the first charge) dispersed in the silicate phase can be 500 nm or less, can be 200 nm or more, and can be 50 nm or less. By appropriately refining the silicon phase in this way, the volume change during charge and discharge becomes smaller, and the structural stability is improved. In addition, by making the expansion and contraction of the silicon phase uniform, particle breakage is suppressed, and the cycle characteristics are improved. The average particle diameter of the silicon phase is measured by observing the cross section of the negative electrode material using SEM or TEM. Specifically, it is obtained by averaging the maximum diameters of any 100 silicon phases.
[0070] The silicon phase dispersed in the silicate phase is a particulate phase of silicon (Si)单质, and is composed of a single or multiple microcrystals. The microcrystal size of the silicon phase can be 5 nm or more and 50 nm or less. When the microcrystal size of the silicon phase is 50 nm or less, the volume change amount caused by the expansion and contraction of the silicon particles accompanying charge and discharge can be reduced, and the cycle characteristics can be further improved. The microcrystal size of the silicon phase is calculated by the Scherrer formula from the half-value width of the diffraction peak attributed to the Si(111) plane in the X-ray diffraction (XRD) pattern.
[0071] From the viewpoints of increasing the capacity and improving the cycle characteristics, the content ratio of the silicon phase in the composite particles containing the silicate phase can be 30 mass% or more and 90 mass% or less, and can also be 35 mass% or more and 75 mass% or less.
[0072] The composition of the composite particles containing the silicate phase can be obtained, for example, by the following analysis method.
[0073] <edx>
[0074] From the cross-sectional images of the reflection electron images of the negative electrode mixture layer, 10 composite particles with a maximum diameter of 5 μm or more were randomly selected, and elemental mapping analysis was performed using energy dispersive X-ray (EDX). The area ratio of the target element was calculated using image analysis software. The observation magnification is preferably 2000 to 20000 times. The measured values of the area ratio of the specified element contained in the 10 particles were averaged. The content of the target element was calculated from the obtained average value.
[0075] The measurement conditions for the desired cross-sectional SEM-EDX analysis are shown below.
[0076] <SEM-EDX Measurement Conditions>
[0077] Processing device: JEOL, SM-09010 (Cross Section Polisher)
[0078] Processing conditions: acceleration voltage 6 kV
[0079] Current value: 140 μA
[0080] Vacuum degree: 1×10 -3 ~2×10 -3 Pa
[0081] Measurement device: electron microscope SU-70 made by HITACHI
[0082] Acceleration voltage during analysis: 10 kV
[0083] Field: free mode
[0084] Probe current mode: Medium
[0085] Probe current range: High
[0086] Anode Ap.: 3
[0087] OBJ Ap.: 2
[0088] Analysis area: 1 μm square
[0089] Analysis software: EDAX Genesis
[0090] CPS: 20500
[0091] Lsec: 50
[0092] Time constant: 3.2
[0093] <aes>
[0094] Randomly select 10 composite particles with a maximum diameter of 5 μm or more from the cross-sectional image of the reflected electron image of the negative electrode mixture layer, and use an Auger electron spectroscopy (AES) analyzer (e.g., JAMP-9510F, manufactured by JEOL Ltd.) to perform qualitative and quantitative analysis of the elements. The measurement conditions are, for example, an acceleration voltage of 10 kV, a beam current of 10 nA, and an analysis area of 20 μmφ. The content of the specified element contained in the 10 particles is averaged to calculate the content.
[0095] It should be noted that, during the charge and discharge process, a coating is formed on the surface of the composite particles by the decomposition of the non-aqueous electrolyte, etc. In addition, the composite particles sometimes have a coating on their surface and also have a conductive layer as needed. Therefore, the mapping analysis using EDX or AES is performed in a manner that does not include a thin coating, a coating and a conductive layer in the measurement range, from the peripheral edge of the cross section of the composite particles (negative electrode material) to the range of 1 μm inside. By mapping analysis, the distribution state of the carbon material inside the composite particles can also be confirmed. At the end of the cycle, it is difficult to distinguish the decomposition product of the non-aqueous electrolyte, so the measurement of the sample before or at the beginning of the cycle is preferred.
[0096] <icp>
[0097] A sample of the composite particles is completely dissolved in a heated acid solution (a mixed acid of hydrofluoric acid, nitric acid, and sulfuric acid), and the carbon of the solution residue is removed by filtration. Then, the resulting filtrate is analyzed by inductively coupled plasma emission spectrometry (ICP) to measure the spectral intensities of the respective elements. Next, a standard curve is prepared using a commercially available standard solution of the element, and the content of each element contained in the composite particles is calculated.
[0098] In addition, the contents of B, Na, K, and Al contained in the silicate phase can be quantitatively analyzed according to JIS R3105 (1995) (Method for Analysis of Borosilicate Glass).
