Doped VO2-based thermochromic multilayer film system structure and preparation method thereof
By designing a doped VO2-based multilayer film system in the VO2-based thermochromic film system, combined with magnetron sputtering and radio frequency sputtering technology, the shortcomings of the VO2 film system in terms of solar modulation efficiency and visible light transmittance are solved. , achieves the reduction of phase change temperature and performance improvement, and has good intelligent energy-saving performance.
Patent Information
- Application Number
- CN202411090095.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
The existing VO2-based thermochromic film system has poor performance in solar light modulation efficiency and visible light transmittance, and the phase transition temperature is higher than room temperature, making it difficult to practically apply.
The multi-layer film structure of doped VO2-based film is prepared by magnetron sputtering method and radio frequency sputtering method. , the thickness of each film layer and the content of doped elements are controlled, and the doped VO2 film is formed in combination with vacuum thermal oxidation to achieve buffering and revising/reducing the reverse layer effect.
The solar light modulation efficiency is higher than 12%, the visible light transmittance is higher than 50%, the phase transition temperature is reduced to close to room temperature, and it has intelligent energy-saving performance.
Smart Images

Figure SMS_1 
Figure HDA0004986292590000011 
Figure HDA0004986292590000012
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thin film material film system structure and its preparation, and specifically relates to a high performance doped VO 2 Thermochromic multilayer film structure and preparation method thereof. Background Art
[0002] As an indispensable building material, glass carries multiple functions such as decoration, sound insulation, safety protection, and light and heat regulation. Compared with other building materials, glass energy consumption accounts for a high proportion of the total building energy consumption, and is a weak link in building energy conservation. Coating on glass is the main technical means to improve the energy-saving performance of glass. Currently, commercial energy-saving glass is mainly energy-saving film system with silver as the functional film. Although it has good energy-saving effect, it is costly and has poor environmental adaptability.
[0003] VO 2 As a type of vanadium oxide, it has semiconductor-to-metal transition (SMT) properties. 2 The metal-insulator transition (MIT) temperature of the film is about 68°C, and its electrical, optical and thermal properties change dramatically before and after the transition. It is a type of SMT transition material that is closest to room temperature. Because its transmittance in the near-infrared band of the solar spectrum changes greatly before and after the MIT, it is a functional film that can be used as a temperature-adaptive sunlight-controlled smart energy-saving glass.
[0004] Currently, single-layer VO 2 It is difficult for thin films to balance transmittance and solar modulation efficiency (solar modulation efficiency <8%, visible light transmittance <40%), and the SMT transition temperature of thin films is higher than room temperature, which cannot be used in practice. At present, multi-layer film structures are often prepared to improve VO 2 Optical properties, so that the film has a high solar modulation efficiency and visible light transmittance. For example, although Jin et al. prepared ZnO / VO on soda-lime glass by magnetron sputtering 2 / ZnO multilayer films, the solar light modulation efficiency and visible average light transmittance can reach 14% and 52%, but the phase transition temperature of the film is still much higher than room temperature. 2 Thin film ZrO 2 / V 1-x W x O 2 / ZrO 2The thermochromic temperature of the membrane structure material has been reduced to 39°C, the solar regulation efficiency is 12%, and the average visible light lumen transmittance at high and low temperatures is 42%. The thermochromic temperature of the membrane system is still higher than room temperature and needs to be further reduced. The solar regulation efficiency and visible light lumen transmittance are still low and need to be further improved through membrane system design and improved preparation process, which is quite difficult. Summary of the invention
[0005] For existing VO 2 The present invention aims to provide a doped VO 2 The thermochromic multilayer film structure and its preparation method have both good solar light modulation efficiency and good visible light transmittance, and the phase change temperature is close to room temperature; and the solar energy modulation efficiency is higher than 12%, and the average visible light lumen transmittance is higher than 50%.
