Preparation method and application of modified binder
Modified adhesives are prepared through high temperature and high pressure treatment to form a cladding structure, which solves the problems of film formation cracking and insufficient mechanical properties of sulfide solid electrolytes, improves the electrochemical performance and cycle stability of the battery, and is used in all solid lithium Ion battery.
Patent Information
- Application Number
- CN202411107768.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The solid electrolyte of sulfide is prone to cracking during film formation, resulting in lithium dendrites forming during battery charge and discharge, affecting electrochemical performance. The existing binder PTFE makes the electrolyte fibrillation under the action of shear force and the film formation effect of the electrolyte fibrillation is poor. , and the film forming performance of PAA and PAA-Li is not ideal, making it difficult to effectively improve the capacity and circulation performance of the battery.
Modified adhesives are prepared by high temperature and high pressure treatment using polymer A (PTFE) and polymer B (PAA or PAA-Li) to form a clad structure, enhance the mechanical properties and ionic conductivity of the electrolyte and improve the overall performance of the battery. and stability.
It achieves higher density and mechanical strength of the electrolyte membrane, improves the electrochemical performance and cycle stability of the battery, and is widely used in the field of all-solid lithium-ion batteries, overcoming the problems of electrolyte film formation cracking and insufficient strength and toughness.
Smart Images

Figure CN118995086A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of sulfide all-solid-state lithium-ion batteries, and specifically relates to a preparation method and application of a modified binder, in particular to a binder for preparing electrolytes by a dry process. Background Art
[0002] Sulfide electrolytes have attracted increasing attention due to their ultra-high ionic conductivity and inherent softness. Correspondingly, the lack of strength and toughness and easy cracking of sulfide electrolytes during the film formation process are problems that need to be solved. At present, the main binder for dry preparation of electrolyte membranes is PTFE, which fibrillates the electrolyte into a film under the action of shear force, thereby realizing a self-supporting film of solid sulfide electrolyte. However, as the proportion of PTFE decreases during the film formation process, its film formation effect becomes worse, which easily leads to cracking of the electrolyte membrane and the formation of lithium dendrites during the charge and discharge process of the battery, affecting the various electrochemical performance indicators of the material.
[0003] The role of polyacrylic acid (PAA) in sulfide solid electrolytes is mainly focused on improving the performance and stability of the electrolyte, especially in sulfide all-solid-state batteries, where the application of PAA can help solve some key technical challenges. The following points outline several important roles of PAA in sulfide solid electrolytes: 1. Interface stabilizer: PAA can be used as an interface stabilizer to reduce the interface reaction between the metal lithium anode and the sulfide electrolyte. Since both metal lithium and lithium sulfide are unstable and easily react with moisture in the air, the introduction of PAA can form a protective film to reduce the side reactions when the sulfide electrolyte contacts lithium metal, thereby improving the cycle stability and safety of the battery. 2. Inhibit electrolyte degradation: PAA can help inhibit the degradation of sulfide solid electrolytes in the air. Sulfide electrolytes easily react with moisture in the air, releasing toxic hydrogen sulfide gas and causing degradation of the electrolyte structure and attenuation of performance. The addition of PAA can improve the air stability of the electrolyte and extend its service life. 3. Enhance mechanical properties: The addition of PAA can enhance the mechanical properties of sulfide solid electrolytes, making them stronger and more durable. By improving the mechanical strength of the electrolyte, cracks and delamination caused by mechanical stress during battery assembly and operation can be reduced, thereby improving the overall performance and reliability of all-solid-state batteries. 4. Improve electrode-electrolyte interface contact: PAA can promote close contact between the electrode and the electrolyte, which is crucial to improving the electrochemical performance of the battery. Good interface contact can reduce contact resistance and improve charge transfer efficiency, thereby improving the power density and energy density of the battery. 5. Regulate the ionic conductivity of the electrolyte: Although PAA itself may not be an ionic conductor, it can indirectly improve the ionic conductivity by adjusting the microstructure of the electrolyte, such as forming a continuous ion conduction path. This usually involves controlling the porosity and crystallinity of the electrolyte to optimize ion migration. In general, the application of PAA in sulfide solid electrolytes is to improve the overall performance and stability of all-solid-state batteries by improving interface stability, enhancing mechanical properties and regulating microstructure. These effects are of great significance to promoting the development and commercialization of solid-state battery technology. However, the specific formulation and addition ratio of PAA need to be optimized according to the specific battery design and working conditions to achieve optimal electrochemical performance.