[0099] In the composite particles containing the silicate phase, there are a silicate phase and a silicon phase, but by using Si-NMR, they can be distinguished and quantified. The Si content obtained by the above method is the sum of the Si amount constituting the silicon phase and the Si amount in the silicate phase. The amount of Si element contained in the composite particles is distributed to the silicate phase and the silicon phase using the results of quantitative analysis based on Si-NMR. It should be noted that as the standard substance required for quantification, a mixture containing a silicate phase and a silicon phase with a known Si content ratio in a specified proportion may be used.
[0100] The following shows the desired measurement conditions for Si-NMR.
[0101] <Si-NMR Measurement Conditions>
[0102] Measuring device: Solid-state nuclear magnetic resonance spectrometer (INOVA-400) manufactured by Varian
[0103] Probe: Varian 7mm CPMAS-2
[0104] MAS: 4.2 kHz
[0105] MAS speed: 4 kHz
[0106] Pulse: DD (45° pulse + signal acquisition time 1H decoupling)
[0107] Repetition time: 1200 sec to 3000 sec
[0108] Observation width: 100 kHz
[0109] Observation center: Around -100 ppm
[0110] Signal acquisition time: 0.05 sec
[0111] Number of accumulations: 560
[0112] Sample amount: 207.6 mg
[0113] Hereinafter, an example of a method for producing composite particles containing a silicate phase will be described in detail.
[0114] Step (i) (Step of Obtaining Lithium Silicate)
[0115] The raw material of lithium silicate uses a raw material mixture containing a raw material containing Si and a Li raw material in a specified ratio. In the raw material mixture, other elements M may also be contained as needed. The mixture mixed with a specified amount of the above raw materials is melted, and the molten metal is passed through a metal roller to form a thin film to produce lithium silicate. Then, in an atmospheric atmosphere, the thin-film silicate is crystallized by heat treatment at a temperature above the glass transition temperature and below the melting point. It should be noted that the thin-film silicate can also be used without crystallization. In addition, it is also possible not to dissolve the mixture mixed with a specified amount, but to sinter it at a temperature below the melting point, and produce silicate by solid phase reaction.
[0116] Silicon oxide can be used as Si raw material. For example, lithium carbonate, lithium oxide, lithium hydroxide, lithium hydride, etc. can be used as Li raw material. They can be used alone or in combination of two or more. The raw material of element M can include oxides, hydroxides, carbonate compounds, hydrides, nitrates, sulfates, etc. of each element.
[0117] The Si raw material that has not reacted with the Li raw material may remain in the lithium silicate. The remaining Si raw material is dispersed in the lithium silicate as fine crystals of silicon oxide.
[0118] Step (ii) (Step of Obtaining Silicate Composite Particles)
[0119] Next, raw material silicon is mixed with lithium silicate to form a composite, for example, through the following steps (a) to (c), to produce composite particles.
[0120] Process (a)
[0121] First, raw silicon powder and lithium silicate powder are mixed at a mass ratio of, for example, 20:80 to 95:5. As the raw silicon, coarse silicon particles having an average particle size of about several μm to several tens of μm may be used.
[0122] Process (b)
[0123] Next, a pulverizing device such as a ball mill is used to pulverize and compound the mixture of raw silicon and lithium silicate while micronizing. At this time, an organic solvent may be added to the mixture to perform wet pulverization. A predetermined amount of organic solvent may be added to the pulverizing container all at once at the beginning of pulverization, or a predetermined amount of organic solvent may be added to the pulverizing container intermittently in multiple times during the pulverization process. The organic solvent serves to prevent the pulverized object from adhering to the inner wall of the pulverizing container.
[0124] As the organic solvent, alcohol, ether, fatty acid, alkane, cycloalkane, silicate, metal alkoxide or the like can be used.
[0125] The raw silicon may be coarse silicon particles having an average particle size of several μm to several tens of μm. The silicon particles finally obtained are preferably controlled so that the crystallite size calculated by the Scherrer equation from the half-value width of the diffraction peak attributable to the Si (111) plane of the X-ray diffraction pattern is 5 nm or more and 50 nm or less.
[0126] It should be noted that the raw silicon and lithium silicate may be micronized and mixed. In addition, silicon nanoparticles and amorphous lithium silicate nanoparticles may be prepared without using a pulverizing device and mixed. Nanoparticles may be prepared using a known method such as a gas phase method (e.g., a plasma method) or a liquid phase method (e.g., a liquid phase reduction method).