[0006] In order to achieve the above technical purpose, the technical solution adopted by the present invention is:
[0007] A doped VO 2 The multi-layer thermochromic film structure comprises a substrate and a first TiO 2 Film layer, VO 2 Film layer, second TiO 2 Film and SiO 2 Film layer, abbreviated as substrate / TiO 2 (1) / VO 2 / TiO 2 (2) / SiO 2 Among them, the first TiO 2 The thickness of the film is 130~150nm, VO 2 The thickness of the film is 45-55nm. 2 The thickness of the film is 130~180nm, SiO 2 The thickness of the film layer is 80 to 150 nm.
[0008] In the above scheme, the VO 2 The film layer is doped VO 2 Thin film, abbreviated as A-VO 2 , where A is a doping element, which can be selected from one or more of Nb, Ta, W and Mo, such as Nb doped VO 2 Thin film, Ta-doped VO 2 Thin film, W-doped VO 2 Thin film and Mo-doped VO 2 Thin films, etc., the total doping content is between 1.5 and 5.0 at.%.
[0009] In the above scheme, the SMT temperature of the multilayer thermochromic film system is not higher than 36° C., within the range of 22 to 36° C., while the visible light lumen efficiency is higher than 50%, and the solar energy regulation efficiency is higher than 12%.
[0010] In the above scheme, the substrate is made of amorphous light-transmitting glass material, the thickness of the substrate is 1 to 3 mm, and the light transmittance is not less than 88%.
[0011] The above doped VO 2 The method for preparing a multi-layer thermochromic film structure is to sequentially prepare a first TiO 2 Film layer, VO 2 Film layer, second TiO 2 Film and SiO 2 film layer; wherein,
[0012] 1) TiO in the film system 2 Film layer, with compound TiO 2 Or metal Ti is used as the target material and prepared by magnetron sputtering. 2 The type of thin film controls the first TiO 2 The thickness of the film is 130-150nm. 2 The thickness of the film is 130-180nm;
[0013] 2) VO in the film system 2 film layer, with V doped 2 O 3 Or doped VO 2 The vanadium oxide target was prepared by radio frequency magnetron sputtering combined with vacuum thermal oxidation. 2 The thickness of the film ranges from 45 to 55 nm;
[0014] 3) SiO in the film system 2 Film layer, compound SiO 2 The target material was prepared by RF sputtering and magnetron sputtering. 2 The type of film is adjusted between 80 and 150 nm. 2 The thickness of the film.
[0015] According to the above scheme, in step 2), VO 2 The preparation of the film layer includes two steps: precursor formation step and oxidation step. The precursor formation step adopts radio frequency magnetron sputtering method: using doped vanadium oxide as the target material, magnetron sputtering is performed on the first TiO 2 The surface of the film forms doped vanadium oxide (VO x) precursor film; the oxidation step adopts a vacuum thermal oxidation method: the annealing furnace is evacuated to a pressure of less than 50mTorr, oxygen is introduced for oxidation, the vanadium oxide precursor film is heated at a heating rate of more than 10°C / min and kept warm for a period of time, and then cooled to room temperature with the furnace to obtain a doped vanadium dioxide film, that is, doped VO 2 Membrane layer.
[0016] Further preferably, the doped VOx precursor film is oxidized in a tubular annealing furnace: the vacuum degree in the tubular annealing furnace is evacuated to below 30mTorr by a mechanical pump, and then oxygen is introduced to control the oxygen pressure in the chamber to be 30mTorr to 100mTorr, and the temperature is increased to 450°C to 650°C, preferably 550°C to 600°C, at a heating rate greater than 10°C / min, and kept warm for 20min to 120min, preferably 40min to 60min, and then cooled to room temperature with the furnace to obtain the doped VO 2 film.