[0004] The role of PAA-Li (polyacrylate lithium) in sulfide solid electrolytes is mainly reflected in the following aspects: 1. Stabilizer and film former: PAA-Li can form a protective solid electrolyte interface film (SEI) on the electrode / electrolyte interface. This film helps stabilize the electrode surface and reduce the side effects caused by direct contact with the sulfide electrolyte, such as inhibiting dendrite growth, thereby improving the safety and cycle stability of the battery. 2. Improve interfacial compatibility: The contact between the sulfide solid electrolyte and the electrode material often leads to a higher interfacial impedance, which affects the transmission efficiency of lithium ions. As a polymer additive, PAA-Li can improve the compatibility between the electrode material and the sulfide electrolyte, promote the efficient conduction of lithium ions, and thus improve the overall electrochemical performance of the battery. 3. Regulate ionic conductivity: Through interaction with the sulfide electrolyte, PAA-Li may affect the microstructure inside the electrolyte, thereby regulating ionic conductivity. Although PAA-Li itself is not a high ionic conductivity material, it can indirectly optimize the ion transmission path by changing the morphology and structure of the electrolyte. 4. Inhibit side reactions: Sulfide solid electrolytes easily react with water or other components in the air to generate toxic gases such as H2S. The introduction of PAA-Li may help form a protective layer to reduce the corrosion of the electrolyte by the external environment, thereby improving the environmental adaptability and long-term storage stability of the battery. 5. Promote lithium ion migration: In some cases, the lithium affinity of PAA-Li can help the transport of lithium ions at the electrode / electrolyte interface, especially in porous electrode structures, where it can penetrate into micropores and promote a more uniform distribution of lithium ions. In summary, the application of PAA-Li as an additive in sulfide solid electrolyte systems is mainly to optimize battery performance, including improving cycle stability, safety, and electrochemical performance.
[0005] However, compared with PTFE, the film-forming properties of PAA and PAA-Li are not ideal. In this field, it is expected to develop a composite modified binder system to solve the problem of film cracking and increase strength and toughness of sulfide solid electrolytes, while further improving the capacity and cycle performance of batteries. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a preparation method and application of a modified binder. The modified binder of the present invention has good bonding force and good ionic conductivity, overcomes the shortcomings of reduced PTFE proportion in the electrolyte during film formation and cracking of sulfide solid electrolyte film formation, and achieves a breakthrough in the existing dry electrolyte membrane production process, thereby making the dry electrolyte membrane technology widely used in the field of sulfide all-solid-state lithium-ion batteries.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] The present invention provides a method for preparing a modified binder, wherein the modified binder is prepared from two polymers, a polymer A and a polymer B, by the following steps:
[0009] S1, dissolving polymer B in a solvent, adding polymer A, and stirring to make it dispersed evenly to form a mixed solution;
[0010] S2, subjecting the mixed solution to high temperature and high pressure treatment, and filtering after cooling to obtain a modified binder;
[0011] The polymer A is PTFE; the polymer B is one or more of PAA and PAA-Li.
[0012] As an embodiment of the present invention, in step S1, the mass fraction of polymer B accounts for 2.5% to 5.5% of polymer A (eg, 2.5%, 3.5%, 4.5%, 5.5%), preferably 3.5% to 4.5%.
[0013] As an embodiment of the present invention, in step S1, the mass of the solvent is 15 to 20 times that of polymer A, preferably 20 times.
[0014] As an embodiment of the present invention, in step S1, the polymer B is preferably PAA-Li.
[0015] As an embodiment of the present invention, in step S1, the solvent includes one or more of ethanol, acetone, and tetrahydrofuran. Acetone is preferably used as the solvent. The solvent selected by the present invention is such that polymer B is soluble in the solvent and polymer A is insoluble in the solvent.
[0016] As an embodiment of the present invention, in step S2, the high temperature and high pressure treatment is carried out under high temperature and high pressure conditions. In the high temperature and high pressure conditions, the temperature is 60 to 120°C, the pressure is 100 kPa to 500 kPa, preferably 200 kPa. The time of the high temperature and high pressure treatment is 6 to 12 hours, for example, 6 hours, 8 hours, 10 hours, 12 hours.