[0127] Process (c)
[0128] Next, the crushed material is sintered while applying pressure by hot pressing or the like to obtain a sintered body. Firing is performed, for example, in an inert atmosphere (e.g., an atmosphere of argon, nitrogen, etc.). The sintering temperature is preferably above 450°C and below 1000°C. In the case of the above temperature range, it is easy to disperse tiny silicon particles in the silicate phase with low crystallinity. During sintering, the lithium silicate softens and flows in a manner that fills the gaps between the silicon particles. As a result, a dense block-shaped sintered body with the silicate phase as the sea and the silicon particles as the island can be obtained. The sintering temperature is preferably above 550°C and below 900°C, and more preferably above 650°C and below 850°C. The sintering time is, for example, above 1 hour and below 10 hours.
[0129] When the obtained sintered body is pulverized, silicate composite particles are obtained. By appropriately selecting the pulverization conditions, silicate composite particles having a predetermined average particle size can be obtained.
[0130] Through the steps (i) and (ii), composite particles having a silicate phase as a matrix and a silicon phase dispersed in the matrix are obtained.
[0131] The composite particles may be composite particles including a silicon oxide phase and a silicon phase dispersed in the silicon oxide phase (composite particles containing a silicon oxide phase). The composite particles containing a silicon oxide phase are represented by, for example, the formula SiOX (0.5≤X<1.6). The composite particles containing a silicon oxide phase are obtained, for example, by heat treating silicon monoxide and separating it into a silicon oxide phase and a fine silicon phase by a disproportionation reaction.
[0132] The composite particles may be composite particles including a carbon phase and a silicon phase dispersed in the carbon phase (composite particles containing a carbon phase). Composite particles containing a carbon phase may be obtained, for example, by pulverizing a mixture of a carbon source and raw silicon with a ball mill or the like while stirring, and then subjecting the mixture to micronization, heat-treating the mixture in an inert atmosphere, and pulverizing the sintered product obtained by the heat treatment. Examples of carbon sources include sugars such as carboxymethyl cellulose (CMC), water-soluble resins such as polyvinyl pyrrolidone, and the like.
[0133] The carbon phase has electrical conductivity, so in the composite particles containing the carbon phase, even if voids are formed around the composite particles, it is easy to maintain the contact points between the composite particles and their surroundings. As a result, it is easy to suppress the reduction in capacity caused by repeated charge and discharge cycles. The carbon phase can be composed of amorphous carbon (i.e., non-shaped carbon). Amorphous carbon can be hard carbon, soft carbon or other carbon. Amorphous carbon (non-shaped carbon) generally refers to a carbon material whose average interplanar spacing d002 of the (002) plane measured by X-ray diffraction exceeds 0.34nm.
[0134] From the viewpoint of increasing capacity and improving cycle characteristics, the content of the silicon phase in the composite particles containing the carbon phase may be 30 mass % to 80 mass %, or 40 mass % to 70 mass %.
[0135] The average particle size of the composite particles is, for example, 1 μm or more and 25 μm or less, or 4 μm or more and 15 μm or less. In the above range, good battery performance is easily obtained. It should be noted that, in this specification, the average particle size refers to the particle size (volume average particle size) at which the volume cumulative value is 50% in the particle size distribution measured by the laser diffraction scattering method. The measuring device can be, for example, "LA-750" manufactured by HORIBA.
[0136] Figure 1 The cross section of the negative electrode material 20 is schematically shown.
[0137] The negative electrode material 20 includes a composite particle 23 (mother particle) and a covering layer 26 covering the surface of the composite particle 23. The composite particle 23 includes an ion conductive phase 21 and a silicon phase (silicon particle) 22 dispersed in the ion conductive phase 21. The composite particle 23 has a sea island structure in which the silicon phase 22 is dispersed in the matrix of the ion conductive phase 21. The covering layer 26 includes a lithium sulfonate compound and a linear saturated fatty acid compound. In addition to the composite particle and the covering layer, the negative electrode material may also include other elements. For example, a conductive layer may be between the composite particle and the covering layer.
[0138] The secondary battery of the embodiment of the present disclosure includes a positive electrode, a negative electrode, and a non-aqueous electrolyte. The negative electrode includes the negative electrode material for the secondary battery described above. The negative electrode of the secondary battery and the like are described below.
[0139] [negative electrode]
[0140] The negative electrode, for example, comprises a negative electrode current collector and a negative electrode mixture layer supported on the surface of the negative electrode current collector. The negative electrode mixture layer can be formed by applying a negative electrode slurry in which a negative electrode mixture is dispersed in a dispersion medium to the surface of the negative electrode current collector and drying it. The dried coating film can be rolled as needed. The negative electrode mixture layer can be formed on one surface of the negative electrode current collector or on both surfaces.