[0017] The optical performance of the multilayer film system is related to the type of film layer, the stacking order of the film layers and the matching of the film layer thickness. In particular, it is very difficult to design and prepare a high-performance multilayer thermochromic film system. 2 , doped VO 2 and SiO 2 As the film material, the film structure was further determined to be TiO 2 (1) / A-VO 2 / TiO 2 (2) / SiO 2 , where the thickness of each film layer and the film structure are interdependent. 2 The multi-layer thermochromic film structure is a four-layer film system, TiO 2 (1) / A-VO 2 / TiO 2 (2) / SiO 2 , where VO is doped 2 The layer is used as the thermochromic functional layer, and the buffer and anti-reflection / anti-reflection layers are TiO 2 and SiO 2 The present invention is based on VO with thermochromic properties. 2 Based on the thin film, the VO 2 The spectral properties of the film can improve the visible lumen efficiency and solar conditional efficiency.
[0018] The doped VO of the present invention 2 In the thermochromic multilayer film structure, by adding buffer, anti-reflection / anti-reflection layer structure, the overall optical properties of the film are regulated to a great extent, and the optical properties are superior to those of single-layer VO.2 The film's visible light lumen transmittance and the technical effect of its solar light modulation efficiency. x Elements such as Nb, Ta, W and Mo are doped into the precursor film, which is then further oxidized to generate doped VO 2 layer, effectively reducing the SMT temperature of these films, making the phase transition temperature of the films close to room temperature, at about 35°C. 2 The thermochromic multilayer film system has intelligent energy-saving performance at room temperature.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The doped VO of the present invention 2 The thermochromic multilayer film structure combines good solar light modulation efficiency and good visible light transmittance, with a phase change temperature close to room temperature; the solar energy modulation efficiency is higher than 12%, and the average visible light lumen transmittance is higher than 52%.
[0021] In addition, the preparation method of the present invention is simple to operate, the subsequent annealing process is simple, and no other gases need to be added except argon and oxygen, which is convenient for large-scale production. 2 VO was prepared on the film layer 2 When the film is oxidized, the heat treatment step involves vacuum and O 2 The partial pressure and heat treatment temperature are critical, which is different from the technical difficulty of directly preparing the corresponding film layer on a substrate such as glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0023] Figure 1 VO prepared in Example 1 2 Field emission scanning electron microscopy (FE-SEM) cross-sectional morphology of the thermochromic film.
[0024] Figure 2 The doped VO prepared in Example 1 2 Optical transmittance diagram of the base thermochromic film.
[0025] Figure 3 The doped VO prepared in Example 1 2The transmittance of the base thermochromic film at 1550nm varies with temperature.
[0026] Figure 4 The doped VO prepared in Example 2 2 Field emission scanning electron microscopy (FE-SEM) cross-sectional morphology of the thermochromic film.
[0027] Figure 5 The doped VO prepared in Example 2 2 Optical transmittance diagram of the thermochromic four-layer film system.
[0028] Figure 6 The doped VO prepared in Example 2 2 The transmittance of the base thermochromic film at 1550nm varies with temperature.
[0029] Figure 7 This is a cross-sectional morphology image of the field emission scanning electron microscope (FE-SEM) of comparative example 1.
[0030] Figure 8 This is the optical transmittance spectrum of Comparative Example 1. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] The doped VO of the present invention 2 The thermochromic multilayer film can be prepared by a preparation method comprising the following steps:
[0033] TiO 2 Thin film formation steps: magnetron sputtering of compound TiO 2 Or metal Ti target, sputtering in argon oxygen mixed gas, on the substrate surface (or VO 2 TiO is formed on the surface of the film 2 Thin film, i.e. TiO 2 film layer; wherein the first TiO 2 The second TiO 2 The film layers are prepared by this method. The first TiO 2 The film layer is formed on the substrate surface; the second TiO 2 Film layer on VO 2 Film surface formation;
[0034] VO 2The preparation steps of the layer thin film include two steps: a precursor formation step and an oxidation step, wherein the precursor formation step: using the doped vanadium oxide as the target material, a first TiO 2 The surface of the film forms doped vanadium oxide (VO x ) precursor film; oxidation step: evacuating the annealing furnace to a pressure of less than 50mTorr, introducing oxygen for oxidation, heating the vanadium oxide precursor film at a heating rate of more than 30°C / min and keeping it warm for a period of time, and then cooling the furnace to room temperature to obtain a doped vanadium dioxide film, i.e., doped VO 2 Membrane layer.