[0017] Under normal temperature and pressure conditions, polymer B (PAA, PAA-Li) is soluble in solvents, while polymer A (PTFE) is insoluble in solvents. However, polymer B (PAA, PAA-Li) has poor solubility. After mixing with polymer A (PTFE) in a solvent, a small portion of polymer A (PTFE) particles will have polymer B (PAA, PAA-Li) adsorbed on the surface, and remain on the particle surface after filtration, forming a similar incomplete coating layer. However, due to the lack of high temperature and high pressure conditions, the bonding effect is poor and it is easy to fall off. In other words, normal temperature and pressure conditions cannot completely coat the particles to form adhesive particles with a stable coating structure. What is obtained are a small number of particles with an unstable coating structure, and most of them are still the original polymer A (PTFE) particles. For particles with a coating layer, the coating layer will also separate from the particles at the beginning of rolling due to its unstable coating structure, resulting in polymer A fiberization while polymer B will not be fiberized.
[0018] During the heating and pressurizing process of the present invention, polymer B (PAA, PAA-Li) has better solubility (polymer macromolecules are better dispersed and can be more evenly adsorbed on the particle surface to form a coating layer). Under high temperature and high pressure conditions, it can be rapidly dissolved in the solvent and physically coated on the surface of polymer A (PTFE) particles to form a coating layer. High temperature and high pressure can also make the coating layer more evenly and tightly combined, and have better bonding strength.
[0019] As an embodiment of the present invention, in step S2, the high temperature and high pressure treatment is carried out under stirring conditions, and the stirring speed is 400-600rpm / min, preferably 500rpm / min. The reaction can be carried out in a magnetic high temperature and high pressure reactor. After the reaction, the mixed solution is cooled to room temperature and then filtered to filter out the solvent to obtain an adhesive.
[0020] As an embodiment of the present invention, in step S2, the modified binder obtained is a particle structure containing a coating layer, and the polymer B is coated on the surface of the polymer A particles.
[0021] The present invention also provides a modified adhesive obtained by the preparation method. The present invention also provides an application of the modified adhesive in the dry process preparation of electrolyte self-supporting membranes.
[0022] The present invention also provides an electrolyte self-supporting membrane, which comprises the modified binder and a sulfide electrolyte.
[0023] As one embodiment of the present invention, the sulfide electrolyte comprises Li6PS5X (X = Cl, Br, I), Li 10 GeP2S 12 At least one of .
[0024] As an embodiment of the present invention, in the dry electrolyte self-supporting membrane, the weight ratio of the modified binder used is 0.5% to 5% (for example: 0.5%, 1.5%, 2.5%, 3.5% or 4.5%), and the weight ratio of the electrolyte is 95% to 99.5% (for example: 95.5%, 96.5%, 97.5%, 98.5% or 99.5%).
[0025] The present invention also provides a method for preparing the dry electrolyte self-supporting membrane, comprising the following steps:
[0026] (1) The electrolyte and the modified binder are fully mixed in proportion;
[0027] (2) Roll grinding with a roller mill to achieve sufficient shearing;
[0028] (3) Rolling with a hot roller press to obtain a dry electrolyte self-supporting membrane.
[0029] Preferably, the rotation speed of the above-mentioned rolling mill is 100-500 rpm / min, preferably 200 rpm / min, and the rolling milling time is 6-10 hours, preferably 8 hours.
[0030] Preferably, the temperature of the hot roller pressing is 50-70°C, preferably 60°C.
[0031] In the process of preparing self-supporting film, electrolyte and modified binder are tumbled, although in this process, the coating structure of adhesive is destroyed, but the polymer B (PAA, PAA-Li) coating layer on its surface is destroyed together with the attachment polymer A (PTFE). In the film-making process, the fibrillation of polymer A is drawn to make dielectric film-forming, and the destroyed coating layer polymer B adheres to the polymer A surface during the fibrillation process, and the binding force of the coating layer is strong, which ensures that polymer B still adheres to polymer A during the destruction process, so that polymer A can drive polymer B to also fibrillate when fibrillating, which is equivalent to polymer B being also fibrillated, thereby enhancing the mechanical properties of polymer A (similar to double-layer material enhancement or fiber enhancement). And the cohesiveness of adhesive is determined by the fibrillation of polymer A, and introducing polymer B further enhances the mechanical strength of dielectric film, making dielectric film more compact. And without being made into coating structure, polymer A is fibrillated in the particle mixing process, and polymer B cannot be fibrillated, and the effect of the present invention is not reached. At the same time, the fibrillated polymer B also improves the compatibility between the electrode material and the sulfide electrolyte, promotes the efficient conduction of lithium ions, and thus enhances the overall electrochemical performance of the battery.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) The modified binder provided by the present invention is a particle structure, which is deformed during rolling and hot rolling, and the particle structure is destroyed, providing more bonding area for the electrolyte, making the electrolyte more dense and stronger.