[0141] The negative electrode mixture contains the above-mentioned negative electrode material as an essential component, and may contain a binder, a conductive agent, a thickener, etc. as an optional component. The silicon particles in the composite particles can absorb a large amount of lithium ions, and thus contribute to increasing the capacity of the negative electrode.
[0142] In addition to the composite particles, the negative electrode active material may also contain other active material materials that electrochemically absorb and release lithium ions. As other active material materials, carbon-based active materials are preferred. The composite particles expand and shrink in volume with charging and discharging, so if the ratio of the composite particles in the negative electrode active material increases, poor contact between the negative electrode active material and the negative electrode collector is likely to occur with charging and discharging. On the other hand, by using composite particles and carbon-based active materials in combination, a high capacity of the silicon phase can be given to the negative electrode, and excellent cycle characteristics can be achieved. The proportion of composite particles in the total of composite particles and carbon-based active materials is preferably 0.5 to 15% by mass, and more preferably 1 to 5% by mass. As a result, it is easy to take into account both high capacity and improved cycle characteristics.
[0143] As carbon-based active materials, for example, graphite, easily graphitized carbon (soft carbon), and difficultly graphitized carbon (hard carbon) can be exemplified. Among them, graphite having excellent charge and discharge stability and low irreversible capacity is preferred. Graphite refers to a material having a graphite-type crystal structure, including, for example, natural graphite, artificial graphite, and graphitized mesophase carbon particles. One carbon-based active material may be used alone, or two or more may be used in combination.
[0144] As the negative electrode current collector, a nonporous conductive substrate (metal foil, etc.) or a porous conductive substrate (mesh, porous body, punched sheet, etc.) is used. As the material of the negative electrode current collector, stainless steel, nickel, nickel alloy, copper, copper alloy, etc. can be exemplified. The thickness of the negative electrode current collector is not particularly limited, but is preferably 1 to 50 μm, more preferably 5 to 20 μm, from the viewpoint of balancing the strength and lightness of the negative electrode.
[0145] Examples of binders include fluororesins, polyolefin resins, polyamide resins, polyimide resins, vinyl resins, styrene-butadiene copolymer rubber (SBR), polyacrylic acid and its derivatives. They can be used alone or in combination of two or more. As conductive agents, examples include carbon black, conductive fibers, fluorinated carbon, organic conductive materials, etc. They can be used alone or in combination of two or more. As thickeners, examples include carboxymethyl cellulose (CMC), polyvinyl alcohol, etc. They can be used alone or in combination of two or more.
[0146] Examples of the dispersion medium include water, alcohol, ether, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.
[0147] [positive electrode]
[0148] The positive electrode, for example, comprises a positive electrode current collector and a positive electrode mixture layer supported on the surface of the positive electrode current collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry formed by dispersing a positive electrode mixture in a dispersion medium to the surface of the positive electrode current collector and drying it. The dried coating film can be rolled as needed. The positive electrode mixture layer can be formed on one surface of the positive electrode current collector or on both surfaces.
[0149] The positive electrode mixture contains a positive electrode active material as an essential component, and may contain a binder, a conductive agent, etc. as optional components.
[0150] As the positive electrode active material, a lithium composite metal oxide can be used. Examples of the lithium composite metal oxide include Li a CoO2、Li a NiO2、Li a MnO2、Li a Co b Ni 1-b O2、Li a Co b M 1-b O c , Li a Ni 1-b M b O c , Li a Mn2O4、Li a Mn 2- b M b O4, LiMePO4, Li2MePO4F. Here, M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb and B. Me contains at least a transition element (for example, at least one selected from the group consisting of Mn, Fe, Co and Ni). Here, 0≤a≤1.2, 0≤b≤0.9, 2.0≤c≤2.3. In addition, the value a representing the molar ratio of lithium increases or decreases according to charge and discharge.
[0151] As the binder and the conductive agent, the same substances as those exemplified for the negative electrode can be used. As the conductive agent, graphite such as natural graphite and artificial graphite can be used.
[0152] The shape and thickness of the positive electrode current collector can be selected from the shape and range based on the negative electrode current collector. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloy, titanium, and the like.
[0153] [Non-aqueous electrolyte]
[0154] The non-aqueous electrolyte includes a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the non-aqueous electrolyte is, for example, 0.5 to 2 mol / L. The non-aqueous electrolyte may contain a known additive.
[0155] As the non-aqueous solvent, for example, cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, etc. can be used. As cyclic carbonates, propylene carbonate (PC) and ethylene carbonate (EC) etc. can be listed. As chain carbonates, diethyl carbonate (DEC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) etc. can be listed. As cyclic carboxylic acid esters, γ-butyrolactone (GBL), γ-valerolactone (GVL) etc. can be listed. The non-aqueous solvent can be used alone or in combination of two or more.