[0035] SiO 2 The formation steps of the thin film are as follows: SiO is sputtered by magnetron sputtering. 2 The target or Si target is sputtered in an argon-oxygen mixed gas on the second TiO 2 SiO is formed on the surface of the film 2 Thin film, namely SiO 2 Membrane layer.
[0036] Furthermore, the substrate is a heat-resistant substrate such as quartz glass, so that it can withstand the high temperature used in subsequent steps, and the light transmittance is greater than 88%.
[0037] Furthermore, TiO 2 , VO x Precursor or SiO 2 The substrate temperature during sputtering is adjustable from room temperature to ~400°C.
[0038] Furthermore, TiO 2 Thin film, doped VO 2 Thin film or SiO 2 In the thin film forming step, radio frequency magnetron sputtering, direct current magnetron sputtering or pulsed direct current magnetron sputtering can be used for formation, and the specific formation conditions adopted can be appropriately set by those skilled in the art according to actual conditions. In the present invention, the mass purity of the argon gas used is preferably 99.99% or more, and the mass purity of the oxygen gas used is 99.99% or more.
[0039] Furthermore, the target material is VO 2 and V 2 O 3 The target material is doped with Nb, Ta, W, Mo and the like, and the doping content is between 1.5 and 5.0 at.%.
[0040] Furthermore, a magnetron sputtering apparatus was used to perform sputtering to form TiO 2 Thin film, VO x Precursor film or SiO 2Before filming, the target is pre-sputtered to remove nitrides, oxides, etc. on the surface of the target to prevent surface impurities from affecting the quality of subsequent films and to increase the sputtering rate of the target. During this process, the baffle is closed to prevent the pre-sputtered material from being deposited on the substrate and affecting the quality of subsequent films. During the pre-sputtering process, the vacuum degree of the sputtering chamber is 1.0×10 -5 Torr~1.0×10 -6 Torr, the flow rate of argon is 10sccm~18sccm (pre-sputtering does not require oxygen), and the working pressure of pre-sputtering is 2mTorr~6mTorr to form TiO 2 , VO x Precursor or SiO 2 The pre-sputtering power before filming is 50W-80W, and the pre-sputtering time is 180s-600s. During the formal sputtering process, the flow rate of argon gas is 10sccm-18sccm, the sputtering working pressure is 2mTorr-6mTorr, and the rotation speed of the substrate is fixed at 5-15 rpm to ensure that the sputtered film has good uniformity.
[0041] Furthermore, during the formal sputtering process, the sputtering power of the Ti target is 150W to 300W, the argon-oxygen ratio is between 10:1 and 3:1, and the sputtering time is 3000s to 4500s. TiO 2 The sputtering power of the doped vanadium dioxide target is 50W to 80W, the sputtering time is 5000s to 8000s, and the deposition is doped VO 2 Film layer; SiO 2 The target sputtering power is 80W~150W, the argon-oxygen ratio is between 180:1~100:1, and the sputtering time is 6000s~12000s. The SiO 2 Membrane layer.
[0042] Furthermore, doped VO x The precursor film is oxidized in a tubular annealing furnace: the vacuum degree in the tubular annealing furnace is evacuated to below 30 mTorr by a mechanical pump, and then oxygen is introduced to control the oxygen pressure in the chamber to be 30 mTorr to 100 mTorr, and the temperature is increased to 450°C to 650°C, preferably 550°C to 600°C, at a heating rate of more than 10°C / min, and the temperature is kept for 20min to 120min, preferably 40min to 60min, and the doped VO is obtained. 2 The oxygen flow rate is controlled by the pressure value displayed by the electronic vacuum gauge.