[0034] (2) The Li-PAA used in the present invention has better conductivity performance after forming an electrolyte self-supporting membrane. This is because the Li-PAA provides more lithium ions to the sulfide solid electrolyte, increasing the number of ion migration, so that the electrolyte membrane has better ion conductivity.
[0035] (3) The present invention achieves a breakthrough in the existing dry solid electrolyte production process, thereby enabling the dry electrolyte technology to be widely used in the field of all-solid-state lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0037] Figure 1 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in Experimental Group 1 in Example 1;
[0038] Figure 2 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in the comparative test group 1 in Example 1;
[0039] Figure 3 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in the comparative test group 2 in Example 1;
[0040] Figure 4 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in the comparative test group 3 in Example 1;
[0041] Figure 5 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in the comparative test group 4 in Example 1;
[0042] Figure 6 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in the comparative test group 5 in Example 1;
[0043] Figure 7 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in the comparative test group 1 in Example 2;
[0044] Figure 8 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in the comparative test group 2 in Example 2;
[0045] Fig. 9This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in the comparative test group 3 in Example 2;
[0046] Fig.10 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in Comparative Example 2;
[0047] Fig.11 This is the SEM microstructure of the dry electrolyte self-supporting membrane obtained in Comparative Example 3;
[0048] Fig.12 This is the SEM microstructure image of the modified binder obtained in Experimental Group 1 in Example 1. DETAILED DESCRIPTION
[0049] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following examples are implemented on the premise of the technical solution of the present invention, provide detailed implementation methods and specific operation processes, and will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.
[0050] Example 1 Optimization of the proportion of modified binder components
[0051] This embodiment provides a method for preparing a modified binder and a dry electrolyte self-supporting film, comprising the following steps:
[0052] Optimization of modified binder component ratio:
[0053] According to Table 1, PAA-Li was dissolved in acetone to form a uniform solution, and PTEF was then added to the solution and stirred to disperse it evenly to form a mixed solution. The mixed solution was placed in a magnetic high-temperature and high-pressure reactor, and subjected to high-temperature and high-pressure treatment for 10 hours at a temperature of 100°C, a pressure of 200 kPa, and a stirring speed of 500 rpm / min. The reacted solution was then cooled to room temperature and filtered to remove the solvent to obtain a modified binder, the microstructure of which is as follows: Fig.12 shown.
[0054] Take 2 g of the modified binder and Li6PS5Cl electrolyte in a mass ratio of 1:99 and put them into a roller mill, keep the speed at 200 rpm / min and roll for 8 hours, then keep the temperature at 60°C on a hot roller press and roll the electrolyte multiple times to obtain a dry electrolyte self-supporting film.
[0055] Table 1 Components and dosage of modified binder
[0056]
[0057] Test method:
[0058] The dry electrolyte self-supporting membrane obtained above was first tested for its microstructure using an electron scanning microscope (SEM) at a magnification of 200 times. Figure 1-6 As shown, the conductivity of the electrolyte support membrane of each component above was tested in the frequency range of 100mHz to 700kHz using an EC-lable test system, and finally a battery was assembled using ternary (NCM811) as the positive electrode material, the above self-supporting membrane as the electrolyte, and lithium silicon as the negative electrode material to test its electrochemical performance.
[0059] The test results are shown in Table 2.
[0060] Table 2
[0061]
[0062]
[0063] It can be seen that when the dosage of PAA-Li is 60-100 mg, the prepared self-supporting film has a good film-forming state.
[0064] Example 2 Optimization of modified binder material composition
[0065] This embodiment provides a method for preparing a modified binder and a dry electrolyte self-supporting film, comprising the following steps:
[0066] Optimization of modified binder materials:
[0067] According to Table 3, PAA-Li and PAA were dissolved in acetone to form a uniform solution, and then PTEF was added to the solution and stirred to disperse it evenly to form a mixed solution; the mixed solution was placed in a magnetic high-temperature and high-pressure reactor and subjected to high-temperature and high-pressure treatment for 10 hours at a temperature of 100°C and a pressure of 200 kPa with a stirring speed of 500 rpm / min; the reacted solution was then cooled to room temperature and the solvent was filtered off to obtain a modified binder.