[0156] As the lithium salt, for example, a lithium salt containing chloric acid (LiClO4, LiAlCl4, LiB 10 Cl 10 etc.), lithium salts of fluorinated acids (LiPF6, LiBF4, LiSbF6, LiAsF6, LiCF3SO3, LiCF3CO2, etc.), lithium salts of fluorinated imides (LiN(CF3SO2)2, LiN(CF3SO2)(C4F9SO2), LiN(C2F5SO2)2, etc.), lithium halides (LiCl, LiI, etc.), etc. The lithium salts may be used alone or in combination of two or more.
[0157] [Separator]
[0158] Generally, it is desirable to sandwich a separator between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation. As the separator, a microporous film, a woven fabric, a nonwoven fabric, etc. can be used. As the material of the separator, for example, polyolefins such as polypropylene and polyethylene can be used.
[0159] As an example of the structure of a secondary battery, an electrode group in which a positive electrode and a negative electrode are wound with a separator and a non-aqueous electrolyte is contained in an outer body can be cited. Alternatively, instead of a wound electrode group, an electrode group in other forms such as a stacked electrode group in which a positive electrode and a negative electrode are stacked with a separator can also be applied. The secondary battery can be in any form such as a cylindrical, square, coin-shaped, button-shaped, laminated, etc.
[0160] As an example of the nonaqueous electrolyte secondary battery disclosed in the present invention, Figure 2 The structure of a prismatic nonaqueous electrolyte secondary battery will be described. Figure 2 This is a schematic perspective view in which a part of a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure is cut away.
[0161] The battery comprises a square-bottomed battery case 4, an electrode group 1 contained in the battery case 4, and a non-aqueous electrolyte (not shown). The electrode group 1 comprises a long strip-shaped negative electrode, a long strip-shaped positive electrode, and a separator interposed therebetween to prevent direct contact. The electrode group 1 is formed by winding the negative electrode, the positive electrode, and the separator around a flat winding core and pulling out the winding core.
[0162] One end of the negative lead 3 is mounted on the negative electrode collector by welding or the like. The other end of the negative lead 3 is electrically connected to the negative terminal 6 provided on the sealing plate 5 via a resin insulating plate (not shown). The negative terminal 6 is insulated from the sealing plate 5 by a resin gasket 7. One end of the positive lead 2 is mounted on the positive electrode collector by welding or the like. The other end of the positive lead 2 is connected to the back of the sealing plate 5 via an insulating plate. That is, the positive lead 2 is electrically connected to the battery case 4 which also serves as the positive terminal. The insulating plate isolates the electrode group 1 from the sealing plate 5 and isolates the negative lead 3 from the battery case 4. The periphery of the sealing plate 5 is fitted with the opening end of the battery case 4, and the fitting portion is laser welded. In this way, the opening of the battery case 4 is sealed by the sealing plate 5. The injection hole for the non-aqueous electrolyte provided in the sealing plate 5 is blocked by the sealing plug 8.
[0163] [Example]
[0164] Hereinafter, examples of the present disclosure will be described in detail, but the present disclosure is not limited to the following examples.
[0165] 《Example 1 to Example 3》
[0166] (Preparation of composite particles)
[0167] Lithium carbonate (Li2CO3) as a Li raw material and silicon dioxide (SiO2) as a Si raw material are mixed in such a way that the atomic ratio: Si / Li becomes 1.05 to obtain a mixture. The mixture is calcined at 800°C for 10 hours in an inert gas atmosphere to obtain lithium silicate (Li2Si2O5). The obtained lithium silicate is crushed into an average particle size of 10μm.
[0168] The crushed lithium silicate and raw silicon (3N, average particle size 10 μm) were mixed at a mass ratio of 40:60. The mixture was filled into a pot (SUS, volume: 500 mL) of a planetary ball mill (Fritsch, P-5). Next, 24 SUS balls (diameter 20 mm) were placed in the pot, the pot was covered with a lid, and the mixture was crushed at 200 rpm in an inert atmosphere for 50 hours.
[0169] Next, the powdered mixture was taken out in an inert atmosphere, and sintered at 600°C for 4 hours under pressure in an inert atmosphere using a hot press to obtain a sintered body of the mixture. The obtained sintered body of the mixture was crushed and passed through a 40 μm mesh to obtain composite particles (composite particles containing a silicate phase). Then, a sieve was used to obtain composite particles with an average particle size of 10 μm.
[0170] The crystallite size of the silicon phase is 15 nm. The silicon phase is granular, and the average particle size of the silicon phase is 20 nm. The main component of the silicate phase is Li2Si2O5, and the content of the silicon phase in the composite particles containing the silicate phase is 60 mass %.