[0043] In the following examples, the optical transmittance spectra from 300 nm to 2500 nm in cold state (5°C) and hot state (90°C) were measured by UV spectrophotometer (UV-3600, Shimadzu, Japan) to characterize the thermochromic properties of the samples. The solar light modulation efficiency (ΔT sol ) and visible light transmittance (T lum ), and its calculation formula is:
[0044]
[0045] Among them, T sol is the solar radiation transmittance, is the solar spectral irradiance, ΔT sol The difference between the solar light modulation efficiency in the hot state and the solar light modulation efficiency in the cold state is defined as the solar light modulation efficiency; T lum is the visible light lumen transmittance, It is a standard luminous efficiency function for human eyes, with a wavelength range of 380 to 780 nm. The average visible light lumen transmittance is defined as the hot and cold T lum The average value of .
[0046] Example 1
[0047] A doped VO 2 The multi-layer thermochromic film structure comprises a substrate and a first TiO 2 Film layer, Nb-doped VO 2 Film layer, second TiO 2 Film and SiO 2 Film layer, abbreviated as substrate / TiO 2 (1) / Nb-VO 2 / TiO 2 (2) / SiO 2 The substrate is made of quartz glass with a thickness of 1 mm. 2 The thickness of the film is 139nm, and Nb-doped VO 2 The thickness of the film layer is 53nm (the doping content of Nb is 2.75at.%), and the second TiO 2 The thickness of the mold layer is 161nm, SiO 2 The thickness of the film is 142nm. Figure 1 shown.
[0048] The above doped VO 2 The preparation method of the multi-layer thermochromic film structure is as follows:
[0049] (1) Using quartz glass with a thickness of 10 mm as a substrate, first use a surfactant to clean the surface of the quartz substrate, then put it in deionized water for ultrasonic cleaning for 30 minutes, and then use anhydrous ethanol for ultrasonic cleaning for 30 minutes. Finally, place the cleaned quartz glass substrate in anhydrous ethanol for later use, and take it out and blow dry when using it;
[0050] (2) The cleaned and dried quartz glass substrate was fixed on the base used for sputtering, and the base was placed in the sputtering chamber of the magnetron sputtering. A Ti target with a mass purity of 99.9% was used as the target material, and the vacuum was evacuated to 5.0×10 -3 mTorr, the flow rate of argon was controlled to be 15sccm and the pre-sputtering working pressure was controlled to be 3mTorr, and the Ti target was pre-sputtered with argon with a mass purity of 99.99% as the working gas. The pre-sputtering power of the Ti target was 70W, the pre-sputtering time was 360s, and the rotation speed of the substrate was always fixed at 10 rpm (including pre-sputtering and formal sputtering); then the flow rate of argon was controlled to be 15sccm, the flow rate of oxygen was 3.3sccm, the sputtering working pressure was 3mTorr, the sputtering power of the Ti target was adjusted to 200W, and after 3675s of sputtering, TiO 2 film.
[0051] Then evacuate to 1.0×10 -5 Torr, using another target head to sputter Nb-VO by RF method 2 The target material (Nb doping content is 2.75at.%) was pre-sputtered, the rotation speed of the substrate was always fixed at 10 rpm, the flow rate of argon was controlled to be 15sccm, the pre-sputtering working pressure was 3mTorr, the pre-sputtering power was 60W, the sputtering time was 600s, and the pre-sputtering power was reduced to 50W after the pre-sputtering was completed. The flow rate of argon was controlled to be 15sccm, the sputtering working pressure was 3mTorr, and TiO was obtained after 7000s of sputtering. 2 / 2.75at.%Nb-VO x Precursor film.