[0068] 2 g of the obtained modified binder and Li6PS5Cl electrolyte were put into a roller mill in a mass ratio of 1:99 and rolled at a speed of 200 rpm / min for 8 hours. Then, the electrolyte obtained after rolling was rolled multiple times on a hot roller press at a temperature of 60°C to obtain a dry electrolyte self-supporting film.
[0069] Table 3
[0070]
[0071] Test method:
[0072] The dry electrolyte self-supporting membrane obtained above was first tested for its microstructure using an electron scanning microscope (SEM) at a magnification of 200 times. Figure 1 , Figure 7-9 As shown, the conductivity of the electrolyte support membrane of each component above was tested in the frequency range of 100mHz to 700kHz using an EC-lable test system, and finally a battery was assembled using ternary (NCM811) as the positive electrode material, the above self-supporting membrane as the electrolyte, and lithium silicon as the negative electrode material to test its electrochemical performance.
[0073] The test results are shown in Table 4
[0074] Table 4
[0075]
[0076] It can be seen that the modified binder obtained by high temperature and high pressure treatment of PAA-Li or PAA and PTFE has a good self-supporting film forming state; when only PTFE or PAA-Li is used, the film forming effect is not good.
[0077] Comparative Example 1
[0078] This comparative example provides a modified binder and a method for preparing a dry electrolyte self-supporting membrane, the composition and preparation method of which are substantially the same as those of the test group 1 in Example 1, except that PTFE is replaced by PVDF.
[0079] Comparative Example 2
[0080] This comparative example provides a modified binder and a method for preparing a dry electrolyte self-supporting film, the composition and preparation method of which are basically the same as those of Experimental Group 1 in Example 1, except that PAA-Li is replaced by lithium bis(difluorosulfonyl)imide (LiFSI).
[0081] Comparative Example 3
[0082] This comparative example provides a method for preparing a mixed binder and a dry electrolyte self-supporting film, the composition and preparation method of which are basically the same as those of Experimental Group 1 in Example 1, except that PAA-Li and PTEF are directly mixed and stirred (at a speed of 500 rpm / min) for 10 h, and then mixed with Li6PS5Cl electrolyte.
[0083] The test results are shown in Table 5.
[0084] Table 5
[0085]
[0086]
[0087] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for preparing a modified binder, characterized in that: The steps include: S1, dissolving polymer B in a solvent, adding polymer A, stirring and dispersing the polymer A uniformly to form a mixed solution; S2, subjecting the mixed solution to high temperature and high pressure treatment, and filtering after cooling to obtain a modified binder; In step S1, the polymer A is PTFE; the polymer B is one or more of PAA and PAA-Li; the solvent includes one or more of ethanol, acetone, and tetrahydrofuran; In step S2, the temperature of the high temperature and high pressure treatment is 60-120°C, the pressure is 100kPa-500kPa, and the time is 6-12h; the obtained modified binder is particles containing a coating layer, and polymer B is coated on the surface of polymer A particles.
2. The preparation method according to claim 1, characterized in that: In step S1, the polymer B accounts for 2.5% to 5.5% of the mass of the polymer A.
3. The preparation method according to claim 1, characterized in that: In step S1, the mass of the solvent is 15 to 20 times that of polymer A.
4. The preparation method according to claim 1, characterized in that: In step S2, the high temperature and high pressure treatment is carried out under stirring conditions, and the stirring speed is 400-600 rpm / min.
5. A modified adhesive obtained by the preparation method according to any one of claims 1 to 4.
6. Use of the modified adhesive as claimed in claim 5 in the dry process for preparing an electrolyte self-supporting membrane.
7. An electrolyte self-supporting membrane, characterized in that: The electrolyte self-supporting film comprises the modified binder as claimed in claim 5 and a sulfide electrolyte.
8. A method for preparing the electrolyte self-supporting membrane according to claim 7, characterized in that: The method comprises the following steps: fully and uniformly mixing the sulfide electrolyte and the modified binder in proportion, and then rolling and rolling to obtain a dry electrolyte self-supporting membrane.
Citation Information
Cited By
Disulfide bond-hydrogen bond synergistically modified PTFE (Polytetrafluoroethylene) binder as well as preparation method and application thereof
CN120623928A
A disulfide-hydrogen bond synergistically modified PTFE binder, preparation method and application thereof
CN120623928B