[0171] (Formation of Conductive Layer)
[0172] Then, 100 parts by mass of the composite particles were mixed with 3 parts by mass of coal tar pitch, and the mixture was calcined at 800° C. in an inert atmosphere to cover the surface of the composite particles with conductive carbon. In this way, a conductive layer was formed on the surface of the composite particles. The covering amount of the conductive layer was 3% by mass relative to the total of the composite particles and the conductive layer.
[0173] (Manufacturing of negative electrode materials (Formation of covering layer on the surface of composite particles))
[0174] (Dry Mixing Process)
[0175] Powders of lithium methanesulfonate (MSL) and lithium stearate (STL) are added to composite particles having a conductive layer, and dry mixing is performed to attach MSL and STL to the surface of the composite particles having a conductive layer to obtain an intermediate. The amount of MSL and STL added relative to 100 parts by mass of the composite particles is the value shown in Table 1. The dry mixing treatment is performed by a ball mill method, and a swing mill manufactured by SEIWA Technology Co., Ltd. is used as the device. The dry mixing treatment uses zirconium oxide balls (diameter 3 mm) and is performed at an ambient temperature of room temperature (25°C) for 30 minutes.
[0176] (Heat treatment process)
[0177] Next, the obtained intermediate is heat treated at 270°C for 2 hours in an inert atmosphere to liquefy the STL attached to the surface of the composite particles and improve the retention of MSL on the surface of the composite particles. In this way, a covering layer (a mixed layer of MSL and STL) is formed on the surface of the composite particles having a conductive layer, thereby obtaining a negative electrode material. The thickness T of the covering layer obtained by the above-mentioned method is about 1nm to 300nm.
[0178] (Production of negative electrode)
[0179] Graphite and composite particles (negative electrode material) having a conductive layer and a covering layer were mixed at a mass ratio of 90:10 and used as a negative electrode active material. 0.9 mass parts of carboxymethyl cellulose (CMC) and 1.0 mass parts of styrene butadiene rubber (SBR) were added to 97.5 mass parts of the negative electrode active material, and a predetermined amount of water was further added to prepare a negative electrode slurry.
[0180] The negative electrode slurry is applied to both sides of the copper foil as the negative electrode collector, and the coating is dried and rolled, and then cut into a predetermined size to obtain a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode collector. At this time, a negative electrode collector exposed portion is provided at a part of the negative electrode.
[0181] (Production of positive electrode)
[0182] 2.5 parts by mass of acetylene black and 2.5 parts by mass of polyvinylidene fluoride were added to 95 parts by mass of the positive electrode active material, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was further added to prepare a positive electrode slurry. 0.88 Co 0.09 Al 0.03 A lithium transition metal composite oxide represented by O2.
[0183] The positive electrode slurry is applied to both sides of an aluminum foil as a positive electrode current collector, the coating is dried and rolled, and then cut into a predetermined size to obtain a positive electrode having positive electrode mixture layers formed on both sides of the positive electrode current collector. At this time, a positive electrode current collector exposed portion is provided at a part of the positive electrode.
[0184] (Preparation of non-aqueous electrolyte)
[0185] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 20:5:75 to obtain a mixed solvent. Lithium hexafluorophosphate was dissolved in the mixed solvent at a concentration of 1 mol / L to prepare a non-aqueous electrolyte.
[0186] (Manufacturing of Secondary Batteries)
[0187] An aluminum positive electrode lead is installed on the exposed part of the positive electrode collector of the positive electrode, and a nickel negative electrode lead is installed on the exposed part of the negative electrode collector of the negative electrode. After the positive electrode and the negative electrode are wound into a spiral shape through a polyolefin separator, they are pressed in the radial direction to produce a flat wound electrode body. The electrode body is housed in an outer casing composed of an aluminum laminate sheet, and after injecting a non-aqueous electrolyte, the opening of the outer casing is sealed to obtain a secondary battery for evaluation. It should be noted that in Table 1, A1 to A3 are secondary batteries of Examples 1 to 3.
[0188] Comparative Example 1
[0189] A secondary battery B1 was obtained in the same manner as in the secondary battery A1 of Example 1 except that the covering layer was not formed on the surface of the composite particles having a conductive layer.
[0190] Comparative Example 2
[0191] Secondary battery B2 was obtained in the same manner as secondary battery A1 of Example 1 except that STL was not added in the dry mixing process.
[0192] Comparative Example 3
[0193] Secondary battery B3 was obtained in the same manner as secondary battery A1 of Example 1 except that MSL was not added in the dry mixing process.
[0194] [evaluate]
[0195] The secondary batteries A1 to A3 and B1 to B3 obtained above were evaluated as follows.