[0052] (3) The obtained TiO 2 / 2.75at.%Nb-VO x The precursor film was placed in a tubular vacuum annealing furnace and evacuated to 20 mTorr using a mechanical pump. The temperature was then rapidly raised to 600 °C at a heating rate of 30 °C / min. The oxygen concentration in the chamber was controlled to be 100 mTorr. After being kept at 600 °C for 30 min, TiO 2 / 2.75at.%Nb-VO 2 After the heat preservation is completed, wait for the temperature in the furnace to cool to room temperature, take out the film and place it in the sputtering chamber of the magnetron sputtering and evacuate it to a vacuum degree of 5.0×10 -6Torr, the flow rate of argon was controlled to 15sccm and the pre-sputtering working pressure was 3mTorr, the rotation speed of the substrate was fixed at 10 rpm, and argon with a mass purity of 99.99% was used as the sputtering gas for direct current pre-sputtering of the Ti target, the pre-sputtering power was 70W, and the pre-sputtering time was 360s; after the pre-sputtering was completed, the sputtering power of the Ti target was adjusted to 200W, the flow rate of argon was controlled to 15sccm, the flow rate of oxygen was controlled to 3.3sccm, and the working pressure was 3mTorr. After 3580s of sputtering, TiO 2 / 2.75at.%Nb-VO 2 / TiO 2 The film was then vacuumed to 1.0×10 -5 After Torr, another target head was used to sputter SiO by radio frequency. 2 The rotation speed of the target and substrate was fixed at 10 rpm, the flow rate of argon was controlled to be 15 sccm, the pre-sputtering working pressure was 3 mTorr, the pre-sputtering power was 60 W, the sputtering time was 600 s, and after the pre-sputtering was completed, the power was increased to 200 W, the flow rate of argon was controlled to be 15 sccm, the flow rate of oxygen was controlled to be 0.1 sccm, the working pressure was 3 mTorr, and TiO was obtained after sputtering for 9600 s. 2 / 2.75at.%Nb-VO 2 / TiO 2 / SiO 2 Thin film, i.e. doped VO 2 The four-layer thermochromic film structure can also be called doped VO 2 Thermochromic film.
[0053] Figure 2 The doped VO prepared in Example 1 2 The optical transmittance diagram of the four-layer thermochromic film structure is shown in Figure 1. The average visible light lumen efficiency and solar energy regulation efficiency calculated from this are 50.1% and 12.3% respectively.
[0054] Figure 3 The doped VO prepared in Example 1 2 The transmittance of the four-layer thermochromic film structure at 1550nm varies with temperature. The SMT temperature is 36℃, which is close to room temperature.
[0055] Example 2
[0056] A doped VO 2 The multi-layer thermochromic film structure comprises a substrate and a first TiO 2 Film layer, Ta-doped VO 2 Film layer, second TiO 2 Film and SiO 2Film layer, abbreviated as substrate / TiO 2 (1) / Nb-VO 2 / TiO 2 (2) / SiO 2 The substrate is made of quartz glass with a thickness of 1 mm. 2 The thickness of the film is 129nm, Ta-doped VO 2 The thickness of the film layer is 48nm (Ta doping content is 2.0at.%), the second TiO 2 The thickness of the mold layer is 150nm, SiO 2 The thickness of the film is 122nm. Figure 4 shown.
[0057] The doped VO in this embodiment 2 Preparation method of multi-layer thermochromic film structure: The same method as in Example 1 is used to obtain TiO 2 Thin film, 2.0at.%Ta-VO was sputtered by RF method using another target head 2 The target material was pre-sputtered and formally sputtered, the formal sputtering power was controlled to be 50 W, the sputtering time was 6000 s, and the other sputtering parameters were the same as in Example 1, to obtain TiO 2 / 2.0at.%Ta-VOx precursor film. Then, the temperature was rapidly raised to 600℃ in a tube furnace at a heating rate of 30℃ / min, and the oxygen concentration in the chamber was controlled to be 100mTorr. After being kept at 600℃ for 60min, TiO 2 / 2.0at.%Ta-VO 2 The same method as in Example 1 was used to obtain TiO 2 / 2.0at.%Ta-VO 2 / TiO 2 / SiO 2 Thin film, i.e. doped VO 2 Four-layer thermochromic film structure.
[0058] Figure 5 The doped VO prepared in Example 2 2 The optical transmittance picture of the four-layer thermochromic film structure, from which the average visible light lumen efficiency and solar energy regulation efficiency calculated are 52.5% and 13.7%.
[0059] Figure 6 The doped VO prepared in Example 2 2 The transmittance of the four-layer thermochromic film structure at 1550nm changes with temperature, from which the SMT transition is obtained to 35℃.
[0060] Comparative Example 1
[0061] The same method as in Example 1 was used to treat the quartz glass substrate, and 2.75 at.% Nb-VO was obtained by sputtering in a magnetron sputtering apparatus under the same parameters. x Precursor film. The obtained 2.75at.% Nb-VO x The precursor film was placed in a tubular annealing furnace, and the mass flow meter was used to control the oxygen concentration to 100 mTorr. The temperature was then rapidly raised to 550°C at a heating rate of 30°C / min and kept at 550°C for 30 min. The temperature in the furnace was cooled to room temperature to obtain 2.75 at.% Nb-VO 2 Thin films, such as Figure 7 As shown, the thickness is 55 nm.
[0062] Figure 8 This is the optical transmittance spectrum of Comparative Example 1, and the average visible light lumen efficiency and solar condition efficiency calculated therefrom are 42% and 6%, both of which are far lower than those of the embodiment.
[0063] In summary, the doped VO provided by the present invention 2 Multilayer thermochromic film structure: substrate / TiO 2 (1) / A-VO 2 / TiO 2 (2) / SiO 2 Among them, the first TiO 2 The thickness of the film is 130~150nm, A-VO 2 The thickness of the film is 45-55nm. 2 The thickness of the mold layer is 130-180nm, SiO 2 The thickness of the film layer is 80 to 150 nm; the doping element A can be one or more of Nb, Ta and W, and the total doping content is between 1.5 and 5.0 at.%. Within the scope of this embodiment, the SMT temperature of the multilayer thermochromic film system is not higher than 36°C, and the visible light lumen efficiency is higher than 50%, and the solar energy regulation efficiency is higher than 12%.
[0064] The above is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A VO2-doped multilayer thermochromic film structure, characterized in that: It includes a substrate, and a first TiO2 film layer, a VO2 film layer, a second TiO2 film layer and a SiO2 film layer sequentially covering the substrate; wherein the thickness of the first TiO2 film layer is 130-150nm, the thickness of the VO2 film layer is 45-55nm, the thickness of the second TiO2 film layer is 130-180nm, and the thickness of the SiO2 film layer is 80-150nm.
2. The VO2-doped multilayer thermochromic film structure according to claim 1, characterized in that: The VO2 film layer is a doped VO2 film, the doping elements are selected from one or more of Nb, Ta, W and Mo, and the total doping content is between 1.5 and 5.0 at.%.
3. The VO2-doped multilayer thermochromic film structure according to claim 1, characterized in that: The SMT temperature of the multi-layer thermochromic film system is not higher than 36° C., while the visible light lumen efficiency is higher than 50%, and the solar energy regulation efficiency is higher than 12%.
4. The VO2-doped multilayer thermochromic film structure according to claim 1, characterized in that: The substrate is made of amorphous glass material with a thickness of 1 to 3 mm and a light transmittance of not less than 88%.
5. The method for preparing the VO2-doped multilayer thermochromic film structure according to claims 1 to 4, characterized in that: A first TiO2 film layer, a VO2 film layer, a second TiO2 film layer and a SiO2 film layer are sequentially prepared on a substrate by magnetron sputtering; wherein, 1) The TiO2 film layer in the film system is prepared by using a radio frequency sputtering magnetron sputtering method with compound TiO2 or metal Ti as a target material, and the thickness of the first TiO2 film layer is controlled to be 130 to 150 nm, and the thickness of the second TiO2 film layer is controlled to be 130 to 180 nm; 2) The VO2 film layer in the film system is prepared by using a doped vanadium oxide target as a target material and adopting a radio frequency magnetron sputtering method combined with a vacuum thermal oxidation method to control the thickness of the VO2 film layer to be in the range of 45 to 55 nm; wherein a doped vanadium oxide precursor film is formed on the surface of the first TiO2 film layer by a magnetron sputtering method; and the vanadium oxide precursor film is oxidized into a doped vanadium dioxide film by a vacuum thermal oxidation method; 3) The SiO2 film layer in the film system is prepared by using compound SiO2 as a target material and a radio frequency sputtering magnetron sputtering method, and the thickness of the SiO2 film layer is controlled to be in the range of 80 to 150 nm.