[0196] (Initial discharge capacity, initial side reaction amount)
[0197] In an environment of 25°C, constant current charging was performed at a current of 0.3C until the voltage reached 4.2V, and then constant voltage charging was performed at a voltage of 4.2V until the current reached 0.02C. Then, the battery was discharged at a current of 0.5C until the voltage reached 2.5V. The initial charge capacity and discharge capacity at this time were calculated. It should be noted that the charge and discharge capacity was calculated as the capacity per 1g of the composite particles.
[0198] The initial charge and discharge efficiency E (%) was calculated by the following formula using the obtained charge capacity and discharge capacity.
[0199] Initial charge and discharge efficiency E = (discharge capacity / charge capacity) × 100
[0200] The amount of initial side reactions was calculated using the obtained initial charge and discharge efficiency E by the following formula: It should be noted that E0 in the formula is the initial charge and discharge efficiency of the secondary battery B1 of Comparative Example 1.
[0201] Initial side reaction amount = {(100-E) / (100-E0)}×100
[0202] (Cycle degradation rate)
[0203] In an environment of 25°C, constant current charging was performed at a current of 0.3C until the voltage reached 4.2V, and then constant voltage charging was performed at a voltage of 4.2V until the current reached 0.02C. Then, the battery was discharged at a current of 0.5C until the voltage reached 2.5V. This charge and discharge was regarded as one cycle, and 100 cycles were performed.
[0204] The discharge capacity retention rate R (%) was calculated by the following formula using the discharge capacity C1 of the first cycle and the discharge capacity C2 of the 100th cycle.
[0205] Discharge capacity retention rate R = (discharge capacity C2 / discharge capacity C1) × 100
[0206] The cycle degradation rate was calculated by the following formula using the obtained discharge capacity retention rate R. In the formula, R0 is the discharge capacity retention rate of the secondary battery B1 of Comparative Example 1.
[0207] Cycle degradation rate = {(100-R) / (100-R0)}×100
[0208] The evaluation results are shown in Table 1. In Table 1, the initial capacity is expressed as a relative value (index) when the initial capacity of the secondary battery B1 of Comparative Example 1 is set to 100.
[0209] [Table 1]
[0210]
[0211] In secondary batteries A1 to A3, the initial capacity is high, the amount of initial side reactions and the cycle degradation rate are small. In secondary batteries A1 to A3, better cycle characteristics than secondary batteries B1 to B3 are obtained. In batteries B2 and B3, the reduction in cycle degradation rate relative to battery B1 is extremely small. On the other hand, in battery A3, the cycle degradation rate is greatly reduced relative to battery B1.
[0212] The negative electrode materials used in secondary batteries A1 to A3 were subjected to surface analysis based on XPS. As a result, it was confirmed that the amount of MSL was large in the inner layer portion at a depth of 0.2T or more from the outermost surface of the covering layer, and the amount of MSL was small or almost non-existent in the surface layer portion at a depth of less than 0.01T from the outermost surface of the covering layer.
[0213] 《Examples 4 to 6, Comparative Examples 4 to 6》
[0214] Composite particles containing a carbon phase are used as the composite particles. The composite particles containing a carbon phase are prepared as follows.
[0215] Coal tar pitch (MCP250 manufactured by JFE Chemical Co., Ltd.) as a carbon source and raw silicon (3N, average particle size 10 μm) were mixed at a mass ratio of 50:50. The mixture was filled into a pot (SUS, volume: 500 mL) of a planetary ball mill (P-5 manufactured by Fritsch Co., Ltd.), 24 SUS balls (diameter 20 mm) were placed in the pot, the lid was closed, and the mixture was pulverized at 200 rpm for 50 hours in an inert atmosphere to obtain a composite of silicon phase and carbon source.
[0216] Next, the composite of the silicon phase and the carbon source is fired in an inert gas atmosphere to carbonize the carbon source, thereby obtaining a sintered product in which the silicon phase is dispersed in the carbon phase containing amorphous carbon. The sintered product is then pulverized using a jet mill to obtain composite particles containing the carbon phase with an average particle size of 10 μm.
[0217] The crystallite size of the silicon phase was 15 nm. The silicon phase was in a granular form, and the average particle size of the silicon phase was 20 nm. The content of the silicon phase in the composite particles containing the carbon phase was 60 mass %.
[0218] No conductive layer is formed on the surface of the composite particles containing the carbon phase. In the manufacturing process of the negative electrode material, the composite particles containing the carbon phase are used instead of the composite particles containing the silicate phase having the conductive layer. Except for this, the operation is similar to the secondary batteries A1 to A3 of Examples 1 to 3, and the secondary batteries A4 to A6 of Examples 4 to 6 are obtained respectively. In addition, except for the above, the operation is similar to the secondary batteries B1 to B3 of Comparative Examples 1 to Comparative Examples 3, and the secondary batteries B4 to B6 of Comparative Examples 4 to 6 are produced respectively.
[0219] The secondary batteries A4 to A6 and B4 to B6 obtained above were evaluated in the same manner as above. It should be noted that E0 of the calculation formula for the initial side reaction amount and R0 of the calculation formula for the cycle degradation rate are the initial charge and discharge efficiency and discharge capacity retention rate of the secondary battery B4 of Comparative Example 4, respectively.
[0220] The evaluation results are shown in Table 2. In Table 2, the initial capacity is expressed as a relative value (index) when the value of the initial capacity of the secondary battery B4 of Comparative Example 4 is set to 100.
[0221] [Table 2]
[0222]
[0223] In secondary batteries A4 to A6, the initial capacity is high, the amount of initial side reactions and the cycle degradation rate are small. In secondary batteries A4 to A6, cycle characteristics superior to those of secondary batteries B4 to B6 are obtained. In batteries B5 and B6, the reduction in cycle degradation rate relative to battery B4 is extremely small. On the other hand, in battery A6, the cycle degradation rate is greatly reduced relative to battery B4.
[0224] The negative electrode materials used in the secondary batteries A4 to A6 were subjected to surface analysis based on XPS. As a result, it was confirmed that the amount of MSL was large in the inner layer portion at a depth of 0.2T or more from the outermost surface of the covering layer, and the amount of MSL was small or almost non-existent in the surface layer portion at a depth of less than 0.01T from the outermost surface of the covering layer.
[0225] Industrial Applicability
[0226] The nonaqueous electrolyte secondary battery of the present invention is useful as a main power source for mobile communication equipment, portable electronic equipment, and the like.
[0227] The present invention has been described with respect to the present preferred embodiment, but such disclosure should not be interpreted in a limiting manner. By reading the above disclosure, various deformations and changes are obvious to those skilled in the art belonging to the technical field of the present invention. Therefore, the attached claims should be interpreted as including all deformations and changes without departing from the true spirit and scope of the present invention.
[0228] Description of Reference Numerals
[0229] 1: electrode group, 2: positive electrode lead, 3: negative electrode lead, 4: battery case, 5: sealing plate, 6: negative electrode terminal, 7: gasket, 8: sealing plug, 20: negative electrode material, 21: ion conductive phase, 22: silicon phase, 23: composite particles, 26: covering layer< / icp> < / aes> < / edx>
Claims
1. A negative electrode material for a secondary battery, comprising silicon-containing particles and a covering layer covering at least a portion of a surface of the silicon-containing particles, The silicon-containing particles include an ion-conducting phase and a silicon phase dispersed in the ion-conducting phase, The coating layer contains a lithium sulfonate compound and a linear saturated fatty acid compound having 10 or more carbon atoms.
2. The negative electrode material for a secondary battery according to claim 1, in, The ion conductive phase includes at least one selected from the group consisting of a silicate phase, a silicon oxide phase, and a carbon phase.
3. The negative electrode material for a secondary battery according to claim 1 or 2, in, The lithium sulfonate compound comprises a compound represented by the general formula (1), In the general formula (1), R is an n-valent aliphatic hydrocarbon group having 1 to 5 carbon atoms, and n is 1 or 2.
4. The negative electrode material for a secondary battery according to claim 3, in, The lithium sulfonate compound includes at least one selected from the group consisting of lithium methanesulfonate, lithium ethanesulfonate, and lithium propanesulfonate.
5. The negative electrode material for a secondary battery according to any one of claims 1 to 4, in, The amount of the lithium sulfonate compound attached to the surface of the silicon-containing particles is 1 part by mass or more relative to 100 parts by mass of the silicon-containing particles.
6. The negative electrode material for a secondary battery according to any one of claims 1 to 5, in, The linear saturated fatty acid compound has 10 or more and 30 or less carbon atoms.
7. The negative electrode material for a secondary battery according to any one of claims 1 to 6, in, The straight-chain saturated fatty acid compound comprises a stearic acid compound.
8. The negative electrode material for a secondary battery according to any one of claims 1 to 7, in, The amount of the straight-chain saturated fatty acid compound attached to the surface of the silicon-containing particles is 1 part by mass or more relative to 100 parts by mass of the silicon-containing particles.
9. The negative electrode material for a secondary battery according to any one of claims 1 to 8, in, When surface analysis was performed by X-ray photoelectron spectroscopy, a peak derived from the lithium sulfonate compound was observed in the inner layer portion of the covering layer.
10. The negative electrode material for a secondary battery according to any one of claims 1 to 9, in, A conductive layer including a conductive carbon material is interposed between the silicon-containing particles and the covering layer.
11. A secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, The negative electrode comprises the negative electrode material for a secondary battery according to any one of claims 1 to 10.