6. The method for preparing a VO2-doped multilayer thermochromic film structure according to claim 5, characterized in that: In step 2), the preparation of the VO2 film layer includes two steps: a precursor formation step and an oxidation step. The precursor formation step adopts a radio frequency magnetron sputtering method: using doped vanadium oxide as a target, a doped vanadium oxide precursor film is formed on the surface of the first TiO2 film layer by a magnetron sputtering method in an argon atmosphere; the oxidation step adopts a vacuum thermal oxidation method: the annealing furnace is evacuated to a pressure below 50mTorr, oxygen is introduced for oxidation, the vanadium oxide precursor film is heated at a heating rate of more than 10°C / min and kept warm for a period of time, and then cooled to room temperature with the furnace to obtain a doped vanadium dioxide film, i.e., a doped VO2 film layer.
7. The method for preparing a VO2-doped multilayer thermochromic film structure according to claim 6, characterized in that: The doped VOx precursor film is oxidized in a tubular annealing furnace: the vacuum degree in the tubular annealing furnace is evacuated to below 30mTorr using a mechanical pump, oxygen is then introduced, and the oxygen pressure in the chamber is controlled to be 30mTorr to 200mTorr. The temperature is increased to 450°C to 650°C at a heating rate greater than 10°C / min, kept warm for 20min to 120min, and cooled to room temperature with the furnace to obtain a doped VO2 film.
8. The method for preparing a VO2-doped multilayer thermochromic film structure according to claim 6, characterized in that: Before using a magnetron sputtering instrument to formally sputter TiO2 film, vanadium oxide precursor film or SiO2 film, the target material needs to be pre-sputtered. During the pre-sputtering process, the vacuum degree of the sputtering chamber is 1.0×10 -5 Torr~1.0×10 -6 Torr, the flow rate of argon is 10sccm~18sccm, the working pressure of pre-sputtering is 2mTorr~6mTorr, the pre-sputtering power is 50W~80W, and the pre-sputtering time is 180s~600s.
9. The method for preparing a VO2-doped multilayer thermochromic film structure according to claim 6, characterized in that: In the process of formally sputtering the TiO2 film, the sputtering power is 150W to 300W, the flow rate of argon gas is 10sccm to 18sccm, the ratio of argon to oxygen is between 10:1 and 3:1, the sputtering working pressure is 2mTorr to 6mTorr, the sputtering time is 3000s to 4500s, and the rotation speed of the substrate is fixed at 5 to 15 rpm; In the process of formally sputtering to form the vanadium oxide precursor film, the sputtering power is 50W to 80W, the flow rate of argon gas is 10sccm to 18sccm, the sputtering working pressure is 2mTorr to 6mTorr, the sputtering time is 5000s to 8000s, and the rotation speed of the substrate is fixed at 5 to 15 rpm; During the formal sputtering process of forming the SiO2 film layer, the sputtering power is 80W~150W, the flow rate of argon gas is 10sccm~18sccm, the ratio of argon to oxygen is between 180:1~100:1, the sputtering working gas pressure is 2mTorr~6mTorr, the sputtering time is 6000s~12000s, and the rotation speed of the substrate is fixed at 5~15 rpm.
Citation Information
Cited By
Ultraviolet-shielding color-dynamically-adjustable VO2 intelligent window and preparation method thereof
CN119805791A